A phthalonitrile resin, its preparation method, and its applications

By optimizing the raw material formulation and preparation method of phthalonitrile resin, the problem of resin having both low melting point and high temperature resistance in liquid phase molding process was solved, and a nitrile resin suitable for composite materials was prepared. A resin system with low viscosity and high heat resistance was achieved, which is suitable for liquid phase molding process and meets the application requirements of aerospace.

CN117510841BActive Publication Date: 2026-11-10NAT UNIV OF DEFENSE TECH
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311549402.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-20
Publication Date
2026-11-10
Estimated Expiration
2043-11-20

AI Technical Summary

Technical Problem

Existing phthalonitrile resins are difficult to combine low melting point, low viscosity, and high temperature resistance in liquid phase molding processes, which makes it difficult to prepare and mold composite materials.

Method used

By optimizing the raw material formulation and preparation method of phthalonitrile resin, and combining the principle of eutectic melting of mixtures, the dosage ratio of each monomer was adjusted to prepare a nitrile resin system suitable for liquid phase molding process. This system includes a mixture of 4-(4-aminophenoxy)phthalonitrile, 1,2-bis(3,4-diacryloxyphenoxy)benzene and 1,2-bis(2,3-diacryloxyphenoxy)benzene. The process involves grinding, ball milling or crushing, melt blending, degassing and curing.

Benefits of technology

This method achieves low viscosity and good heat resistance in resin systems at lower temperatures, making them suitable for liquid phase molding processes. The prepared composite materials have no obvious defects on the surface and cross-section, and possess excellent mechanical and dielectric properties, meeting the application requirements of the aerospace field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117510841B_ABST
    Figure CN117510841B_ABST
Patent Text Reader

Abstract

This invention discloses a phthalonitrile resin, its preparation method, and its applications, belonging to the field of high-temperature resistant resin composites. The phthalonitrile resin raw material formulation of this invention comprises, by mass percentage: 10-20 parts of 4-(4-aminophenoxy)phthalonitrile, and 80-90 parts of a mixture of 1,2-bis(3,4-diacryloxyphenoxy)benzene and 1,2-bis(2,3-diacryloxyphenoxy)benzene. The resin system of this invention has an initial melting temperature below 80℃, a minimum viscosity of approximately 40 mPa·s, a process window temperature range greater than 70℃, and a curing exothermic temperature range of 220-260℃. It is suitable for liquid phase molding processes, and the prepared resin-based carbon fiber reinforced composite material exhibits stable morphology, with no obvious cracks, pores, or voids on the surface, cross-section, or cut surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of high-temperature resistant resin composite materials, specifically relating to an orthophthalonitrile resin, its preparation method, and its application. Background Technology

[0002] Phthalonil resins have attracted much attention due to their excellent temperature resistance, processability, mechanical properties, flame retardancy, and low water absorption, and are widely used in the aerospace field. For example, early biphenyl-type phthalonitriles have excellent mechanical properties and temperature resistance, but their monomer melting point is as high as 234℃, posing numerous challenges to the preparation and molding of composite materials. Later, a large amount of resin research focused on how to reduce the melting point of phthalonitrile monomers. For example, some nitrile resin monomers such as aromatic ether type, alkyl chain type, and silane chain type were prepared. However, these monomers always fail to simultaneously possess low melting point, low viscosity, and high temperature resistance, making it difficult for nitrile resins to be used in liquid phase molding processes, such as RTM.

[0003] Therefore, it is necessary to develop a phthalonitrile resin composition that combines applicability to liquid phase molding processes and temperature resistance, so as to improve the liquid phase molding processability of nitrile resins and reduce the preparation cost of nitrile resin composites while ensuring temperature resistance. Summary of the Invention

[0004] The problem this invention aims to solve is to optimize the raw material formulation of phthalonitrile resin, improve the preparation method, and combine the properties and performance advantages of phthalonitrile monomers. Based on the principle of eutectic melting of mixtures, the proportion of each monomer is reasonably adjusted to formulate a nitrile resin system suitable for liquid phase molding of composite materials. This resin has a low melting temperature and extremely low viscosity in the molten state, making it suitable for preparing carbon fiber reinforced composite materials through liquid phase molding.

[0005] The present invention includes a phthalonitrile resin, wherein the raw material formulation of the phthalonitrile resin comprises, by mass percentage: 10-20 parts of 4-(4-aminophenoxy)phthalonitrile, and 80-90 parts of 1,2-bis(3,4-diacenicophenoxy)benzene and 1,2-bis(2,3-diacenicophenoxy)benzene.

[0006] Furthermore, the formulation comprises, by weight percentage: 20 parts of 4-(4-aminophenoxy)phthalonitrile, 30-50 parts of 1,2-bis(3,4-diacryloxyphenoxy)benzene, and the remainder being 1,2-bis(2,3-diacryloxyphenoxy)benzene.

[0007] Furthermore, this includes curing and crosslinking to generate isoindole, triazine rings, and phthalocyanine rings.

[0008] A method for preparing phthalonitrile resin as described in any of the above claims includes the following steps:

[0009] S1. Weigh the raw materials according to the formula, mix them, and grind them into powder to obtain the raw material powder;

[0010] S2. Melt and blend the raw material powder, cool it, and then grind it into powder again to obtain blended resin powder;

[0011] S2. Melt and degas the blended resin powder to obtain a fluidized resin;

[0012] S3. The fluidized resin is cured and molded to obtain a cured resin product.

[0013] Furthermore, in step S1, the method for mixing and pulverizing the raw materials is grinding and mixing, ball milling, or crushing and pulverizing.

[0014] Furthermore, step S2 specifically includes melting the raw material powder at 150-160°C and holding it at that temperature for 10-30 minutes. Step S3 specifically includes melting the blended resin powder at 150-160°C, evacuating it to -0.1 MPa, and holding it at that temperature for 30-60 minutes to remove bubbles.

[0015] Furthermore, the curing process in step S4 includes a heating process of 220°C for 2 hours, 240°C for 2 hours, and 260°C for 2 hours to obtain a preliminary cured product, followed by a process of 280°C for 2 hours to obtain a resin cured product.

[0016] Furthermore, prior to step S1, a method for preparing 4-(4-aminophenoxy)phthalonitrile is included, comprising: under nitrogen protection, mixing p-aminophenol, anhydrous potassium carbonate, and 4-nitrophthalonitrile in a molar ratio of 1.2:(1.4-1.6):1 with a solvent, wherein the mass or volume of the solvent is 5-6 times that of 4-nitrophthalonitrile, reacting at 60-80°C for 6-8 hours, pouring the resulting reaction mixture into water, precipitating a solid, filtering, washing, and then slurrying with 95% ethanol for 1-2 hours, filtering, and drying at 50-60°C for 2 hours followed by 105°C for 10 hours to constant weight, thereby obtaining the 4-(4-aminophenoxy)phthalonitrile monomer.

[0017] Furthermore, prior to step S1, a method for preparing 1,2-bis(3,4-diacetonitrile)benzene is included, comprising: under nitrogen protection, mixing catechol, anhydrous potassium carbonate, and 4-nitrophthalonitrile in a molar ratio of 0.5:(1.2-1.4):1 with a solvent, wherein the mass or volume of the solvent is 4-6 times that of the 4-nitrophthalonitrile; stirring at 40-80°C for 6-24 h; pouring the resulting reaction mixture into water to precipitate a solid; filtering, washing, and then slurrying with 95% ethanol for 1-2 h; filtering again; and drying at 50-60°C for 2 h followed by 120°C for 10 h to constant weight to obtain the 1,2-bis(3,4-diacetonitrile)benzene monomer.

[0018] Furthermore, prior to step S1, a method for preparing 1,2-bis(2,3-diacetonitrilephenoxy)benzene is included, comprising: under nitrogen protection, mixing catechol, anhydrous potassium carbonate, and 3-nitrophthalonitrile in a molar ratio of 0.5:(1.2-1.4):1 with a solvent, wherein the mass or volume of the solvent is 4-6 times that of the 3-nitrophthalonitrile; stirring at 40-60°C for 12-24 h; pouring the resulting reaction mixture into water to precipitate a solid; filtering, washing, and hot-beating with methanol for 1-2 h; filtering, and drying at 50-60°C for 2 h + 105°C for 10 h to constant weight to obtain 1,2-bis(2,3-diacetonitrilephenoxy)benzene monomer.

[0019] The application of the phthalonitrile resin described above or the phthalonitrile resin prepared by the above method is used to prepare resin-based carbon fiber reinforced composite materials by liquid phase molding process. This includes injecting the fluidized resin into a mold with carbon fiber woven fabric laid on it, fully impregnating it, and then curing it. The curing pressure is 0.2 to 1.5 MPa, and the heating program is 220℃ for 2 hours, 240℃ for 2 hours, and 260℃ for 2 hours. After natural cooling, the resin is demolded and then kept at 280℃ for 2 hours before natural cooling.

[0020] The beneficial effects of this invention are:

[0021] In the phthalonitrile resin formulation of this invention, 4-(4-aminophenoxy)phthalonitrile is a self-catalytic phthalonitrile resin monomer. One function of this monomer is as a curing agent in the curing reaction process of the resin in this formulation. If the amount is too small, the flexural strength of the resin will be too low; if the content is too large, the morphology of the cured product will be unqualified and the mechanical properties cannot be tested normally. The ratio of 1,2-bis(3,4-diacenicophenoxy)benzene to 1,2-bis(2,3-diacenicophenoxy)benzene affects the temperature at which the lowest viscosity is achieved and the heat resistance of the cured product, as well as the mechanical properties and dielectric properties. Other properties, such as viscosity, are not significantly affected. Specifically, there is a partial inverse relationship between the temperature at which the viscosity is lowest and the heat resistance of the cured product in this resin system. The ratio of 1,2-bis(3,4-diacenicophenoxy)benzene to 1,2-bis(2,3-diacenicophenoxy)benzene can be adjusted according to the product performance requirements to meet the viscosity and heat resistance requirements of different applications. The resin system in this invention has a melting point starting temperature of less than 80°C, which is lower than that of the prior art at a lower temperature. It also has good heat resistance, mechanical properties, and dielectric properties, meeting the requirements of liquid phase molding process.

[0022] This invention optimizes the raw material formulation of phthalonitrile resin and improves the preparation method. By combining the properties and performance advantages of phthalonitrile monomers and based on the principle of eutectic melting of mixtures, the proportions of each monomer are rationally adjusted to formulate a nitrile-based resin system suitable for liquid-phase molding processes of composite materials. This resin possesses a low melting temperature and extremely low viscosity in the molten state, making it suitable for preparing carbon fiber reinforced composite materials through liquid-phase molding. The resin system has a melting range initiation temperature below 80°C, a minimum melting endothermic peak temperature of approximately 106°C, and a maximum not exceeding 143.5°C. In the molten state, the viscosity is as low as 1000 mPa·s at 141°C. At 151℃, the viscosity is as low as 100 mPa·s, and the lowest viscosity is about 40 mPa·s, which meets the performance requirements of the equipment involved in the existing liquid phase molding process. The material loss during the curing process is 0.65%, and the material loss is 0.24% at the highest curing temperature of 300℃. The shrinkage rate of the cured product relative to the mold cavity is about 1%. The morphology of the cured product is stable, and there are no obvious cracks, pores or holes on the cross-section and surface. The curing exothermic temperature range is 220~260℃. At the highest curing temperature of 280℃, the flexural strength of the cured product can reach 135.21MPa, the flexural elastic modulus reaches 4.86GPa, and the 5% decomposition temperature is greater than 430℃.

[0023] The phthalonitrile resin system of the present invention is suitable for preparing composite materials by liquid phase molding process. The resulting composite material has a stable morphology and no obvious cracks, pores or holes on the surface and cross-section. Attached Figure Description

[0024] Appendix Figure 1 This is a DSC curve of the raw material powder obtained in S1 of Example 4 of the present invention;

[0025] Appendix Figure 2 This is a DSC curve of the blended resin obtained in S2 of Example 4 of the present invention;

[0026] Appendix Figure 3 This is the rheological viscosity-temperature curve of the blended resin obtained in S2 of Example 4 of the present invention;

[0027] Appendix Figure 4 This is a photograph of the cured resin obtained in S4 of Example 4 of the present invention.

[0028] Appendix Figure 5 This is a cross-sectional view of the resin cured product obtained in S4 of Example 4 of the present invention;

[0029] Appendix Figure 6 This is the TGA curve of the resin cured product obtained in S4 of Example 4 of the present invention;

[0030] Appendix Figure 7 This is a physical image of the resin-based carbon fiber composite material in Example 7 of the present invention. Detailed Implementation

[0031] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to specific embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0032] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the specification of this invention is for the purpose of describing particular embodiments only and is not intended to limit the invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items. Furthermore, the technical solutions of the various embodiments of this invention can be combined with each other, but only on the basis of being achievable by one of ordinary skill in the art. When a combination of technical solutions is contradictory or impossible to implement, such a combination should be considered non-existent and not within the scope of protection claimed by this invention.

[0033] This invention provides a phthalonitrile resin, the raw material formulation of which includes, by mass percentage: 10-20 parts of 4-(4-aminophenoxy)phthalonitrile, and 80-90 parts of a total of 1,2-bis(3,4-diacryloxyphenoxy)benzene and 1,2-bis(2,3-diacryloxyphenoxy)benzene, suitable for liquid phase molding process;

[0034] 4-(4-aminophenoxy)phthalonitrile is a self-catalytic phthalonitrile resin monomer. One of its functions is as a curing agent in the curing reaction of the resin in this formulation. If the amount used is too small, the flexural strength of the resin will be too low. If the amount used is too large, the morphology of the cured product will be unqualified and the mechanical properties cannot be tested normally. Specifically, when the amount of 4-(4-aminophenoxy)phthalonitrile is 10 parts, the properties of the resin and the cured product can still achieve the properties in the preferred embodiment of the present invention, but the error of the mechanical property data increases. If it is further lower than 10 parts, the mechanical properties are significantly worse. When the amount of 4-(4-aminophenoxy)phthalonitrile is 20 parts, the performance data are still basically stable. If it is further higher than 20 parts, the probability of the cured resin bulging and bubbling increases, the morphology becomes unstable, and the heat resistance decreases.

[0035] The ratio of 1,2-bis(3,4-dianitrilephenoxy)benzene to 1,2-bis(2,3-dianitrilephenoxy)benzene affects the temperature at which the lowest viscosity is achieved and the heat resistance of the cured product, but has little effect on other properties such as mechanical properties and dielectric properties. Specifically, there is a partial inverse relationship between the temperature at which the lowest viscosity is achieved and the heat resistance of the cured product in this resin system. The ratio of 1,2-bis(3,4-dianitrilephenoxy)benzene to 1,2-bis(2,3-dianitrilephenoxy)benzene can be adjusted according to the performance requirements of the product to meet the viscosity and heat resistance requirements of different applications. It should be noted that, within the weight percentage range of the raw material ratio in the embodiments of the present invention, the melting point of this resin system is below 80°C. Compared with the prior art, it has a lower viscosity at a lower temperature and good heat resistance, mechanical properties, and dielectric properties, which meets the requirements of liquid phase molding process.

[0036] This invention optimizes the raw material formulation of phthalonitrile resin and improves the preparation method. By combining the properties and performance advantages of phthalonitrile monomers and based on the principle of eutectic melting of mixtures, the proportions of each monomer are rationally adjusted to formulate a nitrile-based resin system suitable for liquid-phase molding processes of composite materials. This resin possesses a low melting temperature and extremely low viscosity in the molten state, making it suitable for preparing carbon fiber reinforced composite materials through liquid-phase molding. The resin system has a melting range initiation temperature below 80°C, a minimum melting endothermic peak temperature of approximately 106°C, and a maximum not exceeding 143.5°C. In the molten state, the viscosity is as low as 1000 mPa·s at 141°C. The viscosity is as low as 100 mPa·s at 151℃, and the lowest viscosity is about 40 mPa·s, which meets the performance requirements of the equipment involved in the existing liquid phase molding process. The material loss during the curing process is 0.65%, and the material loss is 0.24% at the highest curing temperature of 300℃. The shrinkage rate of the cured product relative to the mold cavity is about 1%. The morphology of the cured product is stable, and there are no obvious cracks, pores or holes on the cross-section and surface. The curing exothermic temperature range is 220~260℃. When the highest curing temperature is 280℃, the flexural strength of the cured product can reach 135.21 MPa, the flexural elastic modulus reaches 4.86 GPa, and the 5% decomposition temperature is greater than 430℃.

[0037] In a preferred embodiment, the formulation, calculated by mass percentage, contains 20 parts of 4-(4-aminophenoxy)phthalonitrile. Preferably, in the specific ratio of 1,2-bis(3,4-dianitrilephenoxy)benzene and 1,2-bis(2,3-dianitrilephenoxy)benzene, 1,2-bis(3,4-dianitrilephenoxy)benzene is 30-50 parts, and the remainder is 1,2-bis(2,3-dianitrilephenoxy)benzene. The performance parameters of the resulting resin are basically consistent with the performance data of the formulation resin in the embodiments of the present invention.

[0038] It should be noted that if the amount of 1,2-bis(3,4-dianitrilephenoxy)benzene is further reduced to less than 30 parts, the resin melting peak temperature will decrease to some extent, and the heat resistance will also decrease to some extent. If the amount of 1,2-bis(3,4-dianitrilephenoxy)benzene is reduced to zero, the resin melting curve is close to the ratio in the preferred embodiment of the present invention, and the heat resistance decreases to some extent, but both can meet the melting and viscosity performance indicators that must be met for liquid phase molding. If the amount of 1,2-bis(3,4-dianitrilephenoxy)benzene is further increased to more than 50 parts, the resin melting peak temperature will increase, and the resin heat resistance will be improved. If the amount of 1,2-bis(3,4-dianitrilephenoxy)benzene is further increased to 80 parts, the melting peak temperature will be increased to about 180°C, and other performance data are still close to the resin formulation in the preferred embodiment of the present invention.

[0039] In a preferred embodiment, 4-(4-aminophenoxy)phthalonitrile is a self-catalytic phthalonitrile resin monomer. One of the functions of this monomer is as a curing agent in the curing reaction of the resin formulation. 1,2-bis(3,4-diacrylphenoxy)benzene and 1,2-bis(2,3-diacrylphenoxy)benzene are diphenol disubstituted phthalonitrile compounds, respectively. These three phthalonitrile monomers undergo polymerization reaction, and after curing and crosslinking, areoindole, triazine ring and phthalocyanine ring are generated.

[0040] This invention also provides a method for preparing phthalonitrile resin, comprising the following steps:

[0041] S1. Weigh the raw materials according to the formula, mix them, and grind them into powder to obtain the raw material powder;

[0042] The formula, by mass percentage, includes: 10-20 parts of 4-(4-aminophenoxy)phthalonitrile, and 80-90 parts of a total of 1,2-bis(3,4-diacrylphenoxy)benzene and 1,2-bis(2,3-diacrylphenoxy)benzene;

[0043] Preferably, the method of mixing and grinding can be selected from grinding and mixing in a mortar, ball milling in a ball mill, or crushing and grinding in a crusher and pulverizer;

[0044] S2. Melt and blend the raw material powder, cool it, and then grind it into powder again. Pass the powder through a 100-mesh sieve to obtain the blended resin powder.

[0045] Preferably, the raw material powder is melted at 150-160°C, kept at that temperature for 10-30 minutes, and then naturally cooled before being pulverized by a crusher to achieve further uniform mixing.

[0046] S2. Melt and degas the blended resin powder to obtain a fluidized resin;

[0047] Preferably, the blended resin powder is melted at 150-160°C, then vacuumed to -0.1MPa and held at that temperature for 30-60 minutes to remove bubbles.

[0048] S3. The fluidized resin is cured and molded to obtain a cured resin product;

[0049] Preferably, the curing process specifically involves heating at 220°C for 2 hours, then at 240°C for 2 hours, and finally at 260°C for 2 hours to obtain a partially cured product, followed by curing at 280°C for 2 hours to obtain a resin cured product.

[0050] It should be noted that heating programs can be added as needed.

[0051] The resin system prepared by the method of preparing phthalonitrile resin in the embodiments of the present invention has both applicability to liquid phase molding process and temperature resistance.

[0052] In a preferred embodiment, prior to step S1, the preparation method of the phthalonitrile monomer used as raw material includes: feeding the reaction mixture on a kilogram-scale scale to obtain a reaction mixture; pouring the reaction mixture into water to precipitate a solid; filtering the solid-liquid mixture, washing the filter cake with water to obtain a crude product; slurrying the crude product with 95% ethanol or methanol, filtering, and then drying to obtain the monomer product.

[0053] In a preferred embodiment, prior to step S1, a method for preparing 4-(4-aminophenoxy)phthalonitrile is further included. Specifically, under nitrogen protection, p-aminophenol, anhydrous potassium carbonate, and 4-nitrophthalonitrile are added to a 20-liter double-walled glass reactor in a molar ratio of 1.2:(1.4-1.6):1.0. The mass or volume of the solvent DMF is 5-6 times that of 4-nitrophthalonitrile. The reaction is carried out at 60-80°C for 6-8 hours. The resulting reaction mixture is poured into water, and a solid precipitates. The solid is filtered, washed with water, and crude 4-(4-aminophenoxy)phthalonitrile is obtained. The crude product is slurried with 95% ethanol for 1-2 hours, filtered, and a solid is obtained. The solid is spread out in a forced-air drying oven and dried at 50-60°C for 2 hours followed by 105°C for 10 hours until constant weight is achieved, yielding a muddy yellow powder product.

[0054] In a preferred embodiment, prior to step S1, a method for preparing 1,2-bis(3,4-diacetonitrilephenoxy)benzene is further included. Specifically, under nitrogen protection, catechol, anhydrous potassium carbonate, and 4-nitrophthalonitrile are added to a 20-liter double-walled glass reactor in a molar ratio of 0.5:(1.2-1.4):1.0. The mass or volume of the solvent DMF is 4-6 times that of 4-nitrophthalonitrile. The mixture is stirred at 40-80°C for 6-24 hours. The resulting reaction mixture is poured into water, and a solid precipitates. The solid is filtered, washed with water, and crude 1,2-bis(3,4-diacetonitrilephenoxy)benzene is obtained. The crude product is slurried with 95% ethanol for 1-2 hours, filtered, and a solid is obtained. The solid is spread out in a forced-air drying oven and dried at 50-60°C for 2 hours followed by 120°C for 10 hours until constant weight is achieved, yielding a white or light pink powder product.

[0055] In a preferred embodiment, prior to step S1, a method for preparing 1,2-bis(2,3-diacetonitrilephenoxy)benzene is further included. Specifically, under nitrogen protection, catechol, anhydrous potassium carbonate, and 3-nitrophthalonitrile are added to a 20-liter double-walled glass reactor in a molar ratio of 0.5:(1.2-1.4):1.0. The mass or volume of the solvent DMF is 4-6 times that of the 3-nitrophthalonitrile. The mixture is stirred at 40-60°C for 12-24 hours. The resulting reaction mixture is poured into water, and a solid precipitates. The solid is filtered, washed with water, and crude 1,2-bis(2,3-diacetonitrilephenoxy)benzene is obtained. The crude product is then hot-beaten with methanol for 1-2 hours, filtered, and a solid is obtained. The solid is spread out in a forced-air drying oven and dried at 50-60°C for 2 hours followed by 105°C for 10 hours until constant weight is achieved, yielding a light yellow powder or small granular product.

[0056] In existing technologies, the preparation of these three monomers is mostly carried out on a small-scale laboratory basis, with raw materials input in the gram range. This results in low preparation efficiency, and the complex and delicate preparation process is not suitable for industrial production. The embodiments of this invention optimize the feeding ratio, allowing for preparation in the kilogram range. The crude monomer obtained after the reaction is purified by pulping with methanol or ethanol, enabling large-scale production. Overall, the preparation process of phthalonitrile monomer is simplified, allowing for the preparation of more monomer products in the same amount of time. The process is simpler, with lower production costs and higher economic benefits, making it more suitable for industrial production needs.

[0057] It should be noted that the phthalonitrile monomer used in the phthalonitrile resin in the embodiments of the present invention can also be prepared according to the methods reported in existing patents or papers.

[0058] This invention provides a phthalonitrile resin composite material, which is prepared by liquid-phase molding of carbon fiber woven fabric; as shown in the attached figure. Figure 6As shown, visually, the phthalonitrile resin composite material provided in this embodiment of the invention was successfully prepared, and the finished product has a good appearance, stable surface morphology, and no obvious cracks, pores, holes or bulges. In the actual test, the cross-sectional and cut surface morphology of the finished product remained stable, and the size and weight of the composite material met the design requirements. The resin system provided in this embodiment of the invention is suitable for liquid phase molding process and can be used to prepare resin carbon fiber composite materials.

[0059] In a preferred embodiment, the phthalonitrile resin is vacuum degassed in a molten state and then injected into a preheated mold cavity lined with carbon fiber woven fabric. After being fully impregnated, it is heated and cured. The resin melting temperature, vacuum degassed temperature, injection temperature, and mold preheating temperature are all 150-160°C.

[0060] In a preferred embodiment, the carbon fiber woven fabric impregnated with phthalonitrile resin is cured under a pressure of 0.2 to 1.5 MPa, and the heating program is: 220℃ for 2 hours + 240℃ for 2 hours + 260℃ for 2 hours, followed by natural cooling and demolding. The initially cured material is then cured at 280℃ for 2 hours and then naturally cooled to obtain the carbon fiber reinforced composite material of the resin system.

[0061] The embodiments of the present invention also provide the application of the above-mentioned phthalonitrile resin, the above-mentioned preparation method, or the above-mentioned phthalonitrile resin composite material in weaponry or aerospace fields.

[0062] Example 1

[0063] This embodiment provides a method for preparing 4-(4-aminophenoxy)phthalonitrile, comprising the following steps:

[0064] Under N2 gas protection, 6 L of DMF, 0.906 kg of p-aminophenol, 1.436 kg of potassium carbonate, and 1.2 kg of 4-nitrophthalonitrile were added to a 10 L double-walled glass reactor and reacted for 6–8 h at a reaction temperature of 60–80 °C to obtain a reaction mixture. The reaction mixture was poured into water, and a solid precipitated. The solid was filtered and washed with water to obtain a crude product with a 4-(4-aminophenoxy)phthalonitrile content greater than 92%. The crude product was slurried with 95% ethanol for 1–2 h and filtered to obtain a solid. The solid was spread out in a forced-air drying oven and dried at 50–60 °C for 2 h followed by 105 °C for 10 h until constant weight was obtained to obtain a muddy yellow powder product with a 4-(4-aminophenoxy)phthalonitrile content greater than 98.9%, with a yield greater than 1527.57 g and a yield of 93.7%.

[0065] Example 2

[0066] This embodiment provides a method for preparing 1,2-bis(3,4-dicyandioxyphenoxy)benzene, comprising the following steps:

[0067] Under N2 gas protection, 8 L of DMF, 0.636 kg of catechol, 2.235 kg of anhydrous potassium carbonate, and 2.0 kg of 4-nitrophthalonitrile were added to a 20 L double-walled glass reactor and stirred for 6–24 h at a reaction temperature of 40–80 °C to obtain a reaction mixture. The reaction mixture was poured into water, and a solid precipitated. The solid was filtered and washed with water to obtain a crude product with a 1,2-bis(3,4-diacetonylphenoxy)benzene content greater than 90%. The crude product was slurried with 95% ethanol for 1–2 h and filtered to obtain a solid. The solid was spread out in a forced-air drying oven and dried at 50–60 °C for 2 h followed by 120 °C for 10 h until constant weight was obtained, yielding a white or light pink powder product with a 1,2-bis(3,4-diacetonylphenoxy)benzene content of 96%–99.6%, with a yield greater than 1756.5 g and a recovery rate of 83.93%.

[0068] Example 3

[0069] This embodiment provides a method for preparing 1,2-bis(2,3-dinitrilephenoxy)benzene, comprising the following steps:

[0070] Under N2 gas protection, 8 L of DMF, 0.636 kg of catechol, 2.235 kg of anhydrous potassium carbonate, and 2.0 kg of 3-nitrophthalonitrile were added to a 20 L double-walled glass reactor and stirred for 12–24 h at a reaction temperature of 40–60 °C to obtain a reaction mixture. The reaction mixture was poured into water, and a solid precipitated. The solid was filtered and washed with water to obtain a crude product with a 1,2-bis(2,3-diacetonylphenoxy)benzene content greater than 90%. The crude product was hot-beaten with methanol for 1–2 h, filtered, and a solid was obtained. The solid was spread out in a forced-air drying oven and dried at 50–60 °C for 2 h followed by 105 °C for 10 h until constant weight was achieved, yielding a light yellow powder or small granules product with a 1,2-bis(2,3-diacetonylphenoxy)benzene content of 96.7%–98.6%, with a yield of up to 1631.6 g and a recovery rate of 78.0%.

[0071] Example 4

[0072] This embodiment provides a phthalonitrile resin suitable for liquid phase molding processes, prepared from three phthalonitrile monomers as raw materials. By mass percentage, it includes 20 parts of 4-(4-aminophenoxy)phthalonitrile, 40 parts of 1,2-bis(3,4-diacetonylphenoxy)benzene, and 40 parts of 1,2-bis(2,3-diacetonylphenoxy)benzene. The process includes the following steps:

[0073] S1. Weigh 4-(4-aminophenoxy)phthalonitrile, 1,2-bis(3,4-diacryloxyphenoxy)benzene and 1,2-bis(2,3-diacryloxyphenoxy)benzene respectively, mix them together, and then grind them by hand, ball milling or crushing to make raw material powder.

[0074] S2. Heat the raw material powder to 160℃ until it is completely melted, keep it at this temperature for 10-30 minutes to achieve further uniform mixing, and let it cool naturally to obtain a block solid. Break the block solid and transfer it to a crusher for grinding. Pass the powder through a 100-mesh sieve to obtain the blended resin for later use.

[0075] S3. The above-mentioned blended resin is placed in a vacuum oven at 160°C with a vacuum degree of about -0.1MPa for 30 to 60 minutes to remove bubbles and obtain a fluidized resin.

[0076] S4. Pour the extremely low viscosity fluid resin into the preheated mold cavity, transfer it to a forced-air oven for heating and curing. The curing heating program is: 220℃ for 2h + 240℃ for 2h + 260℃ for 2h, then allow it to cool naturally and demold. Transfer the cured material to a curing oven, heat it to 280℃ for 2h, and then allow it to cool naturally to obtain the finished resin cured product.

[0077] The raw material powder obtained in S1 was tested using DSC to determine its melting and solidification processes. The results are shown in the attached figure. Figure 1 As shown in the figure. The melting and curing process of the blended resin obtained by S2 was tested using DSC, and the results are shown in the attached figure. Figure 2 As shown, its rheological viscosity-temperature curve is attached. Figure 3 As shown. Combining visual observation, DSC curves, and rheological viscosity-temperature curves, the melting point of this resin system is below 80℃; the DSC curves show that its melting endothermic peak temperature is as low as approximately 106℃ and as high as no more than 143.5℃; its rheological viscosity-temperature curves show that in the molten state, the viscosity is as low as 1000 mPa·s at 141℃ and as low as 100 mPa·s at 151℃, with a minimum viscosity of approximately 40 mPa·s, meeting the equipment performance requirements involved in existing liquid phase molding processes.

[0078] As attached Figure 4 The image shown is a photograph of the cured resin in S4. The surface morphology is stable, with no obvious bulging, bubbling, or voids. Based on the mold cavity dimensions, the cured product shows a dimensional shrinkage of approximately 1%. (See attached image.) Figure 5 As shown, the cured material that broke during the bending strength test also showed no obvious pores or other phenomena on the cross-section. By weighing, the weight loss of the material during the curing process was approximately 0.65%.

[0079] The cured material was tested for flexural strength and flexural modulus according to GB / T2567-2021. The flexural strength of the cured material reached 135.21 MPa, and the flexural modulus reached 4.86 GPa. The TGA curve of the cured material is attached. Figure 6 As shown, its 5% decomposition temperature exceeds 430°C; the solidified material was further baked at 300°C for 2 hours, and the weight loss was no more than 0.24%.

[0080] Example 5

[0081] This embodiment provides a phthalonitrile resin suitable for liquid phase molding processes, prepared from three phthalonitrile monomers as raw materials. By mass percentage, it comprises 20 parts of 4-(4-aminophenoxy)phthalonitrile, 30 parts of 1,2-bis(3,4-diacetonylphenoxy)benzene, and 50 parts of 1,2-bis(2,3-diacetonylphenoxy)benzene, and includes the following steps:

[0082] S1. Weigh 4-(4-aminophenoxy)phthalonitrile, 1,2-bis(3,4-diacryloxyphenoxy)benzene and 1,2-bis(2,3-diacryloxyphenoxy)benzene respectively, mix them together, and then grind them by hand, ball milling or crushing to make raw material powder.

[0083] S2. Heat the raw material powder to 160℃ until it is completely melted, keep it at this temperature for 10-30 minutes to achieve further uniform mixing, and let it cool naturally to obtain a block solid. Break the block solid and transfer it to a crusher for grinding. Pass the powder through a 100-mesh sieve to obtain the blended resin for later use.

[0084] S3. The above-mentioned blended resin is placed in a vacuum oven at 160°C with a vacuum degree of about -0.1MPa for 30 to 60 minutes to remove bubbles and obtain a fluidized resin.

[0085] S4. Pour the extremely low viscosity fluid resin into the preheated mold cavity, transfer it to a forced-air oven for heating and curing. The curing heating program is: 220℃ for 2h + 240℃ for 2h + 260℃ for 2h, then allow it to cool naturally and demold. Transfer the cured material to a curing oven, heat it to 280℃ for 2h, and then allow it to cool naturally to obtain the finished resin cured product.

[0086] The resin obtained in this embodiment has a slightly lower peak melting temperature but is close to that in Example 4. The curing curve, morphology of the cured product, and performance data are highly consistent with those in Example 4.

[0087] Example 6

[0088] This embodiment provides a phthalonitrile resin suitable for liquid phase molding processes, prepared from three phthalonitrile monomers as raw materials. By mass percentage, it comprises 20 parts of 4-(4-aminophenoxy)phthalonitrile, 50 parts of 1,2-bis(3,4-diacetonylphenoxy)benzene, and 30 parts of 1,2-bis(2,3-diacetonylphenoxy)benzene, and includes the following steps:

[0089] S1. Weigh 4-(4-aminophenoxy)phthalonitrile, 1,2-bis(3,4-diacryloxyphenoxy)benzene and 1,2-bis(2,3-diacryloxyphenoxy)benzene respectively, mix them together, and then grind them by hand, ball milling or crushing to make raw material powder.

[0090] S2. Heat the raw material powder to 160℃ until it is completely melted, keep it at this temperature for 10-30 minutes to achieve further uniform mixing, and let it cool naturally to obtain a block solid. Break the block solid and transfer it to a crusher for grinding. Pass the powder through a 100-mesh sieve to obtain the blended resin for later use.

[0091] S3. The above-mentioned blended resin is placed in a vacuum oven at 160°C with a vacuum degree of about -0.1MPa for 30 to 60 minutes to remove bubbles and obtain a fluidized resin.

[0092] S4. Pour the extremely low viscosity fluid resin into the preheated mold cavity, transfer it to a forced-air oven for heating and curing. The curing heating program is: 220℃ for 2h + 240℃ for 2h + 260℃ for 2h, then allow it to cool naturally and demold. Transfer the cured material to a curing oven, heat it to 280℃ for 2h, and then allow it to cool naturally to obtain the finished resin cured product.

[0093] The resin obtained in this embodiment has a slightly higher peak melting temperature but is close to that in Example 4. The curing curve, morphology of the cured product, and performance data are highly consistent with those in Example 4.

[0094] Example 7

[0095] This embodiment provides a method for preparing phthalonitrile resin composite materials using a liquid phase molding process, including the following steps:

[0096] Step 1: Cut the carbon fiber woven fabric to a certain size and carefully lay it into the mold cavity;

[0097] Step 2: Place the mold after layering in a forced-air drying oven and preheat it to 150-160℃;

[0098] Step 3: Heat the raw material powder obtained in S1 of Example 4 to 150-160°C, evacuate to a vacuum degree of about -0.1 MPa, and maintain for 30-60 minutes;

[0099] Step 4: Inject the resin into the sealed mold cavity and allow it to fully impregnate the mold.

[0100] Step 5: Curing the resin-impregnated carbon fiber woven fabric, the heating program is: 220℃ 2h + 240℃ 2h + 260℃ 2h, then naturally cooling down and demolding;

[0101] Step 6: Heat the cured material to 280℃, keep it at that temperature for 2 hours, and then let it cool naturally to obtain a resin-based carbon fiber reinforced composite material.

[0102] As attached Figure 7 As shown, the composite material provided in this embodiment has a stable morphology and no obvious cracks, pores or holes on the surface.

[0103] Comparative Example 1

[0104] This comparative example provides a phthalonitrile resin, the raw materials of which, by mass percentage, include 5 parts of 4-(4-aminophenoxy)phthalonitrile, and a total of 95 parts of 1,2-bis(3,4-diacetonylphenoxy)benzene and 1,2-bis(2,3-diacetonylphenoxy)benzene, and include the following steps:

[0105] S1. Weigh out 4-(4-aminophenoxy)phthalonitrile, 1,2-bis(3,4-diacryloxyphenoxy)benzene and 1,2-bis(2,3-diacryloxyphenoxy)benzene respectively, mix them together, and grind them into powder by hand, ball milling or crushing.

[0106] S2. Heat the powder to 160℃ until it is completely melted, keep it at that temperature for 10-30 minutes to achieve further uniform mixing, and let it cool naturally to obtain a block solid. Break the block solid and transfer it to a crusher to grind it into powder. Pass the powder through a 100-mesh sieve to obtain the blended resin for later use.

[0107] S3. The above resin powder is placed in a vacuum oven at 160℃ with a vacuum degree of about -0.1MPa for 30 to 60 minutes to remove bubbles;

[0108] S4. Pour the extremely low viscosity liquid resin into the preheated mold cavity, transfer it to a forced-air oven for heating and curing. The curing heating program is: 220℃ for 2h + 240℃ for 2h + 260℃ for 2h, then allow it to cool naturally and demold. Transfer the cured material to a curing oven and allow it to cool naturally after 280℃ for 2h.

[0109] Through weighing and measurement, the material weight loss during the curing process was approximately 0.84%, the shrinkage rate of the cured product relative to the mold cavity length was approximately 1%, the morphology of the cured product was stable, and there were no obvious cracks, pores, or holes on the cross-section and surface. The cured product was tested for flexural strength according to GB / T2567-2021, and its highest flexural strength value was 73.09 MPa.

[0110] Comparative Example 2

[0111] This comparative example provides a phthalonitrile resin suitable for liquid phase molding processes. Its raw materials, by mass percentage, include 25 parts of 4-(4-aminophenoxy)phthalonitrile, and a total of 75 parts of 1,2-bis(3,4-diacetonylphenoxy)benzene and 1,2-bis(2,3-diacetonylphenoxy)benzene. The process includes the following steps:

[0112] S1. Weigh 4-(4-aminophenoxy)phthalonitrile, 1,2-bis(3,4-diacryloxyphenoxy)benzene and 1,2-bis(2,3-diacryloxyphenoxy)benzene respectively, mix them together, and then grind them by hand, ball milling or crushing to make raw material powder.

[0113] S2. Heat the raw material powder to 160℃ until it is completely melted, keep it at this temperature for 10-30 minutes to achieve further uniform mixing, and let it cool naturally to obtain a block solid. Break the block solid and transfer it to a crusher for grinding. Pass the powder through a 100-mesh sieve to obtain the blended resin for later use.

[0114] S3. The above-mentioned blended resin is placed in a vacuum oven at 160°C with a vacuum degree of about -0.1MPa for 30 to 60 minutes to remove bubbles and obtain a fluidized resin.

[0115] S4. Pour the extremely low viscosity fluid resin into the preheated mold cavity, transfer it to a forced-air oven for heating and curing. The curing heating program is: 220℃ for 2h + 240℃ for 2h + 260℃ for 2h, then allow it to cool naturally and demold. Transfer the cured material to a curing oven, heat it to 280℃ for 2h, and then allow it to cool naturally to obtain the finished resin cured product.

[0116] The resin in this comparative example had a melting point below 80°C. Measurements showed that the cured material in this comparative example had a shrinkage rate of approximately 1% relative to the mold cavity length. The morphology of the cured material may be unstable, with sesame-seed-sized air bubbles potentially appearing on the lower and side surfaces of the mold. The cured material underwent flexural strength testing according to GB / T2567-2021. The highest flexural strength value of the intact casting was approximately 100 MPa. Most castings, due to internal porosity and defects, may have flexural strengths as low as 20 MPa or even below 10 MPa.

[0117] The technical features of the above embodiments can be combined in any way. For the sake of brevity, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0118] The embodiments described above are merely illustrative of several implementations of the present invention, and while the descriptions are relatively specific and detailed, they should not be construed as limiting the scope of the invention patent. It should be noted that those skilled in the art can make various modifications and improvements without departing from the concept of the present invention, and these all fall within the protection scope of the present invention. Therefore, the protection scope of this invention patent should be determined by the appended claims.

[0119] The contents not described in detail in this specification are existing technologies known to those skilled in the art.

Claims

1. A phthalonitrile resin, characterized in that, The formulation of the phthalonitrile resin, by weight, consists of 20 parts of 4-(4-aminophenoxy)phthalonitrile, 80-90 parts of 1,2-bis(3,4-dianitrilephenoxy)benzene and 1,2-bis(2,3-dianitrilephenoxy)benzene, of which 30-50 parts are 1,2-bis(2,3-dianitrilephenoxy)benzene; The preparation method of the phthalonitrile resin includes the following steps: S1. Weigh the raw materials according to the formula, mix them and grind them into powder to obtain raw material powder; S2. The raw material powder is melted and blended, cooled, and then pulverized again to obtain blended resin powder; S3. The blended resin powder is melted and degassed to obtain a fluidized resin; S4. The fluidized resin is cured and molded to obtain a cured resin product.

2. The phthalonitrile resin as described in claim 1, characterized in that, This includes the formation of isoindole, triazine rings, and phthalocyanine rings through curing and cross-linking.

3. A method for preparing phthalonitrile resin as described in any one of claims 1 or 2, characterized in that, Includes the following steps: S1. Weigh the raw materials according to the formula, mix them and grind them into powder to obtain raw material powder; S2. The raw material powder is melted and blended, cooled, and then pulverized again to obtain blended resin powder; S3. The blended resin powder is melted and degassed to obtain a fluidized resin; S4. The fluidized resin is cured and molded to obtain a cured resin product.

4. The preparation method according to claim 3, characterized in that, Step S2 specifically includes melting the raw material powder at 150~160℃ and holding it at that temperature for 10~30 minutes. Step S3 specifically includes melting the blended resin powder at 150~160℃, evacuating it to -0.1MPa, and holding it at that temperature for 30~60 minutes to degas it.

5. The preparation method according to claim 3, characterized in that, The curing process in step S4 includes a heating process of 220℃ for 2 hours, 240℃ for 2 hours, and 260℃ for 2 hours to obtain a preliminary cured product, followed by a process of 280℃ for 2 hours to obtain a resin cured product.

6. The preparation method according to claim 3, characterized in that, Before step S1, a method for preparing 4-(4-aminophenoxy)phthalonitrile is also included, comprising: under nitrogen protection, mixing p-aminophenol, anhydrous potassium carbonate and 4-nitrophthalonitrile in a molar ratio of 1.2:(1.4~1.6):1.0 with a solvent, wherein the mass or volume of the solvent is 5~6 times that of 4-nitrophthalonitrile, reacting at 60~80℃ for 6~8h, pouring the resulting reaction mixture into water, precipitating a solid, filtering, washing, and then slurrying with 95% ethanol for 1~2h, filtering, and then drying at 50~60℃ for 2h + 105℃ for 10h to constant weight to obtain 4-(4-aminophenoxy)phthalonitrile monomer.

7. The preparation method according to claim 3, characterized in that, Before step S1, a method for preparing 1,2-bis(3,4-diacetonitrilephenoxy)benzene is included, comprising: under nitrogen protection, mixing catechol, anhydrous potassium carbonate and 4-nitrophthalonitrile in a molar ratio of 0.5:(1.2~1.4):1 with a solvent, wherein the mass or volume of the solvent is 4~6 times that of 4-nitrophthalonitrile, stirring at 40~80℃ for 6~24h, pouring the resulting reaction mixture into water, precipitating a solid, filtering, washing, and then slurrying with 95% ethanol for 1~2h, filtering, and then drying at 50~60℃ for 2h + 120℃ for 10h to constant weight to obtain 1,2-bis(3,4-diacetonitrilephenoxy)benzene monomer.

8. The preparation method according to claim 3, characterized in that, Before step S1, a method for preparing 1,2-bis(2,3-diacetonitrilephenoxy)benzene is included, comprising: under nitrogen protection, mixing catechol, anhydrous potassium carbonate and 3-nitrophthalonitrile in a molar ratio of 0.5:(1.2~1.4):1 with a solvent, wherein the mass or volume of the solvent is 4~6 times that of 3-nitrophthalonitrile, stirring at 40~60℃ for 12~24h, pouring the resulting reaction mixture into water, precipitating a solid, filtering, washing, and then hot-beating with methanol for 1~2h, filtering, and then drying at 50~60℃ for 2h + 105℃ for 10h to constant weight to obtain 1,2-bis(2,3-diacetonitrilephenoxy)benzene monomer.

9. The application of the phthalonitrile resin as described in any one of claims 1 or 2, or the phthalonitrile resin obtained by the preparation method as described in any one of claims 3 to 8, for use in liquid phase molding processes to prepare resin-based carbon fiber reinforced composite materials.

Citation Information

Patent Citations

  • Phthalonitrile resin composition and preparation method thereof

    CN109096488A

  • Carbon-based composites derived from phthalonitrile resins

    US5965268A