A carboxyl-terminated polyether, its preparation method and application
By converting hydroxyl-terminated polyethers into carboxyl-terminated polyethers through carboxylation, the problems of reaction instability and poor product performance in existing technologies are solved, and high-purity carboxyl-terminated polyethers are prepared. This method is suitable for the synthesis of polyether amide elastomers and can be applied in a variety of fields.
Patent Information
- Application Number
- CN202311600551.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-28
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-11-28
AI Technical Summary
In the preparation of polyether amide elastomers, the selection of end groups in the existing technology leads to unstable reactions, difficulty in controlling esterification reactions, numerous side reactions, poor product performance, and complex processes.
A carboxymethylation reaction was used to convert hydroxyl-terminated polyethers into carboxyl-terminated polyethers. Hydroxyl hydrogen was removed by sodium ethoxide, and chlorocarboxylic acid was used as the carboxymethylation reagent. Combined with extraction and recrystallization purification, high-purity carboxyl-terminated polyethers were obtained.
The reaction stability and purity were improved, and the process was simplified. The prepared carboxyl-terminated polyether exhibited good elasticity and strength when used in polyetheramide elastomers, making it suitable for applications in automobiles, sporting goods, medical supplies, and mechanical parts.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of polymer technology, specifically relating to a carboxyl-terminated polyether, its preparation method, and its application. Background Technology
[0002] Polyethers are polymers formed by the ring-opening reaction of compounds containing epoxy structures with organic compounds containing active hydrogen, resulting in polymers with ether bonds in their main molecular chain. Common compounds containing epoxy structures include ethylene oxide (EO), propylene oxide (PO), and tetrahydrofuran (THF).
[0003] Polyethers have a wide range of applications, and in the polymer field, they are often used as copolymer units in elastomers. For example, in polyamide elastomers, polyethers are copolymerized with polyamides as soft segments to obtain polyetheramide elastomers. Polyetheramide elastomers have high strength, high toughness, good elasticity, low specific gravity, good resistance to flexural fatigue, good wear resistance, and good low-temperature performance, and can be widely used in automobiles, sporting goods, medical supplies, seals, and mechanical parts.
[0004] In the synthesis of polyether amides, the properties of the polyether end groups directly affect the performance of the reactive products. Hydroxyl-terminated polyethers, such as polyethylene glycol (PEG), polypropylene glycol (PPG), and polytetrahydrofuran glycol (PTMG), are the most common comonomers for polyether amide elastomers.
[0005] Invention patent CN 105566639A describes a polyamide 1012-based thermoplastic elastomer material and its preparation method. It uses long-chain nylon 1012 as the hard segment and polyether diol as the soft segment, and performs a melt copolymerization reaction at a vacuum of 20-1000 Pa and a reaction temperature of 150-300℃ to prepare the polyamide 1012-based polyamide elastomer. This method requires an esterification reaction between the terminal carboxyl groups of the polyamide and the terminal hydroxyl groups of the polyether polyol. Because the esterification reaction has a small equilibrium constant, it places high demands on the reaction apparatus and vacuum conditions. Furthermore, the reaction requires the addition of a highly active catalyst, which easily leads to side reactions, resulting in a deterioration in the product's appearance and performance.
[0006] Amino-terminated polyethers can also be used as comonomers for polyetheramide elastomers. Invention patent CN109206613A uses polyamide 6 and amino-terminated polyethers to synthesize polyetheramide elastomers. Using amino-terminated polyethers instead of hydroxyl polyethers in the reaction solves the problem of difficult esterification of hydroxyl polyethers to some extent. However, amino-terminated polyethers are mostly prepared by hydroammoniation of polyether polyols, generally leaving polyether polyol residues. This can lead to monomer residues in the polymerized polyetheramide elastomer, affecting product performance, and can also affect the molar ratio of carboxyl and amino groups, resulting in unstable reaction rates. Polyetheramide elastomers obtained using amino-terminated polyethers have a strong odor, requiring repeated boiling water extraction to reduce the odor and improve performance, making the process complex.
[0007] Invention patent CN113861412B discloses a method for synthesizing carboxyl-terminated polyethers and using them to prepare polyether amide elastomers. Carboxyl-terminated polyethers can be prepared by reacting hydroxyl polyethers with acid anhydrides. The preparation method includes: dehydrating the hydroxyl polyether at 100-120℃ under vacuum (e.g., -0.1MPa) for 3-4 hours until the moisture content is less than 100ppm; then adding acid anhydride at normal pressure, with a molar ratio of acid anhydride to hydroxyl polyether of 2.05-2.2:1; reacting for 4-6 hours; and then removing low-boiling points under vacuum to obtain the carboxyl-terminated polyether. The method for preparing polyether amide elastomer includes the following steps: (1) adding diacid, diamine, lactam, carboxyl-terminated polyether, carboxyl activator, catalyst, and stabilizer into a reaction vessel; the mass ratio of the carboxyl-terminated polyether to the total mass of the diacid, diamine, and lactam is 30-150:100; the molar ratio of the total carboxyl groups of the carboxyl-terminated polyether and diacid to the amine groups of the diamine is 1:1; (2) heating to 190-210℃ and holding the reaction under pressure for 3-6 hours at a pressure of 0.5-1.5 MPa. During the reaction, the pH of the liquid phase in the reaction vessel is adjusted to neutral by adding diacid and / or diamine. Then, the temperature is raised to 220-230℃, and the reaction is carried out under vacuum for 1-4 hours. The polyether amide elastomer is then discharged. The carboxyl-terminated polyether of this invention is prepared by reacting polyether polyol with acid anhydride. Because the terminal carboxyl groups of this type of end-carboxylic acid polyether are still connected to the polyether segments by ester bonds, they are still susceptible to hydrolytic breakage during polymerization, leading to reduced polymer viscosity, difficulty in reaction, and the need for more auxiliaries such as carboxyl activators and catalysts during the reaction, which affects the appearance and performance of the final product. Summary of the Invention
[0008] To address the aforementioned technical problems and shortcomings in this field, the present invention provides a carboxyl-terminated polyether, its preparation method, and its applications. The present invention utilizes the principle of carboxymethylation to convert hydroxyl-terminated polyethers into carboxyl-terminated polyethers. The reaction of the carboxyl-terminated polyether synthesized by the present invention with polyamide is simple, requires no catalyst, and yields a polyetheramide elastomer with good elasticity and high strength, suitable for applications in automobiles, sporting goods, medical supplies, seals, and mechanical parts.
[0009] To achieve the above technical objectives, the technical solution adopted in the embodiments of the present invention is as follows:
[0010] In a first aspect, embodiments of the present invention provide a method for preparing carboxyl-terminated polyethers, comprising the following steps:
[0011] (1) Add hydroxyl-terminated polyether and sodium ethoxide to the reactor in sequence. Under nitrogen protection, heat to 70-80℃ and stir for 3-5 hours. Then, evacuate to an absolute pressure of 50-200 Pa and continue the reaction for 10-15 hours to obtain sodium polyether alcohol.
[0012] (2) Slowly add chlorocarboxylic acid to the reactor, maintain the reaction temperature at 70-80℃, keep the absolute pressure of the system at 50-200Pa, and continue stirring the reaction for 8-10 hours to generate carboxyl-terminated polyether and its sodium salt.
[0013] (3) Cool the reactor to 50-60℃, add hydrogen chloride ethanol solution, stir for 1-2 hours, let stand for 3-5 hours to separate the layers, take out the material in the reactor, filter to remove salt, vacuum dry to remove solvent, and obtain coarse-end carboxyl polyether.
[0014] (4) Add the coarse-end carboxyl polyether to deionized water, stir and disperse, continue stirring for 3-5 hours, then filter and wash with water to further remove water-soluble impurities;
[0015] (5) Add the washed crude carboxyl polyether to anhydrous ethanol and heat to 30-40℃. After the carboxyl polyether is completely dissolved, slowly cool to 10-15℃ and wait for crystals to precipitate. After filtration, vacuum dry to remove the solvent and obtain carboxyl polyether with a purity greater than >99%.
[0016] Further, the hydroxyl-terminated polyether in step (1) is polypropylene glycol or polytetrahydrofuran ether glycol with a molecular weight of 300-3000.
[0017] Furthermore, in step (1), the molar ratio of sodium ethoxide to hydroxyl-terminated polyether is 2.5-4.0.
[0018] Furthermore, in step (2), the chlorocarboxylic acid is one or more of 2-chloropropionic acid, 2-chlorobutyric acid, and 2-chlorovaleric acid;
[0019] The molar ratio of the chlorocarboxylic acid and the hydroxyl-terminated polyether is 2.5-4.0.
[0020] Furthermore, in step (3), the concentration of the hydrogen chloride ethanol solution is 5-10%;
[0021] The amount of hydrogen chloride ethanol solution added is 3-4 times the amount of hydroxyl-terminated polyether added, based on mass.
[0022] Furthermore, in step (4), the amount of deionized water used is 5-10 times the amount of coarse-end carboxyl polyether by mass.
[0023] Further, in step (5), the amount of anhydrous ethanol added is 2-3 times the amount of coarse-end carboxyl polyether by mass.
[0024] Secondly, embodiments of the present invention provide a carboxyl-terminated polyether, which is prepared using the preparation method described in the first aspect.
[0025] Thirdly, embodiments of the present invention provide the application of the carboxyl-terminated polyether described in the second aspect, wherein the carboxyl-terminated polyether is used to prepare polyetheramide elastomers.
[0026] Compared with the prior art, the advantages and positive effects of the present invention are as follows:
[0027] 1) In the preparation method of carboxyl-terminated polyether of the present invention, sodium ethoxide is used to remove the hydroxyl hydrogen of the terminal hydroxyl polyether during the reaction process, and ethanol generated in the reaction is removed by vacuum, thereby improving the utilization rate of reaction raw materials and the reaction conversion rate.
[0028] 2) The method for preparing carboxyl-terminated polyethers of the present invention uses chloropropionic acid, chlorobutyric acid and other substances with long carbon chains as carboxyl methylation reagents, which improves the compatibility of the system materials and increases the reaction rate. After purification by extraction, recrystallization and other processes, the resulting carboxyl-terminated polyether has high purity and can be used to synthesize polyether amide elastomers.
[0029] 3) The carboxyl-terminated polyether prepared by the method of the present invention does not contain ester bonds and has good reaction stability in the synthesis of polyether amide elastomer. Detailed Implementation
[0030] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.
[0031] The evaluation method used in the examples is as follows:
[0032] 1) Acid value and purity of carboxyl-terminated polyethers
[0033] Accurately weigh 0.03-0.04 g of carboxyl-terminated polyether sample and dissolve it in 40 ml of a 1:1 mixture of ethylene glycol and isopropanol. Add 3-5 drops of 0.05% methyl red or methyl orange alcohol solution and titrate with 0.2 mol / L sodium hydroxide in ethylene glycol / isopropanol standard solution until the pink color turns yellow. Perform a blank test.
[0034] Product purity = Acid value obtained from titration / Theoretical acid value
[0035] 2) Relative viscosity of polyetheramide elastomer
[0036] Accurately weigh 0.25g of polyetheramide elastic resin and add it to 25ml of m-cresol. Stir and dissolve at 20-30℃. After complete dissolution, place the solution in an Ubbelohde viscometer and incubate at 25℃ for 10 minutes, then measure the rate of descent (t). Simultaneously, measure the rate of descent (t0) of m-cresol under the same conditions. Calculate the relative viscosity from t and t0 using the following formula:
[0037] Relative viscosity = t / t0.
[0038] 3) Tensile strength
[0039] It is melted in an injection molding machine at a temperature 30°C above the melting point of the polyamide elastomer resin, under an injection pressure of 600 kgf / cm². 2 Injection-molded sheets were obtained under the conditions of 1.0 second injection time and 40℃ mold temperature. The obtained injection-molded sheets were annealed at 25℃ for 24 hours and then tested under absolutely dry conditions. Tensile strength and elongation at break were determined according to GB / T 1040.1-2018, Determination of Tensile Properties of Plastics.
[0040] 4) Hardness
[0041] The Shore hardness of a 6mm thick circular sample was determined according to GB / T 2411-2008, the standard for determining indentation hardness (Shore hardness) of plastics and hard rubber using a hardness tester.
[0042] Example 1
[0043] A method for preparing a carboxyl-terminated polyether includes the following steps:
[0044] (1) Add 1000g of polytetrahydrofurandiol (Mitsubishi Chemical PTMG1000) with an average molecular weight of 1000 and 240g of sodium ethoxide to the reactor in sequence. Under nitrogen protection, heat to 70℃ and stir for 5 hours. Then, evacuate to an absolute pressure of 100Pa and continue the reaction for 12 hours. The reaction equation of polytetrahydrofurandiol and sodium ethoxide is as follows:
[0045]
[0046] (2) Slowly add 360g of 2-chloropropionic acid to the reactor, control the reaction temperature at 70℃, maintain the absolute pressure of the system at 100Pa, and stir the reaction for 8 hours; the reaction equation of sodium polyether alcohol and 2-chloropropionic acid is as follows:
[0047]
[0048] (3) Cool the reactor to 50°C, add 3000g of 5% hydrogen chloride ethanol solution, stir for 1 hour, let stand for 4 hours, filter the material in the reactor, remove the solvent using a rotary evaporator, and obtain 1098g of white crude carboxyl-terminated polyether solid.
[0049] (4) Add the crude carboxyl-terminated polyether to 8000g of deionized water, stir for 3 hours, wash with water and filter to obtain the washed crude carboxyl-terminated polyether.
[0050] (5) Add the crude carboxyl polyether to 2500g of anhydrous ethanol, heat to 30°C, stir continuously until the carboxyl polyether is completely dissolved, slowly cool to 10°C, wait for crystals to precipitate, filter, vacuum dry to remove solvent, and obtain 760g of carboxyl polyether.
[0051] Based on the hydroxyl value of PTMG1000 (112.6 mg KOH / g), the theoretical acid value of the carboxyl-terminated polyether was 1.753 mmol / g. The acid value of the carboxyl-terminated polyether was measured to be 1.740 mmol / g, and the purity was calculated to be 99.2%.
[0052] The method for preparing polyetheramide elastomers using the above-mentioned carboxyl-terminated polyethers includes the following steps:
[0053] Add 500g of carboxyl-terminated polyether, 300g of dodecanoic acid, 150g of decanediamine, and 1000g of deionized water to the polymerization reactor. Purge oxygen twice with nitrogen, heat the polymerization reactor, and slowly increase the pressure until it reaches 1.2MPa. Slowly remove water vapor from the polymerization reactor to maintain the pressure at 1.2MPa. When the temperature of the polymerization reactor reaches 225℃, increase the venting volume to slowly reduce the pressure of the polymerization reactor to atmospheric pressure and the temperature of the polymerization reactor to 250℃. Then maintain the temperature of the polymerization reactor at 250℃, evacuate the polymerization reactor, and reduce the pressure of the polymerization reactor to 5000Pa (absolute pressure). React for 4 hours under the conditions of 250℃ and 5000Pa to obtain polyether amide elastomer.
[0054] The relative viscosity of the polyether amide elastomer was measured to be 2.4.
[0055] Example 2
[0056] A method for preparing a carboxyl-terminated polyether includes the following steps:
[0057] (1) Add 1000g of polytetrahydrofuran diol (Mitsubishi Chemical PTMG650) with an average molecular weight of 650 and 273g of sodium ethoxide to the reactor in sequence. Under nitrogen protection, heat to 70°C and stir for 5 hours. Then, evacuate to an absolute pressure of 100Pa and continue the reaction for 11 hours.
[0058] (2) Slowly add 435g of 2-chloropropionic acid into the reactor, control the reaction temperature at 70℃, maintain the absolute pressure of the system at 100Pa, and stir the reaction for 8 hours.
[0059] (3) Cool the reactor to 50°C, add 3600g of 5% hydrogen chloride ethanol solution, stir for 1 hour, let stand for 4 hours, filter the material in the reactor, remove the solvent using a rotary evaporator, and obtain 1156g of white crude carboxyl-terminated polyether solid.
[0060] (4) Add the crude carboxyl-terminated polyether to 8000g of deionized water, stir for 3 hours, wash with water and filter to obtain the washed crude carboxyl-terminated polyether.
[0061] (5) Add the crude carboxyl polyether to 2700g of anhydrous ethanol, heat to 30°C, stir continuously until the carboxyl polyether is completely dissolved, slowly cool to 10°C, wait for crystals to precipitate, filter, vacuum dry to remove solvent, and obtain 880g of pure carboxyl polyether.
[0062] Based on the hydroxyl value of PTMG650 (169.2 mg KOH / g), the theoretical acid value of the carboxyl-terminated polyether was 2.477 mmol / g. The acid value of the carboxyl-terminated polyether was measured to be 2.455 mmol / g, and the purity was calculated to be 99.1%.
[0063] The method for preparing polyetheramide elastomers using the above-mentioned carboxyl-terminated polyethers includes the following steps:
[0064] Add 500g of carboxyl-terminated polyether, 565g of dodecanoic acid, 316g of decanediamine, and 1000g of deionized water to a polymerization reactor. Purge oxygen twice with nitrogen, then heat the reactor to slowly increase the pressure to 1.3MPa. Slowly remove water vapor from the reactor to maintain the pressure at 1.3MPa. When the reactor temperature reaches 225℃, increase the venting rate to slowly reduce the pressure until it reaches atmospheric pressure and the reactor temperature reaches 250℃. Maintain the reactor temperature at 250℃, then evacuate the reactor and reduce the pressure to 5000Pa (absolute pressure). React at 250℃ and 5000Pa for 3 hours to obtain the polyether amide elastomer.
[0065] The relative viscosity of the polyether amide elastomer was measured to be 2.5.
[0066] Example 3
[0067] A method for preparing a carboxyl-terminated polyether includes the following steps:
[0068] (1) Add 1000g of polytetrahydrofuran diol (Mitsubishi Chemical PTMG2000) with an average molecular weight of 2000 and 136g of sodium ethoxide to the reactor in sequence. Under nitrogen protection, heat to 80°C and stir for 5 hours. Then, evacuate to an absolute pressure of 60Pa and continue the reaction for 14 hours.
[0069] (2) Slowly add 245g of 2-chlorobutyric acid to the reactor, control the reaction temperature at 80℃, maintain the absolute pressure of the system at 60Pa, and stir the reaction for 8 hours.
[0070] (3) Cool the reactor to 50°C, add 3200g of 5% hydrogen chloride ethanol solution, stir for 1 hour, let stand for 4 hours, filter the material in the reactor, remove the solvent using a rotary evaporator, and obtain 1050g of white crude carboxyl-terminated polyether solid.
[0071] (4) Add the crude carboxyl-terminated polyether to 7500g of deionized water, stir for 4 hours, wash with water and filter to obtain the washed crude carboxyl-terminated polyether.
[0072] (5) Add the crude carboxyl polyether to 2800g of anhydrous ethanol, heat to 30°C, stir continuously until the carboxyl polyether is completely dissolved, slowly cool to 10°C, wait for crystals to precipitate, filter, vacuum dry to remove solvent, and obtain 660g of pure carboxyl polyether.
[0073] Based on the hydroxyl value of the raw material PTMG2000 (56.2 mg KOH / g), the theoretical acid value of the carboxyl-terminated polyether was 0.922 mmol / g. The acid value of the carboxyl-terminated polyether was measured to be 0.914 mmol / g, and the purity was calculated to be 99.1%.
[0074] The method for preparing polyetheramide elastomers using the above-mentioned carboxyl-terminated polyethers includes the following steps:
[0075] Add 500g of carboxyl-terminated polyether, 105g of dodecanoic acid, 39g of decanediamine, and 500g of deionized water to the polymerization reactor. Purge oxygen twice with nitrogen, heat the polymerization reactor, and slowly increase the pressure until it reaches 1.2MPa. Slowly remove water vapor from the polymerization reactor to maintain the pressure at 1.2MPa. When the temperature of the polymerization reactor reaches 220℃, increase the venting rate to slowly reduce the pressure of the polymerization reactor until it reaches atmospheric pressure and the temperature reaches 250℃. Then maintain the temperature of the polymerization reactor at 250℃, evacuate the polymerization reactor, and reduce the pressure of the polymerization reactor to 2000Pa (absolute pressure). React for 5 hours at 250℃ and 2000Pa to obtain polyether amide elastomer.
[0076] The relative viscosity of the polyether amide elastomer was measured to be 2.2.
[0077] Example 4
[0078] A method for preparing a carboxyl-terminated polyether includes the following steps:
[0079] (1) Add 1000g of polypropylene glycol (Hai'an Petrochemical PPG-1000) with an average molecular weight of 1000 and 240g of sodium ethoxide to the reactor in sequence. Under nitrogen protection, heat to 80℃ and stir for 5 hours. Then, evacuate to an absolute pressure of 150Pa and continue the reaction for 10 hours.
[0080] (2) Slowly add 410g of 2-chlorobutyric acid to the reactor, control the reaction temperature at 70℃, maintain the absolute pressure of the system at 150Pa, and stir the reaction for 8 hours.
[0081] (3) Cool the reactor to 50°C, add 3600g of 5% hydrogen chloride ethanol solution, stir for 1 hour, let stand for 4 hours, filter the material in the reactor, remove the solvent using a rotary evaporator, and obtain 1006g of white crude carboxyl-terminated polyether solid.
[0082] (4) Add the crude carboxyl-terminated polyether to 8000g of deionized water, stir for 4 hours, wash with water and filter to obtain the washed crude carboxyl-terminated polyether.
[0083] (5) Add the crude carboxyl polyether to 2800g of anhydrous ethanol, heat to 30°C, and stir continuously until the carboxyl polyether is completely dissolved. Slowly cool to 10°C until crystals precipitate. After filtration, remove the solvent by vacuum drying to obtain 701g of pure carboxyl polyether.
[0084] Based on the hydroxyl value of PPG-1000 (113.8 mg KOH / g), the theoretical acid value of the carboxyl-terminated polyether was 1.727 mmol / g. The acid value of the carboxyl-terminated polyether was measured to be 1.711 mmol / g, and the purity was calculated to be 99.1%.
[0085] The method for preparing polyetheramide elastomers using the above-mentioned carboxyl-terminated polyethers includes the following steps:
[0086] 544g of carboxyl-terminated polyether, 295g of dodecanoic acid, 147g of decanediamine, and 1500g of deionized water were added to a polymerization reactor. Nitrogen was purged twice to remove oxygen. The reactor was heated, and the pressure was slowly increased to 1.5MPa. Water vapor was slowly released from the reactor to maintain the pressure at 1.5MPa. When the reactor temperature reached 230℃, the venting rate was increased to slowly reduce the pressure until atmospheric pressure was reached and the reactor temperature reached 250℃. The reactor temperature was then maintained at 250℃, and a vacuum was applied to reduce the pressure to 1000Pa (absolute pressure). The reaction was carried out at 250℃ and 3000Pa for 5 hours to obtain the polyether amide elastomer.
[0087] The relative viscosity of the polyether amide elastomer was measured to be 2.3.
[0088] Table 1 Performance parameters of polyetheramide elastomers in Examples 1-4 of the present invention
[0089]
[0090] As can be seen from Table 1, the polyetheramide elastomers obtained in Examples 1-4 have a wide hardness range, high tensile strength and elongation at break, and can meet the needs of various applications such as automobiles, sporting goods, medical supplies, seals, and mechanical parts.
[0091] Finally, it should be noted that the above specific embodiments are only used to illustrate the technical solutions of the present invention and not to limit it. Although the present invention has been described in detail with reference to examples, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention without departing from the spirit and scope of the technical solutions of the present invention, and all such modifications or substitutions should be covered within the scope of the claims of the present invention.
Claims
1. A method for preparing a carboxyl-terminated polyether, characterized in that, Includes the following steps: (1) Add hydroxyl-terminated polyether and sodium ethoxide to the reactor in sequence. Under nitrogen protection, heat to 70-80℃ and stir for 3-5 hours. Then, evacuate to an absolute pressure of 50-200 Pa and continue the reaction for 10-15 hours. (2) Slowly add chlorocarboxylic acid to the reactor, maintain the reaction temperature at 70-80℃, keep the absolute pressure of the system at 50-200Pa, and continue stirring the reaction for 8-10 hours; (3) Cool the reactor to 50-60℃, add hydrogen chloride ethanol solution, stir for 1-2 hours, let stand for 3-5 hours to separate the layers, take out the material in the reactor, filter to remove salt, vacuum dry to remove solvent, and obtain coarse-end carboxyl polyether. (4) Add the coarse-end carboxyl polyether to deionized water, stir and disperse, continue stirring for 3-5 hours, then filter and wash with water to further remove water-soluble impurities; (5) Add the washed crude carboxyl polyether to anhydrous ethanol and heat to 30-40°C. After the carboxyl polyether is completely dissolved, slowly cool to 10-15°C until crystals precipitate. After filtration, vacuum dry to remove the solvent and obtain carboxyl polyether with a purity greater than 99%.
2. The method for preparing carboxyl-terminated polyether according to claim 1, characterized in that, The hydroxyl-terminated polyether mentioned in step (1) is polypropylene glycol or polytetrahydrofuran ether glycol with a molecular weight of 300-3000.
3. The method for preparing carboxyl-terminated polyether according to claim 1, characterized in that, In step (1), the molar ratio of sodium ethoxide and hydroxyl-terminated polyether is 2.5-4.
0.
4. The method for preparing carboxyl-terminated polyether according to claim 1, characterized in that, In step (2), the chlorocarboxylic acid is one or more of 2-chloropropionic acid, 2-chlorobutyric acid and 2-chlorovaleric acid; The molar ratio of the chlorocarboxylic acid and the hydroxyl-terminated polyether is 2.5-4.
0.
5. The method for preparing carboxyl-terminated polyether according to claim 1, characterized in that, In step (3), the concentration of the hydrogen chloride ethanol solution is 5-10%; The amount of hydrogen chloride ethanol solution added is 3-4 times the amount of hydroxyl-terminated polyether added, based on mass.
6. The method for preparing carboxyl-terminated polyether according to claim 1, characterized in that, In step (4), the amount of deionized water used is 5-10 times that of coarse-end carboxyl polyether by mass.
7. The method for preparing carboxyl-terminated polyether according to claim 1, characterized in that, In step (5), the amount of anhydrous ethanol added is 2-3 times the amount of coarse-end carboxyl polyether by mass.
8. A carboxyl-terminated polyether, characterized in that, It is prepared by the preparation method according to any one of claims 1-7.
9. The application of the carboxyl-terminated polyether of claim 8, characterized in that, The carboxyl-terminated polyether is used to prepare polyetheramide elastomers.
Citation Information
Patent Citations
Polyamide 1012 serial thermoplastic elastomer material and preparation method thereof
CN105566639A
Preparation method of polyamide elastomer, elastomer prepared by preparation method and use of elastomer
CN109206613A
A method for preparing polyetheramide elastomer and its product
CN113861412B
Epoxy-terminated polyether and preparation method thereof and application thereof to serve as epoxy resin toughening agent
CN105906814A
Polyether surface active agent and synthetizing method thereof and neutral cleaning agent