Vertically stacked high-voltage Micro LED chips and their fabrication method
By using a high-voltage Micro LED chip structure stacked vertically, the problem of Micro LED chips operating at high voltage in existing technologies has been solved, improving photoelectric performance and stability.
Patent Information
- Application Number
- CN202311242520.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-09-25
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-09-25
AI Technical Summary
Existing Micro LED chips are difficult to operate at high voltages, and their photoelectric performance and stability are limited due to size and spacing constraints.
A high-voltage Micro LED chip structure with vertical stacking is adopted. A stepped mesa structure is formed by etching, and a passivation layer and metal electrodes are deposited on the chip surface to achieve electrical connection between the two chips.
This enables Micro LED chips to operate normally under high voltage, improving photoelectric performance and stability, and reducing the adverse effects caused by size reduction.
Smart Images

Figure CN117542845B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of Micro LED technology, specifically to a high-voltage Micro LED chip stacked vertically and its fabrication method. Background Technology
[0002] Micro LEDs have outstanding advantages such as high resolution, high brightness, long lifespan, and wide color gamut. Compared with traditional LCDs and OLEDs, they have greater advantages in terms of brightness, resolution, contrast, energy consumption, lifespan, response speed, and thermal stability, and are gradually being used in augmented reality (AR), virtual reality (VR), and micro-displays.
[0003] In the prior art, a vertically arranged full-color display Micro LED chip and its manufacturing method (CN116564947 A) is constructed by vertically stacking and assembling three epitaxial structures of red, green and blue light. A filter layer is set between the red light epitaxial layer and the green light epitaxial layer. The filter layer can reflect blue and green light, while red light can be transmitted through it, so that the three epitaxial structures can emit light independently, forming a vertically arranged full-color display Micro-LED.
[0004] In the prior art, a red micro LED chip and its fabrication method are disclosed. The fabrication method includes: growing an AlGaInP LED epitaxial layer structure on a first GaAs substrate inverted; bonding the epitaxial wafer with the AlGaInP LED epitaxial structure to a second GaAs substrate; depositing a protective layer on the surface of the second GaAs substrate, and then using a chemical solution to etch and remove the first GaAs substrate used for epitaxial growth; performing LED chip front-end processes; covering the entire wafer surface with temporary bonding adhesive to obtain a flat wafer surface; using a temporary bonding process to bond the wafer surface and a temporary substrate together; removing the protective layer on the surface of the second GaAs substrate using an etchant, and then using a chemical solution to etch and remove the second GaAs substrate and the bonding layer; and peeling off the micro LED chip to complete the fabrication.
[0005] In the prior art, a Micro-LED chip structure includes a plurality of arrayed Micro-LED chips. Each Micro-LED chip includes a substrate, a Micro-LED body, and an active addressing driving circuit. The Micro-LED body comprises, from bottom to top, a Si-doped n-type GaN layer, a multiple quantum well layer, and a Mg-doped p-type GaN layer deposited on the substrate. The Micro-LED body has a stepped structure with a stepped surface, the stepped surface being the upper surface of the Si-doped n-type GaN layer. The Micro-LED body also includes layers spaced apart by a first insulating layer and respectively connected to the Si-doped n-type GaN layers. The substrate includes a first metal layer and a Mg-doped p-type GaN layer; the active addressing driving circuit includes a first transistor, a second transistor, and a capacitor, all disposed on the substrate, and the Micro-LED body, the first transistor, and the second transistor are sequentially distributed on the substrate; the first transistor controls the pixel circuit of the Micro-LED body to turn on and off, the second transistor is connected to a power supply and provides a stable current to the Micro-LED body during a specific pulse period, and the capacitor used to store signals provides a stable current to the Micro-LED body after the pulse ends, so as to enable active addressing driving of the Micro-LED body.
[0006] In the prior art, a microchip structure with uniform light emission includes: an epitaxial unit comprising an N-type epitaxial layer, a light-emitting layer, and a P-type epitaxial layer; wherein the first surface of the N-type epitaxial layer has a first step, and the light-emitting layer and the P-type epitaxial layer are stacked sequentially on the first step; the second surface of the N-type epitaxial layer is serrated; a lens unit disposed on the N-type epitaxial layer and connected to the second surface of the N-type epitaxial layer, wherein the first surface of the lens unit is serrated, and the second surface of the lens unit has a hollow structure; wherein the serration of the first surface of the lens unit matches the second surface of the N-type epitaxial layer, and the lens unit is used to achieve uniform light emission; a conductive unit disposed on the P-type epitaxial layer; an electrode unit comprising a P electrode and an N electrode, wherein the N electrode is disposed on the first surface of the N-type epitaxial layer; the P electrode is disposed on the conductive unit; and a substrate bonded to the second surface of the lens unit.
[0007] Compared to large-size LED chips, Micro LED chips are limited by size and spacing, making it difficult for them to operate at high voltages. Vertically stacked Micro-LED manufacturing technology provides a feasible way to realize high-voltage Micro LEDs. Summary of the Invention
[0008] The present invention aims to at least solve one of the technical problems existing in the prior art. To this end, the present invention proposes a method for fabricating high-voltage Micro LED display chips stacked in columns.
[0009] The objective of this invention is achieved by at least one of the following technical solutions.
[0010] A vertically stacked high-voltage Micro LED chip includes, from bottom to top, a second substrate, a second LED light-emitting layer, a second transparent conductive layer, an adhesive bonding layer, a first LED light-emitting layer, and a first transparent conductive layer;
[0011] The first LED light-emitting layer and the second LED light-emitting layer both include an N-type GaN layer, multiple quantum wells and a P-type GaN layer stacked from bottom to top;
[0012] The N-type GaN layer of the first transparent conductive layer is etched from one side of the upper surface to the second LED light-emitting layer to form a mesa structure, dividing the second LED light-emitting layer into a second step portion including the N-type GaN layer and a second mesa portion including multiple quantum wells and P-type GaN layers; the side of the second LED light-emitting layer that is etched is defined as the left side;
[0013] The upper right surface of the first transparent conductive layer is etched to the second transparent conductive layer. On this basis, the upper right surface of the first transparent conductive layer is etched again to the N-type GaN layer of the first LED light-emitting layer to form a stepped mesa structure, dividing the first LED light-emitting layer into a first step portion including an N-type GaN layer and a first mesa portion including multiple quantum wells and a P-type GaN layer.
[0014] Metal electrodes are provided on the upper surface of the second transparent conductive layer exposed by etching and on the upper surface of the first step portion, i.e., the upper surface of the N-type GaN layer of the first LED light-emitting layer. In addition to the locations where metal electrodes are provided, passivation layers are deposited at all other locations. The two metal electrodes are connected on the passivation layers.
[0015] A P-electrode is disposed on the upper surface of the first transparent conductive layer, and an N-electrode is disposed on the upper surface of the N-type GaN layer of the second LED light-emitting layer. In addition to the locations where the P-electrode and N-electrode are disposed, passivation layers are deposited on the surfaces of the two metal electrode connection portions, the second transparent conductive layer, the adhesive bonding layer, the first LED light-emitting layer, and the sides of the first transparent conductive layer.
[0016] Furthermore, the width of the second step portion is greater than that of the second mesa portion, and the width of the second substrate is the same as the width of the second step portion, and the width of the second transparent conductive layer is the same as the width of the second mesa portion.
[0017] Furthermore, in the stepped platform structure, the width of the first step portion is greater than that of the first platform portion, and the width of the adhesive bonding layer is the same as that of the first step portion. The left side of the adhesive bonding layer is flush with the left side of the second transparent conductive layer, and the width of the first transparent conductive layer is the same as that of the first platform portion.
[0018] A method for fabricating vertically stacked high-voltage Micro LED chips includes the following steps:
[0019] S1. Provide a first chip and a second chip. The first chip includes a first substrate, a first LED light-emitting layer and a first transparent conductive layer. The second chip includes a second substrate, a second LED light-emitting layer and a second transparent conductive layer. Both the first LED light-emitting layer and the second LED light-emitting layer include an N-type GaN layer, multiple quantum wells and a P-type GaN layer stacked from bottom to top.
[0020] S2. The first chip is bonded to the temporary substrate through the first transparent conductive layer, and the first substrate is peeled off by laser to expose the first LED light-emitting layer.
[0021] S3. The first chip and the second chip are bonded together using an adhesive bonding layer. After bonding, the temporary substrate of the first chip is peeled off.
[0022] S4. Etch the upper right surface of the first transparent conductive layer to the second transparent conductive layer (302) of the second chip; etch the same side surface again to the N-type GaN layer of the first LED light-emitting layer to form a stepped mesa structure. The lower step surface of the stepped mesa structure is the second transparent conductive layer, and the upper step surface is the N-type GaN layer of the first LED light-emitting layer.
[0023] S5. Etch the N-type GaN layer from the upper left surface of the first transparent conductive layer to the second chip to form a mesa structure. The step surface is the N-type GaN layer of the second LED light-emitting layer.
[0024] S6. Deposit a passivation layer on the stepped mesa structure and open holes for metal electrodes, then deposit metal electrodes at the openings.
[0025] S7. Deposit a passivation layer on the entire chip surface, create openings for the N and P electrodes of the Micro LED chip, and deposit the N and P electrodes at the openings.
[0026] Furthermore, the temporary substrate for bonding the first chip is for the subsequent process of removing the first substrate. The temporary substrate is removed after the first chip and the second chip are bonded.
[0027] Furthermore, the metal electrodes deposited on the stepped mesa structure connect the N-type GaN layer of the first LED light-emitting layer to the second transparent conductive layer, thereby achieving the electrical connection between the first chip and the second chip.
[0028] Furthermore, the passivation layer deposited in step S7 will cover the metal electrodes connecting the first chip and the second chip.
[0029] Furthermore, the passivation layer is silicon dioxide.
[0030] Furthermore, the hole of the N electrode is located on the upper surface of the N-type GaN layer of the second LED light-emitting layer, and the hole of the P electrode is located on the upper surface of the first transparent conductive layer.
[0031] Furthermore, metal electrodes are deposited on the pore sites of the N and P electrodes, which are the corresponding N and P electrodes.
[0032] Compared with the prior art, the advantages of this invention are:
[0033] This invention assembles two Micro LED chip structures by stacking them vertically, enabling Micro LED chips to operate at high voltage. Furthermore, the size of the vertically stacked Micro LEDs can be larger than that of conventionally horizontally arranged Micro LEDs, effectively reducing the adverse effects of reduced LED device size and improving the photoelectric performance and stability of the LED device. Attached Figure Description
[0034] Figure 1 This is a cross-sectional view of the side (B side) of the Micro LED display chip described in this embodiment;
[0035] Figure 2 This is a cross-sectional view of the side (side A) of the Micro LED display chip described in this embodiment;
[0036] Figure 3 This is a top view of the Micro LED display chip described in this embodiment;
[0037] Figure 4 This is a schematic diagram of the structure of the first chip and the second chip in step S1 of this embodiment;
[0038] Figure 5 This is a schematic diagram of the LED chip structure described in step S2 of this embodiment;
[0039] Figure 6 This is a schematic diagram of the LED chip structure described in step S3 of this embodiment;
[0040] Figure 7 This is a cross-sectional view of the side (B side) of the LED chip described in step S4 of this embodiment;
[0041] Figure 8 This is a cross-sectional view of the side (B side) of the LED chip described in step S5 of this embodiment;
[0042] Figure 9This is a cross-sectional view of the side (B side) of the LED chip described in step S6 of this embodiment. Detailed Implementation Plan
[0043] To better understand the above-mentioned objectives, features, and advantages of this disclosure, the solutions disclosed herein will be further described below. It should be noted that, unless otherwise specified, the embodiments and features described herein can be combined with each other.
[0044] Numerous specific details are set forth in the following description in order to provide a full understanding of this disclosure, but this disclosure may also be implemented in other ways different from those described herein; obviously, the embodiments in the specification are only some, and not all, of the embodiments of this disclosure.
[0045] Example:
[0046] Vertically stacked high-voltage Micro LED chips, such as Figure 1 , Figure 2 and Figure 3 As shown, it includes a second substrate 102, a second LED light-emitting layer 202, a second transparent conductive layer 302, an adhesive bonding layer 500, a first LED light-emitting layer 201, and a first transparent conductive layer 301 stacked from bottom to top;
[0047] The first LED light-emitting layer 201 and the second LED light-emitting layer 202 both include an N-type GaN layer, multiple quantum wells and a P-type GaN layer stacked from bottom to top;
[0048] The N-type GaN layer of the second LED light-emitting layer 202 is etched from one side of the upper surface of the first transparent conductive layer 301 to form a mesa structure, dividing the second LED light-emitting layer 202 into a second step portion including an N-type GaN layer and a second mesa portion including multiple quantum wells and a P-type GaN layer; the side of the second LED light-emitting layer 202 that is etched is defined as the left side;
[0049] The upper right surface of the first transparent conductive layer 301 is etched to the second transparent conductive layer 302. On this basis, the upper right surface of the first transparent conductive layer 301 is etched again to the N-type GaN layer of the first LED light-emitting layer 201 to form a stepped mesa structure, dividing the first LED light-emitting layer 201 into a first step portion including an N-type GaN layer and a first mesa portion including multiple quantum wells and a P-type GaN layer.
[0050] Metal electrodes are provided on the upper surface of the second transparent conductive layer 302 exposed by etching and on the upper surface of the first step portion, i.e., the upper surface of the N-type GaN layer of the first LED light-emitting layer 201. In addition to the locations where metal electrodes are provided, passivation layers 600 are deposited at all other locations. The two metal electrodes are connected on the passivation layer 600.
[0051] A P electrode is disposed on the upper surface of the first transparent conductive layer 301, and an N electrode is disposed on the upper surface of the N-type GaN layer of the second LED light-emitting layer 202. In addition to the positions where the P electrode and N electrode are disposed, a passivation layer 600 is deposited on the surface of the connection portion of the two metal electrodes 700, the second transparent conductive layer 302, the adhesive bonding layer 500, the first LED light-emitting layer 201, and the side surface of the first transparent conductive layer 301.
[0052] Furthermore, the width of the second step portion is greater than that of the second mesa portion, and the width of the second substrate 102 is the same as the width of the second step portion, and the width of the second transparent conductive layer 302 is the same as the width of the second mesa portion.
[0053] Furthermore, in the stepped platform structure, the width of the first step portion is greater than that of the first platform portion, and the width of the adhesive bonding layer 500 is the same as that of the first step portion. The left side of the adhesive bonding layer 500 is flush with the left side of the second transparent conductive layer 302, and the width of the first transparent conductive layer 301 is the same as that of the first platform portion.
[0054] A method for fabricating vertically stacked high-voltage Micro LED chips includes the following steps:
[0055] S1. Provide a first chip and a second chip, such as Figure 4 As shown, the first chip includes a first substrate 101, a first LED light-emitting layer 201 and a first transparent conductive layer 301, and the second chip includes a second substrate 102, a second LED light-emitting layer 202 and a second transparent conductive layer 302. Both the first LED light-emitting layer 201 and the second LED light-emitting layer 202 include an N-type GaN layer, multiple quantum wells and a P-type GaN layer stacked from bottom to top.
[0056] S2. The first chip is bonded to the temporary substrate 400 through the first transparent conductive layer 301. The first substrate 101 is then laser-peeled off to expose the first LED light-emitting layer 201. Figure 5 As shown;
[0057] S3. The first chip and the second chip are bonded together using the adhesive bonding layer 500. After bonding, the temporary substrate 400 of the first chip is peeled off. Figure 6 As shown;
[0058] S4. Etch the upper right surface of the first transparent conductive layer 301 to the second transparent conductive layer 302 of the second chip; etch the same side surface again to the N-type GaN layer of the first LED light-emitting layer 201 to form a stepped mesa structure, such as... Figure 7 As shown, the lower step surface of the stepped platform structure is the second transparent conductive layer 302, and the upper step surface is the N-type GaN layer of the first LED light-emitting layer 201.
[0059] S5. Etch the upper left surface of the first transparent conductive layer 301 down to the N-type GaN layer of the second chip to form a mesa structure, such as... Figure 8 As shown, the stepped surface is the N-type GaN layer of the second LED light-emitting layer 202;
[0060] S6. Deposit a passivation layer 600 on the stepped mesa structure, and create apertures for the metal electrodes. Deposit a metal electrode 700 at the apertures. Figure 9 As shown;
[0061] S7. Deposit a passivation layer of 600 on the entire chip surface, and create openings for the N-electrode and P-electrode of the Micro LED chip. Deposit the N-electrode and P-electrode at the openings, such as... Figure 1 As shown.
[0062] Furthermore, the first chip bonding temporary substrate 400 is for the subsequent process of stripping the first substrate 101. The temporary substrate 400 is removed after the first chip and the second chip are bonded.
[0063] Furthermore, the metal electrode 700 deposited on the stepped mesa structure connects the N-type GaN layer of the first LED light-emitting layer 201 to the second transparent conductive layer 302, thereby realizing the electrical connection between the first chip and the second chip.
[0064] Furthermore, the passivation layer 600 deposited in step S7 will cover the metal electrodes 700 connecting the first chip and the second chip.
[0065] Furthermore, the passivation layer 600 is silicon dioxide.
[0066] Furthermore, the hole of the N electrode is located on the upper surface of the N-type GaN layer of the second LED light-emitting layer 202, and the hole of the P electrode is located on the upper surface of the first transparent conductive layer 301.
[0067] Furthermore, metal electrodes are deposited on the pore sites of the N and P electrodes, which are the corresponding N and P electrodes.
[0068] The above description is merely a specific embodiment of this disclosure, enabling those skilled in the art to understand or implement it. Various modifications to these embodiments will be readily apparent to those skilled in the art, and the general principles defined above may be implemented in other embodiments without departing from the spirit or scope of this disclosure. Therefore, this disclosure is not to be limited to the above embodiments, but is to be accorded the widest scope consistent with the disclosed principles and novel features.
Claims
1. A high voltage micro LED chip in a vertical stack, characterized in that, It includes, from bottom to top, a second substrate (102), a second LED light-emitting layer (202), a second transparent conductive layer (302), an adhesive bonding layer (500), a first LED light-emitting layer (201), and a first transparent conductive layer (301); The first LED light-emitting layer (201) and the second LED light-emitting layer (202) both include N-type GaN layers, multiple quantum wells and P-type GaN layers stacked from bottom to top; The N-type GaN layer of the second LED light-emitting layer (202) is etched from one side of the upper surface of the first transparent conductive layer (301) to form a mesa structure, dividing the second LED light-emitting layer (202) into a second step portion including the N-type GaN layer and a second mesa portion including multiple quantum wells and P-type GaN layers; the side of the second LED light-emitting layer (202) that is etched is defined as the left side; The upper right surface of the first transparent conductive layer (301) is etched to the second transparent conductive layer (302). On this basis, the upper right surface of the first transparent conductive layer (301) is etched again to the N-type GaN layer of the first LED light-emitting layer (201) to form a stepped mesa structure, dividing the first LED light-emitting layer (201) into a first step portion including an N-type GaN layer and a first mesa portion including multiple quantum wells and a P-type GaN layer. Metal electrodes are provided on the upper surface of the second transparent conductive layer (302) exposed by etching and on the upper surface of the first step portion, i.e., the upper surface of the N-type GaN layer of the first LED light-emitting layer (201). In addition to the locations where metal electrodes are provided, passivation layers (600) are deposited at all locations. The two metal electrodes are connected on the passivation layer (600). A P electrode is disposed on the upper surface of the first transparent conductive layer (301), and an N electrode is disposed on the upper surface of the N-type GaN layer of the second LED light-emitting layer (202). In addition to the positions where the P electrode and the N electrode are disposed, a passivation layer (600) is deposited on the surface of the connection part of the two metal electrodes (700), the second transparent conductive layer (302), the adhesive bonding layer (500), the first LED light-emitting layer (201), and the side surface of the first transparent conductive layer (301).
2. The high-voltage Micro LED chip stacked in columns according to claim 1, characterized in that, The width of the second step portion is greater than that of the second mesa portion, and the width of the second substrate (102) is the same as that of the second step portion, and the width of the second transparent conductive layer (302) is the same as that of the second mesa portion.
3. The high-voltage Micro LED chip stacked in columns according to claim 1, characterized in that, In the stepped platform structure, the width of the first step is greater than that of the first platform, and the width of the adhesive bonding layer (500) is the same as that of the first step. The left side of the adhesive bonding layer (500) is flush with the left side of the second transparent conductive layer (302), and the width of the first transparent conductive layer (301) is the same as that of the first platform.
4. The method for fabricating high-voltage Micro LED chips stacked vertically according to claim 1, characterized in that, Includes the following steps: S1. A first chip and a second chip are provided. The first chip includes a first substrate (101), a first LED light-emitting layer (201), and a first transparent conductive layer (301). The second chip includes a second substrate (102), a second LED light-emitting layer (202), and a second transparent conductive layer (302). Both the first LED light-emitting layer (201) and the second LED light-emitting layer (202) include N-type GaN layers, multiple quantum wells, and P-type GaN layers stacked from bottom to top. S2. The first chip is bonded to the temporary substrate (400) through the first transparent conductive layer (301), and the first substrate (101) is peeled off by laser to expose the first LED light-emitting layer (201); S3. The first chip and the second chip are bonded together by the adhesive bonding layer (500), and the temporary substrate (400) of the first chip is peeled off after bonding. S4. Etch the upper right surface of the first transparent conductive layer (301) to the second transparent conductive layer (302) of the second chip; etch the same side surface again to the N-type GaN layer of the first LED light-emitting layer (201) to form a stepped mesa structure. The lower step surface of the stepped mesa structure is the second transparent conductive layer (302), and the upper step surface is the N-type GaN layer of the first LED light-emitting layer (201). S5. Etch the upper left surface of the first transparent conductive layer (301) to the N-type GaN layer of the second chip to form a mesa structure, with the step surface being the N-type GaN layer of the second LED light-emitting layer (202); S6. Deposit a passivation layer (600) on the stepped mesa structure and open holes for metal electrodes, and deposit metal electrodes (700) at the openings. S7. Deposit a passivation layer (600) on the entire chip surface, and open holes for the N and P electrodes of the Micro LED chip, depositing the N and P electrodes at the openings.
5. The method for fabricating vertically stacked high-voltage Micro LED chips according to claim 4, characterized in that, The first chip bonding temporary substrate (400) is for the subsequent process of removing the first substrate (101). The temporary substrate (400) is removed after the first chip and the second chip are bonded.
6. The method for fabricating high-voltage Micro LED chips stacked vertically according to claim 4, characterized in that, The metal electrode (700) deposited on the stepped mesa structure connects the N-type GaN layer of the first LED light-emitting layer (201) to the second transparent conductive layer (302), thereby realizing the electrical connection between the first chip and the second chip.
7. The method for fabricating vertically stacked high-voltage Micro LED chips according to claim 6, characterized in that, The passivation layer (600) deposited in step S7 will cover the metal electrodes (700) connecting the first chip and the second chip.
8. The method for fabricating vertically stacked high-voltage Micro LED chips according to claim 4, characterized in that, The passivation layer (600) is silicon dioxide.
9. The method for fabricating vertically stacked high-voltage Micro LED chips according to claim 4, characterized in that, The N electrode hole is located on the upper surface of the N-type GaN layer of the second LED light-emitting layer (202), and the P electrode hole is located on the upper surface of the first transparent conductive layer (301).
10. The method for fabricating vertically stacked high-voltage Micro LED chips according to claim 4, characterized in that, Metal electrodes are deposited on the pore sites of the N and P electrodes, which are the corresponding N and P electrodes.
Citation Information
Patent Citations
Tandem full-color display Micro-LED chip and manufacturing method thereof
CN116564947A
Miniature light-emitting diode, preparation method thereof and light-emitting device
CN115732610A
Vertically stacked LED chip, manufacturing method, device and manufacturing method thereof
CN115763454A