Naphthalene-containing polyesterimide resin and its preparation method

By introducing naphthalene rings and low-polarity groups into polyimide resin, the problem of poor solubility of polyimide resin is solved, achieving good solubility and toughness, while maintaining low dielectric loss and water absorption, making it suitable for electronic packaging materials and circuit boards.

CN117430811BActive Publication Date: 2026-11-17SHENZHEN UNIV
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202311462625.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-03
Publication Date
2026-11-17
Estimated Expiration
2043-11-03

AI Technical Summary

Technical Problem

Existing polyimide resins have poor solubility and are difficult to disperse well in solvents.

Method used

By introducing a naphthalene ring structure and replacing the traditional benzene ring with low-polarity groups, the polyesterimide resin is ensured to contain at least two ester bonds, thereby reducing the proportion of polar groups in the molecular chain and disrupting the regularity of the molecular chain.

Benefits of technology

It improves the solubility and toughness of polyesterimide resin while maintaining low dielectric loss, dielectric constant and water absorption, making it suitable for electronic packaging materials and circuit boards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117430811B_ABST
    Figure CN117430811B_ABST
Patent Text Reader

Abstract

This application discloses a naphthalene-containing polyesterimide resin and its preparation method, belonging to the field of polymer materials technology. The preparation method of the naphthalene-containing polyesterimide resin includes: mixing a naphthalene-containing diamine monomer, a dianhydride monomer, and a solvent and carrying out a polycondensation reaction to obtain a polyesteramic acid solution; molding the polyesteramic acid solution and carrying out an imidization reaction to obtain the naphthalene-containing polyesterimide resin. This application solves the technical problem of poor solubility in existing polyimide resins.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application relates to the field of polymer materials technology, and in particular to a naphthalene ring-containing polyesterimide resin and its preparation method. Background Technology

[0002] Polyimide (PI) is an important engineering plastic today. This engineering plastic possesses excellent mechanical properties and thermal stability, and therefore is widely used in the semiconductor industry, optoelectronics industry, aerospace materials, automotive industry, communication materials, machinery industry, and thin film industry. Due to its superior optoelectronic properties, polyimide is also used as a substrate and packaging material for semiconductors, becoming an indispensable polymer material in cutting-edge technology industries.

[0003] Traditional aromatic polyimides generally contain benzene and imide ring structures in their main chain. The electronic polarization and molecular conjugation structure result in strong intermolecular interactions, causing the polyimide molecular chains to be tightly packed. The strong intermolecular forces make it difficult for solvents to penetrate during processing, leading to poor solubility.

[0004] The above content is only used to help understand the technical solution of this application and does not represent an admission that the above content is prior art. Summary of the Invention

[0005] The main objective of this application is to provide a naphthalene ring-containing polyesterimide resin and its preparation method, aiming to solve the technical problem of poor solubility of existing polyimide resins.

[0006] To achieve the above objectives, this application provides a naphthalene-containing polyesterimide resin having the structure shown in formula (1):

[0007]

[0008] Where n is greater than or equal to 1;

[0009] A1, A2 and A3 respectively include any one of aromatic groups and heterocyclic compounds with 1-20 carbon atoms;

[0010] X1, X2, X3 and X4 are all low polar groups, and at least two of X1, X2, X3 and X4 are ester bonds;

[0011] R1, R2, R3, R4, R5, and R6 respectively include H, F, Cl, Br, I, CN, NH2, and C. r+1 H 2r+2 C r H2 r+1 C r H 2r+1 COOH, OC r H2r+1 CF3, C(CH3)3, Any one of them.

[0012] Optionally, the substituents of any one or more of A1, A2 and A3 include any one of hydrogen atom, alkoxy, aralkyl, alkyl with 1-6 carbon atoms and haloalkyl.

[0013] Optionally, A1, A2, and A3 respectively have the structure shown in any one of equations (2), (3), (4), and (5):

[0014]

[0015] Among them, B1, B2, B3, B4, B5, B6, B7, and B8 respectively include H, F, Cl, Br, I, CN, NH2, and C. r+1 H 2r+2 C r H2 r+1 C r H 2r+1 COOH, OC r H 2r+1 CF3, C(CH3)3, Any one of them.

[0016] Optionally, any one or more of A1, A2 and A3 have a structure represented by D1-L-D2, wherein D1 and D2 have structures represented by any one of formulas (2), (3), (4) and (5), respectively, and L is a low polar group.

[0017] Optionally, L includes any one of -(C=O)O-, -O(C=O)-, -O-, -S-, -SO2-, -SO-, -C(O)-, -CH2-, -C(CH3)2- and -C(CF3)2-.

[0018] Optionally, X1, X2, X3 and X4 respectively include any one of -(C=O)O-, -O(C=O)-, -O-, -S-, -SO2-, -SO-, -C(O)-, -CH2-, -C(CH3)2- and -C(CF3)2-.

[0019] This application also provides a method for preparing a naphthalene-containing polyesterimide resin, wherein the method for preparing the naphthalene-containing polyesterimide resin as described above includes the following steps:

[0020] A naphthalene ring-containing diamine monomer, a dianhydride monomer, and a solvent are mixed and subjected to a polycondensation reaction to obtain a polyesteramic acid solution.

[0021] The polyesteramide acid solution is shaped and subjected to an imidization reaction to obtain a polyesterimide resin containing a naphthalene ring.

[0022] Optionally, the molar ratio between the dianhydride monomer and the naphthalene-containing diamine monomer is 0.98 to 1.02;

[0023] And / or, the mass ratio of the solvent to the total mass of the dianhydride monomer and the naphthalene-containing diamine monomer is 10 to 30;

[0024] And / or, the temperature of the polycondensation reaction is -5 to 30°C, and the time of the polycondensation reaction is 6 to 24 hours;

[0025] And / or, the heating rate of the imidization reaction is 1–20 °C / min;

[0026] And / or, the imidization reaction is carried out at a temperature of 30–400°C.

[0027] Optionally, the solvent includes any one or more of N,N-dimethylformamide, N-methylpyrrolidone, N,N-dimethylacetamide, dimethyl sulfoxide, and γ-butyrolactone.

[0028] Optionally, the naphthalene-containing diamine monomer has the structure shown in formula (6), and the dianhydride monomer has the structure shown in formula (7):

[0029]

[0030] Among them, A1, A2 and A3 respectively include any one of aromatic groups and heterocyclic compounds with 1-20 carbon atoms;

[0031] X1, X2, X3 and X4 are all low polar groups, and at least two of X1, X2, X3 and X4 are ester bonds;

[0032] R1, R2, R3, R4, R5, and R6 respectively include H, F, Cl, Br, I, CN, NH2, and C. r+1 H 2r+2 C r H2 r+1 C r H 2r+1 COOH, OC r H 2r+1 CF3, C(CH3)3, Any one of them.

[0033] This application discloses a naphthalene-containing polyesterimide resin. By introducing a large number of low-polarity groups into the polyimide molecular chain, the proportion of polar groups in the polyimide molecular chain is reduced, while ensuring that the polyesterimide resin contains at least two ester bonds. Since ester bonds, compared to other low-polarity groups, reduce the polarity of the polyesterimide resin without affecting its heat resistance, coefficient of thermal expansion, or other properties, a polyesterimide resin with low dielectric loss, dielectric constant, and water absorption can be obtained. Simultaneously, by replacing the conventional benzene ring with a naphthalene ring, the regularity of the molecular chain can be disrupted, thereby giving the polyesterimide resin good toughness and solubility. While ensuring the resin has low dielectric constant, dielectric loss, and water absorption, the problem of poor solubility of polyimide resins is effectively solved. Attached Figure Description

[0034] Figure 1 This is a schematic flowchart of the method for preparing naphthalene-containing polyesterimide resin involved in the embodiments of this application;

[0035] Figure 2 The Fourier transform infrared spectrum of the naphthalene ring-containing polyesterimide resin prepared in Example 1 of this application;

[0036] Figure 3 This is the thermogravimetric spectrum of the naphthalene ring-containing polyesterimide resin prepared in Example 1 of this application.

[0037] The realization of the purpose, functional features and advantages of this application will be further explained in conjunction with the embodiments and with reference to the accompanying drawings. Detailed Implementation

[0038] To make the objectives, technical solutions, and advantages of the embodiments of this application clearer, the technical solutions in the embodiments of this application will be clearly and completely described below. Where specific conditions are not specified in the embodiments, conventional conditions or conditions recommended by the manufacturer shall apply. Reagents or instruments whose manufacturers are not specified are all conventional products that can be purchased commercially.

[0039] Furthermore, the meaning of "and / or" throughout the text includes three parallel solutions. Taking "A and / or B" as an example, it includes solution A, solution B, or a solution that simultaneously satisfies A and B. In addition, the technical solutions of the various embodiments can be combined with each other, but this must be based on the ability of those skilled in the art to implement them. When the combination of technical solutions is contradictory or impossible to implement, it should be considered that such a combination of technical solutions does not exist and is not within the scope of protection claimed in this application. Based on the embodiments in this application, all other embodiments obtained by those skilled in the art without inventive effort are within the scope of protection of this application.

[0040] The first aspect of this application provides a naphthalene-containing polyesterimide resin, wherein the naphthalene-containing polyesterimide resin has the structure shown in formula (1):

[0041]

[0042] Where n is greater than or equal to 1;

[0043] A1, A2, and A3 each include any one of aromatic and heterocyclic compounds with 1-20 carbon atoms, whether substituted or unsubstituted;

[0044] In this embodiment, A1, A2, and A3 are selected from any one of aromatic groups and heterocyclic compounds, respectively. By introducing low-polarity groups, the proportion of polar groups in the molecular chain is reduced, thereby reducing the dielectric loss, dielectric constant, and water absorption of the polyesterimide resin. Furthermore, the introduction of pure extended-chain structures is avoided; for example, any one of A1, A2, and A3 is a substituted or unsubstituted alkyl group. Because it is a pure extended-chain structure, the molecular chain is also extended, leading to increased molecular rigidity, reduced entanglement, insufficient toughness of the polyesterimide resin, and difficulty in bending. Simultaneously, the close distance between molecular chains results in stronger intermolecular forces, making it difficult for solvents to penetrate and reducing solubility. In contrast, A1, A2, and A3 in this application each include any one of substituted or unsubstituted aromatic groups with 1-20 carbon atoms and heterocyclic compounds, which can disrupt the regularity of the molecular chain, thereby improving the toughness and solubility of the polyesterimide resin, making it more suitable for application in electronic packaging materials or circuit boards.

[0045] X1, X2, X3 and X4 are all low polar groups, and at least two of X1, X2, X3 and X4 are ester bonds;

[0046] In this embodiment, X1, X2, X3, and X4 are all low-polarity groups, and at least two of X1, X2, X3, and X4 are ester bonds. By introducing a large number of low-polarity groups into the polyimide molecular chain, the proportion of polar groups in the polyimide molecular chain is reduced, while ensuring that the polyesterimide resin contains at least two ester bonds. Since ester bonds, compared to other low-polarity groups, reduce the polarity of the polyesterimide resin without affecting its heat resistance, coefficient of thermal expansion, or other properties; for example, introducing fluorinated groups to modify the polyimide resin; fluorinated groups have strong electronegativity and other properties, which can be used to prepare polyimide films with low dielectric constant, good solubility, and high transparency. However, the introduction of fluorinated groups leads to an increase in the coefficient of thermal expansion, making it difficult to match the polyimide resin with metals such as copper; while ester bonds reduce the polarity of the polyesterimide resin without affecting its other properties; therefore, a polyesterimide resin with lower dielectric loss, dielectric constant, and water absorption can be obtained.

[0047] R1, R2, R3, R4, R5, and R6 respectively include H, F, Cl, Br, I, CN, NH2, and C. r+1 H 2r+2 C r H2 r+1 C r H 2r+1 COOH, OC r H 2r+1 CF3, C(CH3)3, Any one of them.

[0048] In this embodiment, R1, R2, R3, R4, R5 and R6 are selected from groups with low polarity, which can avoid increasing the polarity of the polyesterimide and keep it with low dielectric loss, dielectric constant and water absorption.

[0049] In one feasible embodiment, any one or more of A1, A2 and A3 are any one of substituted aromatic groups and heterocyclic compounds having 1-20 carbon atoms, and their substituents include any one of hydrogen atoms, alkoxy groups, aralkyl groups, alkyl groups having 1-6 carbon atoms and haloalkyl groups.

[0050] In one feasible embodiment, A1, A2, and A3 respectively have the structure shown in any one of equations (2), (3), (4), and (5):

[0051]

[0052] Among them, B1, B2, B3, B4, B5, B6, B7, and B8 respectively include H, F, Cl, Br, I, CN, NH2, and C. r+1 H 2r+2 C r H2 r+1 C r H 2r+1 COOH, OC r H 2r+1 CF3, C(CH3)3, Any one of them.

[0053] In this embodiment, formulas (2) and (5) can increase the number of benzene rings in the polyesterimide resin, reducing the proportion of polar groups, thereby further reducing polarity and decreasing the dielectric loss, dielectric constant, and water absorption of the polyesterimide resin. Although formulas (2) and (5) have higher symmetry than formulas (3) and (4), i.e., better molecular chain regularity, the repeating unit of the polyesterimide resin itself contains a naphthalene ring, which can greatly improve the solubility of the polyesterimide resin. Therefore, the introduction of formulas (2) and (5) can still maintain good toughness and solubility of the polyesterimide resin. Formulas (3) and (4) are meta-substitution and 2,6-position substitution, respectively, with poor symmetry, which can disrupt the regularity of the polyesterimide molecular chain and improve the toughness and solubility of the polyesterimide resin. Furthermore, the naphthalene ring in formula (4) can further disrupt the regularity of the molecular chain and improve the toughness and solubility of the polyesterimide resin.

[0054] In one feasible embodiment, any one or more of A1, A2 and A3 have a structure represented by D1-L-D2, wherein D1 and D2 have structures represented by any one of formulas (2), (3), (4) and (5), respectively, and L is a low polar group.

[0055] Optionally, L includes any one of -(C=O)O-, -O(C=O)-, -O-, -S-, -SO2-, -SO-, -C(O)-, -CH2-, -C(CH3)2- and -C(CF3)2-.

[0056] In this embodiment, L is selected from low polar groups, which can avoid increasing the polarity of the polyesterimide, thus maintaining its low dielectric loss, dielectric constant, and water absorption. The polyesterimide molecular chain simultaneously contains multiple structures from formulas (2), (3), (4), and / or (5), thereby improving the toughness and solubility of the polyesterimide resin, or reducing the dielectric loss, dielectric constant, and water absorption of the polyesterimide resin while maintaining its good toughness and solubility.

[0057] In one feasible embodiment, X1, X2, X3 and X4 respectively include any one of -(C=O)O-, -O(C=O)-, -O-, -S-, -SO2-, -SO-, -C(O)-, -CH2-, -C(CH3)2- and -C(CF3)2-, and at least two of X1, X2, X3 and X4 are ester bonds, that is, -(C=O)O- and / or -O(C=O)-.

[0058] In this embodiment, X1, X2, X3, and X4 are selected from low-polarity groups. All X1, X2, X3, and X4 are low-polarity groups, and at least two of X1, X2, X3, and X4 are ester bonds. By introducing a large number of low-polarity groups into the polyimide molecular chain, the proportion of polar groups in the polyimide molecular chain is reduced, while ensuring that the polyesterimide resin contains at least two ester bonds. Since ester bonds, compared to other low-polarity groups, reduce the polarity of the polyesterimide resin without affecting its heat resistance, coefficient of thermal expansion, or other properties; for example, introducing fluorinated groups to modify the polyimide resin; fluorinated groups have strong electronegativity and other properties, which can be used to prepare polyimide films with low dielectric constant, good solubility, and high transparency. However, the introduction of fluorine-containing groups leads to an increase in the coefficient of thermal expansion, making it difficult to match polyimide resin with metals such as copper. Ester bonds, on the other hand, reduce the polarity of polyesterimide resin without affecting its other properties. Therefore, polyesterimide resin with lower dielectric loss, dielectric constant and water absorption can be obtained.

[0059] The second aspect of this application provides a method for preparing a naphthalene-containing polyesterimide resin, referring to... Figure 1 The preparation method of naphthalene ring-containing polyesterimide resin includes the following steps:

[0060] Step S10: The diamine monomer containing a naphthalene ring, the dianhydride monomer, and the solvent are mixed and subjected to a polycondensation reaction to obtain a polyesteramic acid solution.

[0061] A polycondensation reaction is carried out by mixing a diamine monomer containing a naphthalene ring and a dianhydride monomer in a solvent to obtain a polyesteramide acid solution.

[0062] In one feasible embodiment, the molar ratio between the dianhydride monomer and the diamine monomer containing a naphthalene ring is 0.98 to 1.02; for example, the molar ratio between the dianhydride monomer and the diamine monomer containing a naphthalene ring is (0.98:1), (0.99:1), (1:1), (1.01:1), (1.02:1), etc.

[0063] In one feasible embodiment, the mass ratio of the solvent to the total mass of the dianhydride monomer and the naphthalene-containing diamine monomer is 10 to 30; for example, the mass ratio of the solvent to the total mass of the dianhydride monomer and the naphthalene-containing diamine monomer is (10:1), (15:1), (20:1), (25:1), (30:1), etc.

[0064] Optionally, the solvent is an organic solvent, including any one or more of N,N-dimethylformamide, N-methylpyrrolidone, N,N-dimethylacetamide, dimethyl sulfoxide, and γ-butyrolactone. This can provide a polycondensation reaction environment for the dianhydride monomer and the naphthalene-containing diamine monomer.

[0065] Optionally, the temperature of the polycondensation reaction is -5 to 30°C; for example, -5°C, 0°C, 5°C, 10°C, 15°C, 20°C, 25°C, 30°C, etc.

[0066] Optionally, the polycondensation reaction time is 6 to 24 hours; for example, 6 hours, 10 hours, 15 hours, 20 hours, 24 hours, etc.

[0067] In one feasible embodiment, the naphthalene-containing diamine monomer has the structure shown in formula (6), and the dianhydride monomer has the structure shown in formula (7):

[0068]

[0069] Among them, A1, A2 and A3 respectively include any one of the aromatic groups and heterocyclic compounds with 1-20 carbon atoms that are substituted or unsubstituted;

[0070] X1, X2, X3 and X4 are all low polar groups, and at least two of X1, X2, X3 and X4 are ester bonds;

[0071] R1, R2, R3, R4, R5, and R6 respectively include H, F, Cl, Br, I, CN, NH2, and C. r+1 H 2r+2 C r H2 r+1 C r H 2r+1 COOH, OC r H 2r+1 CF3, C(CH3)3, Any one of them.

[0072] Optionally, the substituents of any one or more of A1, A2 and A3 include any one of hydrogen atom, alkoxy, aralkyl, alkyl with 1-6 carbon atoms and haloalkyl.

[0073] Optionally, A1, A2, and A3 respectively have the structure shown in any one of equations (2), (3), (4), and (5):

[0074]

[0075] Among them, B1, B2, B3, B4, B5, B6, B7, and B8 respectively include H, F, Cl, Br, I, CN, NH2, and C. r+1 H 2r+2 C r H2 r+1 C r H 2r+1 COOH, OC r H 2r+1CF3, C(CH3)3, Any one of them.

[0076] Optionally, any one or more of A1, A2 and A3 have a structure represented by D1-L-D2, wherein D1 and D2 have structures represented by any one of formulas (2), (3), (4) and (5), respectively, and L is a low polar group.

[0077] Optionally, L includes any one of -(C=O)O-, -O(C=O)-, -O-, -S-, -SO2-, -SO-, -C(O)-, -CH2-, -C(CH3)2- and -C(CF3)2-.

[0078] Optionally, X1, X2, X3 and X4 respectively include any one of -(C=O)O-, -O(C=O)-, -O-, -S-, -SO2-, -SO-, -C(O)-, -CH2-, -C(CH3)2- and -C(CF3)2-.

[0079] In step S20, the polyesteramide acid solution is shaped and subjected to an imidization reaction to obtain a polyesterimide resin containing a naphthalene ring.

[0080] To form a polyestermica solution, the polyestermica solution can be coated onto a board using methods such as spin coating or casting to form a polyestermica film. Then, the polyestermica film undergoes an imidization reaction, i.e., dehydration treatment, to obtain a polyesterimide resin containing naphthalene rings.

[0081] Optionally, the heating rate of the imidization reaction is 1 to 20 °C / min; for example, 1 °C / min, 5 °C / min, 10 °C / min, 15 °C / min, 20 °C / min, etc.

[0082] Optionally, the imidization reaction is carried out at a temperature of 30–400°C; for example, 30°C, 50°C, 100°C, 150°C, 200°C, 250°C, 300°C, 350°C, 400°C, etc.

[0083] Optionally, the imidization reaction is carried out at a temperature of 100–300°C for a holding time of 60–120 min.

[0084] Optionally, the chemical reaction formula for preparing the naphthalene ring-containing polyesterimide resin is as follows:

[0085]

[0086] In this embodiment, a naphthalene-containing diamine monomer is reacted with a dianhydride monomer to synthesize a polyesterimide acid solution containing a naphthalene ring and ester groups. This solution is then subjected to an imidization reaction to prepare a naphthalene-containing polyesterimide resin. By introducing a large number of low-polarity groups into the polyimide molecular chain, the proportion of polar groups in the polyimide molecular chain is reduced, while ensuring that the polyesterimide resin contains at least two ester bonds. Since ester bonds, compared to other low-polarity groups, reduce the polarity of the polyesterimide resin without affecting its heat resistance, coefficient of thermal expansion, or other properties, a polyesterimide resin with lower dielectric loss, dielectric constant, and water absorption can be obtained. Simultaneously, by replacing the conventional benzene ring with a naphthalene ring, the regularity of the molecular chain is disrupted, thereby giving the polyesterimide resin good toughness and solubility. While ensuring the resin has low dielectric constant, dielectric loss, and water absorption, the problem of poor solubility in polyimide resins is effectively solved.

[0087] In order to enable those skilled in the art to clearly understand the details and operations of the above embodiments of this application, and to demonstrate the significant improvement in performance of the embodiments of this application, the above technical solutions are illustrated below through multiple embodiments.

[0088] Example 1

[0089] (1) 1.9921g of naphthalene ring-containing diamine monomer mNm and 2.2917g of p-phenylene-bisphenyltriester dianhydride (TAHQ) were mixed in N,N-dimethylformamide, the total concentration of mNm and TAHQ was adjusted to 20wt%, and the mixture was subjected to polycondensation reaction at 20℃ for 4h to obtain mNm-T polyesteramic acid solution;

[0090] (2) Coat a thin film from the mNm-T polyesteramide acid solution onto a glass plate, place it in an oven to remove the solvent, and then place it in a muffle furnace. Heat at the following temperatures: 30–80℃ (heating rate 3℃ / min, holding time 60min), 80–150℃ (heating rate 3℃ / min, holding time 60min), 150–200℃ (heating rate 3℃ / min, holding time 50min), and 200–250℃ (heating rate 3℃ / min, holding time 60min).

[0091]

[0092] The imidization reaction was carried out by a heating program of 50 min to obtain polyester imide resin mNm-T.

[0093] The chemical reaction formula for the preparation method of polyesterimide resin mNm-T is as follows:

[0094] Fourier transform infrared spectroscopy analysis of mNm-T yielded the following results: Figure 2 As shown; refer to Figure 2 It can be seen that at 1775cm-1 1500cm -1 1255cm -1 The presence of symmetrical or asymmetric stretching vibration peaks of C=O and CO, as well as bending vibration stretching peaks of CN, indicates the successful preparation of the polyesterimide structure.

[0095] Thermogravimetric analysis was performed on mNm-T, and the results are as follows: Figure 3 As shown; refer to Figure 3 It can be seen that mNm-T has a very high thermal decomposition temperature in nitrogen, with thermal decomposition temperatures of 462℃ and 486℃ for 5% and 10% respectively, exhibiting very good thermal stability.

[0096] Solubility tests on mNm-T revealed that it is soluble in organic solvents such as N,N-dimethylformamide, N-methylpyrrolidone, N,N-dimethylacetamide, and dimethyl sulfoxide, demonstrating excellent solubility.

[0097] A transparent mNm-T thin film can be prepared by solvent evaporation, with a transmittance of 81% at 500 nm. The tensile strength of the mNm-T film is 113 MPa, the tensile modulus is 3.0 GPa, the elongation at break is 5.5%, and it exhibits good flexibility and can be bent. The dielectric constant of mNm-T at 10 GHz was measured using a split-column dielectric resonator to be 3.04, the dielectric loss was 0.0031, and the water absorption rate was 0.853%, demonstrating low dielectric constant, dielectric loss, and water absorption rate.

[0098] Example 2

[0099] (1) 1.9921g of naphthalene ring-containing diamine monomer pNp and 2.2917g of p-phenylene-bisphenyltriester dianhydride (TAHQ) were mixed in N,N-dimethylformamide, the total concentration of mNm and TAHQ was adjusted to 20wt%, and the mixture was subjected to polycondensation reaction at 20℃ for 4h to obtain pNp-T polyesteramic acid solution;

[0100] (2) The pNp-T polyester amide acid solution was scraped onto a glass plate to form a film, which was then placed in an oven to remove the solvent and placed in a muffle furnace. The imidization reaction was carried out according to the following heating programs: 30-80℃ (heating rate 1℃ / min, holding time 60min), 80-150℃ (heating rate 1℃ / min, holding time 60min), 150-200℃ (heating rate 1℃ / min, holding time 50min) and 200-250℃ (heating rate 1℃ / min, holding time 50min) to obtain the polyester imide resin pNp-T.

[0101] The chemical reaction formula for the preparation method of polyesterimide resin pNp-T is as follows:

[0102]

[0103] Fourier transform infrared spectroscopy analysis of pNp-T yielded the following results: Figure 2 As shown; refer to Figure 2 It can be seen that at 1775cm -1 1500cm -1 1255cm -1 The presence of symmetrical or asymmetric stretching vibration peaks of C=O and CO, as well as bending vibration stretching peaks of CN, indicates the successful preparation of the polyesterimide structure.

[0104] Thermogravimetric analysis of pNp-T was performed, and the results are as follows: Figure 3 As shown; refer to Figure 3 It can be seen that pNp-T has a very high thermal decomposition temperature in nitrogen, with thermal decomposition temperatures of 5% and 10% being 506℃ and 524℃ respectively, exhibiting very good thermal stability.

[0105] Solubility tests on pNp-T revealed that it is soluble in organic solvents such as N,N-dimethylformamide, N-methylpyrrolidone, N,N-dimethylacetamide, and dimethyl sulfoxide, demonstrating excellent solubility.

[0106] A semi-transparent pNp-T film can be prepared by solvent evaporation, with a transmittance of 38% at 500 nm. The pNp-T film has a tensile strength of 104 MPa, a tensile modulus of 2.0 GPa, an elongation at break of 7%, and good flexibility, allowing it to be bent. Using a split-column dielectric resonator, the dielectric constant of pNp-T at 10 GHz was measured to be 3.34, the dielectric loss was 0.0025, and the water absorption rate was 0.849%, exhibiting low dielectric constant, dielectric loss, and water absorption rate.

[0107] Comparative Example 1

[0108] (1) 1.7418 g of diamine monomer ppp and 2.2917 g of p-phenylene-bisphenyltriester dianhydride (TAHQ) were mixed in N,N-dimethylformamide, the total concentration of ppp and TAHQ was adjusted to 20 wt%, and the polycondensation reaction was carried out at 20 °C for 0.5 h to obtain ppp-T polyesteramic acid solution.

[0109] (2) The ppp-T polyester amide acid solution was scraped onto a glass plate to form a film, which was then placed in an oven to remove the solvent and placed in a muffle furnace. The imidization reaction was carried out according to the following heating programs: 30-80℃ (heating rate 3℃ / min, holding time 60min), 80-150℃ (heating rate 3℃ / min, holding time 60min), 150-200℃ (heating rate 3℃ / min, holding time 50min) and 200-250℃ (heating rate 3℃ / min, holding time 50min) to obtain the polyester imide resin ppp-T.

[0110] The chemical reaction formula for the preparation method of polyesterimide resin PP-T is as follows:

[0111]

[0112] Solubility tests on ppp-T revealed that it does not dissolve well in organic solvents such as N,N-dimethylformamide, N-methylpyrrolidone, N,N-dimethylacetamide, and dimethyl sulfoxide, indicating poor solubility.

[0113] An opaque PP-T film can be prepared by solvent evaporation, with a transmittance of 23% at 500 nm. The tensile strength of the PP-T film is 78 MPa, the tensile modulus is 3.1 GPa, and the elongation at break is 1.8%. It is brittle and cannot be bent. The dielectric constant of PP-T at 10 GHz was measured using a separation column dielectric resonator to be 3.23, the dielectric loss was 0.0025, and the water absorption rate was 0.603%. Due to the presence of numerous benzene rings in PP-T, it has low polarity, resulting in low dielectric constant, dielectric loss, and water absorption rate. However, since the PP monomer has a pure extended chain structure, the resulting PP-T molecular chain is also a straight extended chain, leading to high molecular rigidity, low entanglement, insufficient toughness and elongation at break, difficulty in bending, and poor solubility.

[0114] Comparative Example 2

[0115] (1) 1.7120 g of diamine monomer E-pNp and 2.0116 g of 4,4'-terephthalodioxydiphthalic anhydride (HQDA) were mixed in N,N-dimethylformamide, the total concentration of E-pNp and HQDA was adjusted to 20 wt%, and polycondensation reaction was carried out at 20 °C for 0.5 h to obtain E-pNp-H polyether ammonium acid solution;

[0116] (2) The E-pNp-H polyether amic acid solution was scraped onto a glass plate to form a film, which was then placed in an oven to remove the solvent and placed in a muffle furnace. The imidization reaction was carried out according to the following heating programs: 30-80℃ (heating rate 3℃ / min, holding time 60min), 80-150℃ (heating rate 3℃ / min, holding time 60min), 150-200℃ (heating rate 3℃ / min, holding time 50min) and 200-250℃ (heating rate 3℃ / min, holding time 50min) to obtain polyether imide resin E-pNp-H.

[0117] The chemical reaction formula for the preparation method of polyetherimide resin E-pNp-H is as follows:

[0118]

[0119] Solubility tests on E-pNp-H revealed that it is soluble in organic solvents such as N,N-dimethylformamide, N-methylpyrrolidone, N,N-dimethylacetamide, and dimethyl sulfoxide, indicating good solubility.

[0120] A transparent E-pNp-H film can be prepared by solvent evaporation, with a transmittance of 82% at 500 nm. The tensile strength of the E-pNp-H film is 103 MPa, the tensile modulus is 2.8 GPa, the elongation at break is 6.5%, and it exhibits good flexibility and can be bent. Using a separation column dielectric resonator, the dielectric constant of E-pNp-H at 10 GHz was measured to be 3.37, the dielectric loss was 0.0118, and the water absorption rate was 1.052%. Because E-pNp-H contains a naphthalene ring, it can disrupt the regularity of the molecular chain, giving it good toughness and solubility; however, the absence of ester bonds in E-pNp-H results in high overall polarity, leading to high water absorption and a high dielectric constant.

[0121] The above are merely preferred embodiments of this application and do not limit the patent scope of this application. Various modifications and variations can be made to this application by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of this application should be included within the patent protection scope of this application.

Claims

1. A polyesterimide resin containing a naphthalene ring, characterized in that, The naphthalene ring-containing polyesterimide resin has the structure shown in formula (1): Where n is greater than or equal to 1; A1, A2, and A3 each comprise any one of aromatic groups and heterocyclic compounds having 1-20 carbon atoms, wherein A1, A2, and A3 each have the structure shown in any one of formulas (2), (3), (4), and (5): Among them, B1, B2, B3, B4, B5, B6, B7, and B8 respectively include H, F, Cl, Br, I, CN, NH2, Cr+1H2r+2, CrH2r+1, CrH2r+1COOH, OCrH2r+1, CF3, and C(CH3)3. , and Any one of them; X1, X2, X3, and X4 are all low polar groups, and at least two of X1, X2, X3, and X4 are ester bonds. X1, X2, X3, and X4 respectively include any one of -(C=O)O-, -O(C=O)-, -O-, -S-, -SO2-, -SO-, -C(O)-, -CH2-, -C(CH3)2-, and -C(CF3)2-. R1, R2, R3, R4, R5, and R6 respectively include H, F, Cl, Br, I, CN, NH2, Cr+1H2r+2, CrH2r+1, CrH2r+1COOH, OCrH2r+1, CF3, and C(CH3)3. , and Any one of them.

2. The naphthalene-containing polyesterimide resin as described in claim 1, characterized in that, One or more of A1, A2 and A3 have a structure represented by D1-L-D2, wherein D1 and D2 have a structure represented by any one of formula (2), formula (3), formula (4) and formula (5), respectively, and L is a low polar group.

3. The naphthalene-containing polyesterimide resin as described in claim 2, characterized in that, The L includes any one of -(C=O)O-, -O(C=O)-, -O-, -S-, -SO2-, -SO-, -C(O)-, -CH2-, -C(CH3)2- and -C(CF3)2-.

4. A method for preparing a naphthalene ring-containing polyesterimide resin, characterized in that, The method for preparing the naphthalene-containing polyesterimide resin is applied to the preparation of the naphthalene-containing polyesterimide resin as described in any one of claims 1 to 3, and includes the following steps: A naphthalene ring-containing diamine monomer, a dianhydride monomer, and a solvent are mixed and subjected to a polycondensation reaction to obtain a polyesteramic acid solution. The polyesteramide acid solution is shaped and subjected to an imidization reaction to obtain a polyesterimide resin containing a naphthalene ring.

5. The method for preparing the naphthalene-containing polyesterimide resin as described in claim 4, characterized in that, The molar ratio between the dianhydride monomer and the naphthalene-containing diamine monomer is 0.98 to 1.02; And / or, the mass ratio of the solvent to the total mass of the dianhydride monomer and the naphthalene-containing diamine monomer is 10 to 30; And / or, the temperature of the polycondensation reaction is -5 to 30 °C, and the time of the polycondensation reaction is 6 to 24 h; And / or, the heating rate of the imidization reaction is 1~20 °C / min; And / or, the imidization reaction is carried out at a temperature of 30~400 °C.

6. The method for preparing the naphthalene-containing polyesterimide resin as described in claim 4, characterized in that, The solvent includes any one or more of N,N-dimethylformamide, N-methylpyrrolidone, N,N-dimethylacetamide, dimethyl sulfoxide, and γ-butyrolactone.

7. The method for preparing the naphthalene-containing polyesterimide resin as described in claim 4, characterized in that, The diamine monomer containing a naphthalene ring has the structure shown in formula (6), and the dianhydride monomer has the structure shown in formula (7): A1, A2, and A3 each comprise any one of aromatic groups and heterocyclic compounds having 1-20 carbon atoms, wherein A1, A2, and A3 each have the structure shown in any one of formulas (2), (3), (4), and (5): Among them, B1, B2, B3, B4, B5, B6, B7, and B8 respectively include H, F, Cl, Br, I, CN, NH2, Cr+1H2r+2, CrH2r+1, CrH2r+1COOH, OCrH2r+1, CF3, and C(CH3)3. , and Any one of them; X1, X2, X3, and X4 are all low polar groups, and at least two of X1, X2, X3, and X4 are ester bonds. X1, X2, X3, and X4 respectively include any one of -(C=O)O-, -O(C=O)-, -O-, -S-, -SO2-, -SO-, -C(O)-, -CH2-, -C(CH3)2-, and -C(CF3)2-. R1, R2, R3, R4, R5, and R6 respectively include H, F, Cl, Br, I, CN, NH2, Cr+1H2r+2, CrH2r+1, CrH2r+1COOH, OCrH2r+1, CF3, and C(CH3)3. , and Any one of them.

Citation Information

Patent Citations

  • Transparent polyesterimide resin and preparing method thereof

    CN105085912A