laminated polyester film
By forming a coating layer containing carboxyl polyurethane resin and crosslinking agent on the surface of polyester film, the problem of poor adhesion of polyester film surface, especially insufficient adhesion to UV curable ink, is solved, achieving high level, long-term adhesion and resistance to damp heat.
Patent Information
- Application Number
- CN202311417812.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Priority Date
- 2019-10-29
- Filing Date
- 2020-10-23
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2040-10-23
AI Technical Summary
Existing polyester films have poor surface adhesion, especially with UV-curable inks, and it is difficult to maintain a high level of adhesion over a long period of time.
A coating layer is formed on the surface of a polyester film. The coating layer contains a polyurethane resin having carboxyl groups and an acid value of 30-50 mg KOH/g and a crosslinking agent. The crosslinking agent also has carboxyl groups and an acid value of 30-50 mg KOH/g, preferably using an isocyanate-based compound as the crosslinking agent.
It improves the adhesion of polyester film to UV-curable resins, especially UV-curable inks, maintains a high level of adhesion over a long period of time, and improves resistance to damp heat.
Smart Images

Figure BDA0004520098470000241 
Figure BDA0004520098470000281
Abstract
Description
[0001] This application is a divisional application of the application filed on October 23, 2020, with application number 202080075402.1 and invention title "Laminated Polyester Film". Technical Field
[0002] This invention relates to laminated polyester films. More specifically, this invention relates to laminated polyester films comprising an easily adhesive coating layer that are highly suitable for use in all fields such as optics, packaging, and labeling.
[0003] Thermoplastic resin films, especially polyester films, possess excellent properties in terms of mechanical properties, electrical properties, dimensional stability, transparency, and chemical resistance. Therefore, these films are widely used in applications such as magnetic recording materials; packaging materials; solar cell applications; anti-reflective films for flat panel displays; diffusers; optical films such as prism sheets; and films for label printing. However, due to the highly oriented crystals on its surface, polyester films exhibit poor adhesion to various coatings, resins, and inks during processing for these applications.
[0004] To this end, various methods have been studied to impart adhesive properties to the surface of polyester films.
[0005] For example, surface activation methods are known to date as a way to impart adhesion, including methods such as corona discharge treatment, ultraviolet irradiation treatment, and plasma treatment of the surface of the substrate polyester film. However, the adhesion effect obtained by these treatments decreases over time, making it difficult to maintain a high level of adhesion for a long period of time (Patent Document (PTL) 1).
[0006] Therefore, methods including applying various resins to the surface of polyester films to form an easy-to-adhere coating layer are frequently used.
[0007] To date, a technique is known that involves forming a coating layer using a coating liquid containing a copolyester resin or a polyurethane resin, or using a coating liquid containing a copolyester resin, a polyurethane resin, and a crosslinking agent, to enhance affinity with them, thereby enabling easy adhesion to resin components such as polyurethane acrylates or acrylates used in hard coating agents and prism lens agents (Patent Documents (PTL) 2 and 3). However, UV-curable inks (ultraviolet-curable inks) used for label printing contain dyes or pigments that express hue in addition to resins, with pigments exhibiting good lightfastness comprising approximately 15–25 wt.% of the ink composition. Furthermore, since white inks requiring opacity contain a high proportion of white pigment (approximately 50 wt.%), conventional techniques are still insufficient to achieve good adhesion to white inks, especially when white inks are cured under low doses of UV irradiation.
[0008] Citation List
[0009] Patent documents
[0010] PTL 1: JPS58-27724A
[0011] PTL 2: JP2000-229355A
[0012] PTL 3: JP2009-220376A Summary of the Invention
[0013] The problem the invention aims to solve
[0014] The present invention was made in view of the aforementioned problems of the prior art. More specifically, the object of the present invention is to provide a laminated polyester film that exhibits good adhesion to UV-curable resins, particularly coating agents such as UV-curable inks, and also demonstrates excellent adhesion over a long period of time.
[0015] Solution for solving the problem
[0016] Specifically, the present invention has the following features.
[0017] 1. A laminated polyester film, comprising:
[0018] Polyester film and,
[0019] A coating layer on at least one surface of the polyester film,
[0020] The coating layer comprises a composition containing: a polyurethane resin having carboxyl groups and an acid value of 30-50 mg KOH / g, and a crosslinking agent having carboxyl groups and an acid value of 30-50 mg KOH / g.
[0021] 2. The laminated polyester film according to claim 1, wherein the crosslinking agent is an isocyanate compound.
[0022] The effects of the invention
[0023] The laminated polyester film of the present invention exhibits excellent adhesion to UV-curable resins such as hard coatings, lens layers, and inks, and in particular, it has a high level of adhesion to UV-curable inks. Detailed Implementation
[0024] Polyester film substrate
[0025] Examples of polyester resins that can be used to form the polyester film substrate of the present invention include polyethylene terephthalate, polyethylene terephthalate, polyethylene 2,6-naphthalenedicarboxylate, and polyethylene terephthalate; copolyester resins in which a portion of the diol component or dicarboxylic acid component of the above-mentioned polyester resins is replaced by a copolymer component. Examples of such copolymer components include, for example, diethylene glycol, neopentyl glycol, 1,4-cyclohexanediol, polyalkylene glycol, and other diol components; and, for example, adipic acid, sebacic acid, phthalic acid, isophthalic acid, sodium 5-isophthalate, 2,6-naphthalenedicarboxylic acid, and other dicarboxylic acid components; and so on.
[0026] The polyester resin preferably used in the polyester film substrate of the present invention is mainly selected from polyethylene terephthalate, polyethylene terephthalate, polyethylene butylene terephthalate, and polyethylene 2,6-naphthalate. Among these polyester resins, polyethylene terephthalate is most preferred from the viewpoint of balancing physical properties and cost. The polyester film substrate formed using such a polyester resin is preferably a biaxially stretched polyester film, which can improve chemical resistance, heat resistance, mechanical strength, etc.
[0027] There are no particular limitations on the polycondensation catalyst used in the production of polyester resins. From the viewpoint of low cost and excellent catalytic activity, antimony trioxide is preferred. The use of germanium compounds or titanium compounds is also preferred. Examples of more preferred polycondensation catalysts include catalysts containing aluminum and / or aluminum compounds and phenolic compounds; catalysts containing aluminum and / or aluminum compounds and phosphorus compounds; and catalysts containing aluminum salts of phosphorus compounds.
[0028] The layer structure of the polyester film substrate of the present invention is not particularly limited. It can be a single-layer polyester film, a two-layer polyester film with different compositions, or a polyester film substrate composed of at least three layers including an outer layer and an inner layer.
[0029] Coating layer
[0030] To improve adhesion to hard coatings, adhesion to UV-curable inks, and resistance to tack, the laminated polyester film of the present invention preferably has a coating layer formed on at least one surface of the polyester film using a composition comprising a polyurethane resin having carboxyl groups and an acid value of 30-50 mg KOH / g and a crosslinking agent having carboxyl groups and an acid value of 30-50 mg KOH / g. The coating layer may be formed on both surfaces of the polyester film; or it may be formed on only one surface of the polyester film, and a different type of resin coating layer may be formed on the other surface.
[0031] The coating layer of the present invention exhibits excellent adhesion to UV-curable or thermosetting resins such as hard coatings, lens layers, or inks, and particularly excellent adhesion to inks containing pigments. This effect is presumably due to the interaction between the carboxyl groups in the coating layer and the pigment particles in the ink. Furthermore, since both the polyurethane resin and the crosslinking agent contain a certain amount of carboxyl groups, the present invention allows the coating layer itself to contain many carboxyl groups, while suppressing disadvantages such as poor resistance to damp heat caused by reduced water resistance due to the presence of many carboxyl groups in only one resin.
[0032] The weight ratio of the carboxyl-containing polyurethane resin to the carboxyl-containing crosslinking agent is preferably in the range of 90 / 10 to 10 / 90, more preferably 80 / 20 to 20 / 80, and even more preferably 70 / 30 to 30 / 70. If the amount of crosslinking agent is low, durability such as resistance to damp heat is reduced. On the other hand, if the amount of polyurethane resin is low, adhesion is reduced.
[0033] The components of the coating layer will be described in detail below.
[0034] Polyurethane resins containing carboxyl groups and with an acid value of 30–50 mg KOH / g
[0035] A polyurethane resin containing a carboxyl group refers to a polyurethane resin synthesized using at least a polyol component and a polyisocyanate component, and further using chain extenders, etc., as needed; and containing a carboxyl group in the molecule or side chain. The term "carboxyl group in the molecule" as used herein refers to a carboxyl group present in the main chain or at least one end of the polyurethane resin. The term "carboxyl group in the side chain" as used herein refers to a carboxyl group introduced into the branch chain of the polyurethane resin by synthesizing or polymerizing at least one raw material component having three or more terminal functional groups, such as those described above.
[0036] In this invention, the polyurethane resin with carboxyl groups is obtained by primarily using a carboxyl-containing polyol component as the urethane component.
[0037] Examples of carboxyl-containing polyol components include relatively high molecular weight polyols, such as carboxyl-containing polyalkylene glycols, carboxyl-containing acrylic polyols, carboxyl-containing polyolefin polyols, and carboxyl-containing polyester polyols. Examples also include relatively low molecular weight polyols, such as 2,2-dimethylolpropionic acid, 2,2-dimethylolbutyric acid, 2,2-dimethylolbutyric acid, and 2,2-dimethylolvalerate. Dimethylolpropionic acid and dimethylolbutyric acid are particularly preferred for introducing carboxyl groups.
[0038] The acid value of the polyurethane resin containing carboxyl groups is preferably 30–50 mg KOH / g, more preferably 35–45 mg KOH / g. When the acid value is 30 mg KOH / g or higher, the adhesion to UV-curable resins, especially UV-curable inks, increases. On the other hand, an acid value of 50 mg KOH / g or lower is preferred because it maintains the water resistance of the coating layer and the films do not tend to adhere to each other due to moisture absorption. To compensate for the water solubility or water dispersibility of the polyurethane resin, other hydrophilic groups, such as hydroxyl, ether, sulfonic acid, phosphonic acid, and quaternary ammonium groups, can be introduced into the polyurethane resin of the present invention, as long as the performance is not degraded.
[0039] The carboxyl groups in polyurethane resins can be neutralized by basic compounds. Basic compounds suitable for neutralization include alkali metals such as sodium and potassium, alkaline earth metals such as magnesium and calcium, and organic amine compounds. Among these, organic amine compounds that readily dissociate from the carboxyl groups upon heating are preferred. Examples of organic amine compounds include ammonia; C1-20 straight-chain or branched primary, secondary, or tertiary amines, such as methylamine, ethylamine, propylamine, isopropylamine, butylamine, 2-ethylhexylamine, cyclohexylamine, dimethylamine, diethylamine, dipropylamine, diisopropylamine, dibutylamine, trimethylamine, triethylamine, triisopropylamine, tributylamine, and ethylenediamine; cyclic amines, such as morpholine, N-alkylmorpholine, and pyridine; hydroxyl-containing amines, such as monoisopropanolamine, methylethanolamine, methylisopropanolamine, dimethylethanolamine, diisopropanolamine, diethanolamine, triethanolamine, diethylethanolamine, and triethanolamine; and so on.
[0040] Preferred examples of other polyol components used in the synthesis and polymerization of the polyurethane resin of the present invention include polycarbonate polyols. Particularly preferred are aliphatic polycarbonate polyols with excellent heat resistance and hydrolysis resistance. Examples of aliphatic polycarbonate polyols include aliphatic polycarbonate diols and aliphatic polycarbonate triols. Preferably, aliphatic polycarbonate diols can be used. Examples of aliphatic polycarbonate diols used in the synthesis and polymerization of the polycarbonate-structured polyurethane resin of the present invention include aliphatic polycarbonate diols obtained by reacting one or more diols with a carbonate. Examples of diols include ethylene glycol, propylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, 1,9-nonanediol, 1,8-nonanediol, neopentanediol, diethylene glycol, dipropylene glycol, etc. Examples of carbonates include dimethyl carbonate, ethylene carbonate, phosgene, etc.
[0041] The number-average molecular weight of the polycarbonate polyol of the present invention is preferably 300 to 5000, more preferably 400 to 4000, and most preferably 500 to 3000. For improved ink adhesion, a number-average molecular weight of 300 or higher is preferred. For improved anti-blocking properties, a number-average molecular weight of 3000 or less is preferred.
[0042] Examples of polyisocyanates used in the synthesis or polymerization of the polyurethane resins of the present invention include aliphatic diisocyanates having an aromatic ring, such as xylene diisocyanate; alicyclic diisocyanates, such as isophorone diisocyanate, 4,4-dicyclohexylmethane diisocyanate, 1,3-bis(isocyanate methyl)cyclohexane; aliphatic diisocyanates, such as hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate; modified polyisocyanates containing isocyanurate bonds, biuret bonds, or ureocarbamate bonds, each derived from a diisocyanate; and polyisocyanates produced by adding one or more diisocyanates to, for example, trimethylolpropane. The above-described aliphatic diisocyanates, alicyclic diisocyanates, or aliphatic diisocyanates having an aromatic ring are preferred because they do not cause yellowing problems.
[0043] Examples of chain extenders include diols, such as ethylene glycol, diethylene glycol, 1,4-butanediol, neopentyl glycol, and 1,6-hexanediol; polyols, such as glycerol, trimethylolpropane, and pentaerythritol; diamines, such as ethylenediamine, hexamethylenediamine, and piperazine; amino alcohols, such as monoethanolamine and diethanolamine; thiodiethylene glycols, such as thiodiethylene glycol; and water. Polyols and polyamines with three or more functional groups can also be used, provided the amount is small.
[0044] The polyurethane resin of the present invention may have reactive groups, such as end-capped isocyanates, in one or both ends of the resin or in one or more side chains to improve toughness.
[0045] Crosslinking agent
[0046] In this invention, a crosslinking agent having a carboxyl group and an acid value of 30–50 mg KOH / g is used. Similar to the case of the polyurethane resin described above, the carboxyl group of the crosslinking agent can be neutralized with an alkaline compound. The acid value of the crosslinking agent having a carboxyl group is preferably 30–50 mg KOH / g, more preferably 35–45 mg KOH / g. An acid value of 30 mg KOH / g or higher is preferred because it improves adhesion to UV-curable resins, especially UV-curable inks. On the other hand, an acid value of 50 mg KOH / g or lower is preferred because it maintains the water resistance of the applied coating and makes it less likely to adhere easily to each other due to moisture absorption. To compensate for the water solubility or water dispersibility of the crosslinking agent of this invention, other hydrophilic groups, such as hydroxyl, ether, sulfonic acid, phosphonic acid, and quaternary ammonium groups, can be introduced, as long as the performance is not degraded.
[0047] Examples of crosslinking agents containing carboxyl groups include oxazoline compounds, carbodiimide compounds, epoxy compounds, and isocyanate compounds that incorporate one or more carboxyl groups into the molecule. The carboxyl groups may also be pre-neutralized with a basic compound to prevent intramolecular or intermolecular reactions with the introduced carboxyl groups. Among these crosslinking agents, isocyanate compounds that readily incorporate carboxyl groups into the molecule are preferred, and terminally capped isocyanate compounds are particularly preferred.
[0048] Examples of end-capping agents include sulfite compounds such as sodium bisulfite; pyrazole compounds such as 3,5-dimethylpyrazole, 3-methylpyrazole, 4-bromo-3,5-dimethylpyrazole, and 4-nitro-3,5-dimethylpyrazole; phenolic compounds such as phenol and cresol; aliphatic alcohol compounds such as methanol and ethanol; active methylene compounds such as dimethyl malonate and acetylacetone; thiol compounds such as butanethiol and dodecylthiol; acid amide compounds such as acetanilide and acetamide; lactam compounds such as ε-caprolactam and δ-valeronamide; acid imide compounds such as succinimide and maleimide; oxime compounds such as acetaldehyde oxime, acetone oxime, and methyl ethyl ketone oxime; amine compounds such as diphenylaniline, aniline, and ethyleneimine; and so on.
[0049] The lower limit of the boiling point of the capping agent for the isocyanate is preferably 150°C, more preferably 160°C, even more preferably 180°C, particularly preferably 200°C, and most preferably 210°C. The higher the boiling point of the capping agent, the better it suppresses the volatilization of the capping agent caused by heating during the drying process after coating and during film formation in the case of online coating, and the better it suppresses the formation of minute irregularities on the coating surface, thereby improving the transparency of the film. Although the upper limit of the boiling point of the capping agent is not particularly limited, around 300°C seems to be an upper limit for production purposes. Since the boiling point is related to molecular weight, it is preferable to use a capping agent with a high molecular weight to increase the boiling point of the capping agent. The molecular weight of the capping agent is preferably 50 or more, more preferably 60 or more, and even more preferably 80 or more.
[0050] The upper limit of the dissociation temperature of the capping agent is preferably 200°C, more preferably 180°C, even more preferably 160°C, particularly preferably 150°C, and most preferably 120°C. The capping agent dissociates during the drying process after coating or during film formation in the case of online coating, generating regenerated isocyanate groups. Therefore, the crosslinking reaction of the polyurethane resin, etc., progresses, thereby improving adhesion. If the dissociation temperature of the capping isocyanate is below the above-mentioned temperature, the dissociation of the capping agent progresses sufficiently, resulting in good adhesion, especially good resistance to damp heat.
[0051] Examples of capping agents with a dissociation temperature below 120°C and a boiling point above 150°C, which can be used in the capping isocyanates of the present invention, as described above, include sodium bisulfite, 3,5-dimethylpyrazole, 3-methylpyrazole, dimethyl malonate, diethyl malonate, acetone oxime, and methyl ethyl ketone oxime. Among these, pyrazole compounds such as 3,5-dimethylpyrazole and 3-methylpyrazole are preferred due to their resistance to damp heat and yellowing.
[0052] The capped isocyanate preferably has two or more functional groups. In view of the crosslinking properties of the coating film, the capped isocyanate having three or more functional groups is more preferred.
[0053] Polyisocyanates having three or more functional groups, which serve as precursors to the terminated isocyanates of the present invention, can preferably be obtained from isocyanate monomers. Examples include biuret, isocyanurates, and adducts obtained by modifying isocyanate monomers having two isocyanate groups, such as aromatic diisocyanates, aliphatic diisocyanates, aromatic aliphatic diisocyanates, or alicyclic diisocyanates.
[0054] Biuret is a self-condensing compound having a biuret bond formed by the self-condensation of an isocyanate monomer. Examples include biuret of hexamethylene diisocyanate.
[0055] Isocyanurates are trimers of isocyanate monomers. Examples include trimers of hexamethylene diisocyanate, isophorone diisocyanate, and toluene diisocyanate.
[0056] Adducts are isocyanate compounds containing three or more functional groups, obtained by reacting an isocyanate monomer with a low molecular weight compound containing three or more active hydrogen functional groups. Examples include compounds obtained by reacting trimethylolpropane with hexamethylene diisocyanate, compounds obtained by reacting trimethylolpropane with toluene diisocyanate, compounds obtained by reacting trimethylolpropane with xylene diisocyanate, and compounds obtained by reacting trimethylolpropane with isophorone diisocyanate.
[0057] Examples of isocyanate monomers include aromatic diisocyanates, such as 2,4-toluene diisocyanate, 2,6-toluene diisocyanate, 4,4'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, 1,5-naphthalene diisocyanate, 1,4-naphthalene diisocyanate, benzene diisocyanate, tetramethylxylene diisocyanate, 4,4'-diphenyl ether diisocyanate, 2-nitrodiphenyl-4,4'-diisocyanate, 2,2'-diphenylpropane- 4,4'-diisocyanates, 3,3'-dimethyldiphenylmethane-4,4'-diisocyanate, 4,4'-diphenylpropane diisocyanate, 3,3'-dimethoxydiphenyl-4,4'-diisocyanate, and xylene diisocyanate, etc.; alicyclic diisocyanates, such as isophorone diisocyanate, 4,4-dicyclohexylmethane diisocyanate, 1,3-bis(isocyanate-methyl)cyclohexane, etc.; and aliphatic diisocyanates, such as hexamethylene diisocyanate and 2,2,4-trimethylhexamethylene diisocyanate, etc. Aliphatic and alicyclic diisocyanates and their modified forms are preferred due to their transparency, resistance to yellowing, adhesion, and resistance to damp heat.
[0058] In this invention, one or more other resins can be used with polyurethane resin and crosslinking agent, as long as they do not affect performance. Examples of such other resins used with polyurethane resin include carboxyl-free polyurethane, polyester resin, acrylic resin, cellulose resin, polyolefin resin, polyacetal resin, etc. Among these resins, polyester resin is particularly preferred because it improves adhesion to UV-curable resin when used with polyurethane resin. When polyester resin is used with polyurethane resin, the content of polyester resin can be more than 1.5 times the combined content of carboxyl-containing polyurethane resin and carboxyl-containing crosslinking agent. Because polyester resin has better affinity for substrates than carboxyl-containing polyurethane resin or carboxyl-containing crosslinking agent, polyester resin can be easily positioned on the substrate side in the thickness direction, increasing adhesion to the substrate. The carboxyl-containing polyurethane resin and carboxyl-containing crosslinking agent located on the surface of the coating layer exhibit a synergistic effect of increasing adhesion to UV-curable resin.
[0059] Polyester resin
[0060] In this invention, the polyester resin used to form the coating layer can be linear; however, polyester resins containing dicarboxylic acids and branched diols (diols) or diols having one or more ether bonds are preferred. Examples of dicarboxylic acids mentioned herein mainly include aliphatic dicarboxylic acids such as adipic acid and sebacic acid; and aromatic dicarboxylic acids such as terephthalic acid, isophthalic acid, phthalic acid, and 2,6-naphthalenedicarboxylic acid. Branched diols refer to diols having branched alkyl groups. Examples include 2,2-dimethyl-1,3-propanediol, 2-methyl-2-ethyl-1,3-propanediol, 2-methyl-2-butyl-1,3-propanediol, 2-methyl-2-propyl-1,3-propanediol, 2-methyl-2-isopropyl-1,3-propanediol, 2-methyl-2-n-hexyl-1,3-propanediol, 2,2-diethyl-1,3-propanediol, 2-ethyl-2-n-butyl-1,3-propanediol, 2-ethyl-2-n-hexyl-1,3-propanediol, 2,2-di-n-butyl-1,3-propanediol, 2-n-butyl-2-propyl-1,3-propanediol, 2,2-di-n-hexyl-1,3-propanediol, etc.
[0061] In addition, examples of diols containing one or more ether bonds include condensation products of alkylene glycols such as diethylene glycol, triethylene glycol, and dipropylene glycol; ethylene oxide adducts of bisphenol compounds; and propylene oxide adducts of bisphenol compounds. The number of ether bonds in the molecule is not particularly limited, but is preferably four or less, more preferably two or less, because a large number of ether bonds can reduce the strength or glass transition temperature of the polyester resin.
[0062] In the polyester resin, the branched diol component or diol component containing one or more ether bonds, as a more preferred embodiment described above, is considered to be present in a proportion of 10 mol% or more, more preferably 20 mol% or more, based on the total diol component. A content of 10 mol% or more is preferred because the crystallinity will not be too high and the adhesion of the coating layer is maintained. The upper limit of the diol component content in the total diol component is preferably 80 mol% or less, more preferably 70 mol% or less by mass. A diol component content of 80 mol% or less is preferred because the concentration of oligomers as byproducts is unlikely to increase, which maintains the transparency of the coating layer. Ethylene glycol is most preferred as a diol component other than the aforementioned compounds. Propylene glycol, butanediol, hexanediol, 1,4-cyclohexanediethanol, etc., can be used, as long as the amount is small.
[0063] The most preferred dicarboxylic acid component of the polyester resin is terephthalic acid or isophthalic acid. In addition to the aforementioned dicarboxylic acids, 1 to 10 mol% of 5-sulfoisophthalic acid is preferably copolymerized to impart water dispersibility to the copolyester resin. Examples of such compounds include sulfoterephthalic acid, 5-sulfoisophthalic acid, and sodium 5-sulfoisophthalate.
[0064] When the total solids content of the resin and crosslinking agent in the coating liquid for forming the coating layer is defined as 100% by mass, a polyester resin content of 10% by mass or more is preferred because it provides good adhesion between the coating layer and the polyester film substrate. The upper limit of the polyester resin content is preferably 65% by mass or less, more preferably 60% by mass or less. A polyester resin content of 70% by mass or less is preferred because it provides good heat resistance after ink processing.
[0065] Resins other than polyester resins can also be used in the coating layer, as long as the film performance is not impaired. A typical example of a resin other than polyester resin is a carboxyl-containing polyurethane resin. Other resins may also be included, or only carboxyl-containing polyurethane resins may be used. In this case, when the total solids content of the resin and crosslinking agent in the coating liquid for forming the coating layer is 100% by mass, the content of the resin other than polyester resin is preferably 40% by mass or less, more preferably 30% by mass or less, and particularly preferably 20% by mass or less. The total content of polyester resin and resins other than polyester resin is preferably 70% by mass or less. Based on the total solids content of the resin and crosslinking agent, the content of polyurethane resin and the content of crosslinking agent in the coating liquid for forming the coating layer are each preferably 3% by mass or more.
[0066] A content of 3% by mass or more is preferred because it provides excellent adhesion to UV-curable resins and coating agents such as UV-curable inks. This content is more preferably in the range of 3.5% to 90% by mass, more preferably 7% to 80% by mass, and particularly preferably 10.5% to 70% by mass.
[0067] additive
[0068] The coating layer of the present invention may contain known additives, such as surfactants, antioxidants, heat stabilizers, weather stabilizers, ultraviolet absorbers, organic lubricants, pigments, dyes, organic or inorganic particles, antistatic agents and nucleating agents, as long as they do not impair the effects of the present invention.
[0069] In a preferred embodiment of the invention, particles are added to the coating layer to further improve the coating layer's resistance to adhesion. Examples of particles contained in the coating layer in this invention include inorganic particles such as titanium dioxide, barium sulfate, calcium carbonate, calcium sulfate, silica, alumina, talc, kaolin, clay, or mixtures thereof, or combinations thereof with other general inorganic particles such as calcium phosphate, mica, lithium montmorillonite, zirconium oxide, tungsten oxide, lithium fluoride, and calcium fluoride; organic polymer particles, such as styrene, acrylics, melamine, benzoguanamine, silicone, etc.; and so on.
[0070] The average particle size of the particles in the coating layer (based on the average particle size of the number of particles measured by scanning electron microscopy (SEM), the same below) is preferably 0.04 to 2.0 μm, more preferably 0.1 to 1.0 μm. Inert particles with an average particle size of 0.04 μm or more are preferred because they easily form irregularities on the film surface, resulting in improved film operability, such as slipability and winding ability, and good processability during bonding. On the other hand, inert particles with an average particle size of 2.0 μm or less are preferred because the particles are less likely to detach. Based on the solid composition of the coating layer, the particle concentration in the coating layer is preferably 1 to 20% by mass.
[0071] The average particle size was measured by a method that included observing 30 particles in a cross-section of the laminated polyester film using a scanning electron microscope and defining the average particle size as the average particle size.
[0072] The shape of the particles is not particularly limited, as long as it meets the purpose of this invention. Spherical particles or non-spherical particles with irregular shapes can be used. The particle size of particles with irregular shapes can be calculated as the circular equivalent diameter. The circular equivalent diameter is obtained by dividing the observed area of the particle by π, calculating the square root, and doubling the value of the square root.
[0073] Production of laminated polyester film
[0074] The method for producing the laminated polyester film of the present invention will be described using a polyethylene terephthalate (PET) film substrate as an example. However, naturally, the method of the present invention is not limited to this example.
[0075] After the PET resin is thoroughly dried in a vacuum, it is fed into an extruder. The molten PET resin at approximately 280°C is molten and extruded from a T-die in sheet form onto a rotating cooling roller. The sheet is then cured by applying electrostatic cooling, thus forming an unstretched PET sheet. The unstretched PET sheet can be single-layered or multi-layered through co-extrusion.
[0076] The resulting unstretched PET sheet is subjected to uniaxial or biaxial stretching for crystal orientation. For example, in biaxial stretching, the unstretched PET sheet is stretched longitudinally by 2.5 to 5.0 times using rollers heated to 80–120°C to obtain a uniaxially stretched PET film; then, the ends of the film are clamped and guided to a hot air zone heated to 80–180°C, and then stretched 2.5–5.0 times in the width direction. In uniaxial stretching, the unstretched PET sheet is stretched 2.5–5.0 times in a tenter frame. After stretching, the resulting film is guided to a heat treatment zone and subjected to heat treatment to complete crystal orientation.
[0077] The lower limit of the temperature in the heat treatment zone is preferably 170°C, more preferably 180°C. A temperature of 170°C or higher is preferred because curing proceeds sufficiently, good anti-blocking properties are achieved in the presence of liquid water, and drying does not require a long time. On the other hand, the upper limit of the temperature in the heat treatment zone is preferably 250°C, more preferably 240°C. A temperature of 240°C or lower is preferred because it reduces the possibility of film degradation.
[0078] The coating layer can be formed after or during film production. In particular, for productivity reasons, it is preferable to form the coating layer at any stage of the film production process; that is, it is preferable to form the coating layer by applying a coating liquid to at least one surface of an unstretched or uniaxially stretched PET film, stretching it along at least one axial direction, and heat-treating the resulting film.
[0079] Coating solutions can be applied to PET films using any known method. Examples of available methods include reverse roll coating, gravure coating, kiss coating, die coating, roller brush coating, spray coating, air knife coating, wire bar coating, tube doctor blade coating, dip coating, curtain coating, etc. These methods can be used alone or in combination to apply the coating solution.
[0080] In this invention, the thickness of the coating layer can be appropriately determined within the range of 0.001 to 2.00 μm. To balance processability and adhesion, this thickness is preferably in the range of 0.01 to 1.00 μm, more preferably 0.02 to 0.80 μm, and even more preferably 0.05 to 0.50 μm. A coating layer thickness of 0.001 μm or more is preferred due to good adhesion. A coating layer thickness of 2.00 μm or less is preferred because adhesion is unlikely to occur.
[0081] The upper limit of haze of the laminated polyester film of the present invention is preferably 2.5%, more preferably 2.0%, even more preferably 1.5%, and particularly preferably 1.2%. Given its transparency, a laminated polyester film with a haze of 2.5% or less is preferred, as it is suitable for use in optical films requiring transparency. Generally, a lower haze value is preferred. However, a haze of 0.1% or more is also preferred, and even a haze of 0.2% or more is preferred.
[0082] Example
[0083] The present invention will now be described in more detail with reference to embodiments and comparative examples. However, the present invention is not limited to the following embodiments. The evaluation method used in the present invention will be described first.
[0084] (1) Haze
[0085] The haze of the laminated polyester film was measured using a turbidimeter (NDH5000, manufactured by Nippon Denshoku Industries, Co., Ltd.) in accordance with JISK 7136:2000.
[0086] (2) Acid value
[0087] The acid values of the resin and crosslinking agent were measured by titration as described in JIS K1557-5:2007.
[0088] When measuring carboxyl groups neutralized with amines, the measurement is performed after removing the amines by high-temperature treatment or by pretreatment with hydrochloric acid to release or remove them. When measuring crosslinking agents, reactive groups such as isocyanate groups are reacted with amines before measurement. If the resin to be measured has poor solubility in isopropanol, an solvent, N-methylpyrrolidone is used instead of isopropanol. Complete control measurements were performed in all of the above-mentioned treatments.
[0089] (3) Anti-adhesion
[0090] Two identical membrane samples were stacked on top of each other with their coated surfaces facing each other. A load of 98 kPa was applied to ensure close contact between the two identical membrane samples, and they were placed in an atmosphere at 50°C for 24 hours. The two identical membrane samples were then separated, and the separation status was evaluated according to the following criteria.
[0091] 〇: These two layers can be easily separated from each other without one coating layer being arbitrarily transferred to the other.
[0092] △: The coating layer remains largely intact; however, the surface layer of one coating layer is partially transferred to the opposite surface.
[0093] ×: The two sheets are bonded together so tightly that they cannot be separated from each other; or even if the two sheets can be separated from each other, cracking of the membrane substrate will occur.
[0094] (4) UV-curable ink adhesion
[0095] Using a printing press (trade name "RI Tester", manufactured by Akira Seisakusho Co., Ltd.), two rollers apply UV-curable ink (trade names "BEST CURE UV161 Indigo S" or "BEST CURE UV161 White S"; both manufactured by T&K TOKA Co., Ltd.) to a coated layer of laminated polyester film at a volume of 4 on the ink tube to form a print. Subsequently, a high-pressure mercury lamp is used with 100 or 40 mJ / cm² ink. 2UV light is used to irradiate the film coated with the ink layer, thereby curing the UV-curable ink. Then, cuts are made through the ink layer to the film substrate using a 2mm spaced cutter guide to form a grid of 100 squares on the ink layer surface. Next, cellophane tape (manufactured by Nichiban Co., Ltd., No. 405, width: 24mm) is firmly adhered to the cut surfaces in a grid pattern to ensure complete adhesion. The cellophane tape is then vertically peeled from the ink layer surface of the ink laminate, and the number of squares peeled from the ink layer surface is visually counted. The adhesion between the ink layer and the film substrate is determined according to the following formula. Partially peeled squares are also counted as peels.
[0096] Ink adhesion (%) = 100 - (number of peeled squares)
[0097] The ink adhesion is evaluated according to the following criteria.
[0098] ◎: 100%
[0099] 0: 96-99%
[0100] △: 80-95%
[0101] ×: Less than 80%
[0102] In the evaluation criteria, ◎ and 〇 are acceptable levels.
[0103] (5) Adhesion to hard coatings
[0104] The UV-curable hard coating agent Opstar Z7503 (manufactured by Arakawa Chemical Industries, Ltd.) was applied to the coating layer of the laminated polyester film using a #5 wire rod and dried at 80°C for 1 minute. The film coated with the hard coating agent was then dried under a high-pressure mercury lamp at 100 mJ / cm². 2 The film is obtained by irradiating it with ultraviolet light, thereby obtaining a hard coating film with a thickness of 4μm.
[0105] Subsequently, using a 2mm spaced cutter guide, incisions were made through the hard coating to reach the membrane substrate, forming a grid of 100 squares. Cellophane tape (manufactured by Nichiban Co., Ltd., No. 405, width: 24mm) was then firmly adhered to the cut surfaces in a grid pattern to ensure complete adhesion. The cellophane tape was then vertically peeled off the hard coating surface of the hard-coated laminate. After this peeling operation was performed five times in the same location, the number of squares peeled off from the hard coating surface of the hard-coated laminate was visually counted, and the adhesion between the hard coating and the membrane substrate was determined according to the following formula. Partially peeled squares were also counted as peels.
[0106] Adhesion to hard coatings (%) = 100 - (number of peeled squares)
[0107] The adhesion between the hard coating and the film substrate is evaluated according to the following criteria.
[0108] ◎: 100%
[0109] 0: 96-99%
[0110] △: 80-95%
[0111] ×: Less than 80%
[0112] In the evaluation criteria, ◎ and 〇 are acceptable levels.
[0113] (6) Resistance to damp heat
[0114] The UV-curable ink coating film prepared in the same manner as described in (4) and (5) above (after applying BEST CUREUV161 White) was subjected to a curing process at 100 mJ / cm 2 The UV-cured product and the hard-coated film were placed in an environment of 80°C and 80% RH for 500 hours with the coated surface in a vertical position, without any other film or object in contact with the coated surface. After treatment, the film was placed in an environment of 23°C and 65% RH for 10 minutes with no other film or object in contact with the coated surface. After this period of time, the adhesion of the coated surface was immediately evaluated in the same manner as described above.
[0115] Polymerization of polyurethane resin A-1
[0116] 82.8 parts by weight of hydrogenated m-xylene diisocyanate, 25.0 parts by weight of dimethylolpropionic acid, 21.0 parts by weight of 1,6-hexanediol, and 150.0 parts by weight of polyester glycol containing adipic acid and 1,4-butanediol with a number average molecular weight of 2000, along with 110 parts by weight of methyl ethyl ketone as solvent, were placed in a four-necked flask equipped with a stirrer, a serpentine condenser, a nitrogen inlet tube, a silica gel drying tube, and a thermometer. The resulting mixture was stirred at 75°C for 3 hours under a nitrogen atmosphere, and the predetermined amine equivalent was confirmed to have been reached. Subsequently, after lowering the temperature of the reaction mixture to 40°C, 19.8 parts by weight of triethylamine were added to obtain a polyurethane polymer solution. Then, 500 g of water was added to a reaction vessel equipped with a homogenizer capable of high-speed stirring, and the temperature was adjusted to 25°C. The resulting mixture was passed through a homogenizer for 2000 min... -1 While stirring and mixing, a polyurethane polymer solution was added to obtain an aqueous dispersion. The solvent methyl ethyl ketone was then removed under reduced pressure. The concentration was adjusted with water to prepare a solution containing 35% by mass of polyurethane resin (A-1) with an acid value of 37.5 mg KOH / g.
[0117] Polymerization of polyurethane resin A-2
[0118] 63.0 parts by weight of hydrogenated m-xylene diisocyanate, 21.0 parts by weight of dimethylolpropionic acid, 147.0 parts by weight of polycarbonate diol (derived from 1,6-hexanediol) with a number average molecular weight of 2000, and 110 parts by weight of methyl ethyl ketone as solvent were placed in a four-necked flask equipped with a stirrer, a serpentine condenser, a nitrogen inlet tube, a silica gel drying tube, and a thermometer. The resulting mixture was stirred at 75°C for 3 hours under a nitrogen atmosphere, and the predetermined amine equivalent was confirmed to have been reached. Subsequently, after the temperature of the reaction mixture was lowered to 40°C, 16.6 parts by weight of triethylamine were added to obtain a polyurethane polymer solution. Then, 500 g of water was added to a reaction vessel equipped with a homogenizer capable of high-speed stirring, and the temperature was adjusted to 25°C. The resulting mixture was passed through a homogenizer for 2000 min... -1 While stirring and mixing, a polyurethane polymer solution was added to obtain an aqueous dispersion. The solvent methyl ethyl ketone was then removed under reduced pressure. The concentration was adjusted with water to prepare a solution containing 35% by mass of polyurethane resin (A-2) with an acid value of 36.3 mg KOH / g.
[0119] Polymerization of polyurethane resin A-3
[0120] 64.5 parts by weight of hydrogenated diphenylmethane diisocyanate, 21.5 parts by weight of dimethylolpropionic acid, 11.2 parts by weight of neopentyl glycol, and 150.5 parts by weight of polycarbonate diol (derived from 1,6-hexanediol) with a number average molecular weight of 2000, along with 110 parts by weight of methyl ethyl ketone as a solvent, were placed in a four-necked flask equipped with a stirrer, a serpentine condenser, a nitrogen inlet tube, a silica gel drying tube, and a thermometer. The resulting mixture was stirred at 75°C for 3 hours under a nitrogen atmosphere, and the predetermined amine equivalent was confirmed to have been reached. Subsequently, after lowering the temperature of the reaction mixture to 40°C, 17.0 parts by weight of triethylamine were added to obtain a polyurethane polymer solution. Then, 500 g of water was added to a reaction vessel equipped with a homogenizer capable of high-speed stirring, and the temperature was adjusted to 25°C. The resulting mixture was passed through a homogenizer for 2000 min... -1 While stirring and mixing, a polyurethane polymer solution was added to obtain an aqueous dispersion. The solvent methyl ethyl ketone was then removed under reduced pressure. The concentration was adjusted with water to prepare a solution containing 35% by mass of polyurethane resin (A-3) with an acid value of 36.0 mg KOH / g.
[0121] Polymerization of polyurethane resin A-4
[0122] 83.4 parts by weight of hydrogenated m-xylene diisocyanate, 16.9 parts by weight of dimethylolpropionic acid, 28.4 parts by weight of 1,6-hexanediol, and 151.0 parts by weight of polyester glycol containing adipic acid and 1,4-butanediol with a number average molecular weight of 2000, along with 110 parts by weight of methyl ethyl ketone as solvent, were placed in a four-necked flask equipped with a stirrer, a serpentine condenser, a nitrogen inlet tube, a silica gel drying tube, and a thermometer. The resulting mixture was stirred at 75°C for 3 hours under a nitrogen atmosphere, and the predetermined amine equivalent was confirmed to have been reached. Subsequently, after cooling the reaction mixture to 40°C, 13.3 parts by weight of triethylamine were added to obtain a polyurethane polymer solution. Then, 500 g of water was added to a reaction vessel equipped with a homogenizer capable of high-speed stirring, and the temperature was adjusted to 25°C. The resulting mixture was passed through a homogenizer for 2000 min... -1 While stirring and mixing, a polyurethane polymer solution was added to obtain an aqueous dispersion. The solvent methyl ethyl ketone was then removed under reduced pressure. The concentration was adjusted with water to prepare a solution containing 35% by mass of polyurethane resin (A-4) with an acid value of 25.3 mg KOH / g.
[0123] Polymerization of polyurethane resin A-5
[0124] 104.9 parts by weight of hydrogenated m-xylene diisocyanate, 41.8 parts by weight of dimethylolpropionic acid, 19.0 parts by weight of 1,6-hexanediol, and 152.0 parts by weight of polyester glycol containing adipic acid and 1,4-butanediol with a number average molecular weight of 2000, along with 110 parts by weight of methyl ethyl ketone as solvent, were placed in a four-necked flask equipped with a stirrer, a serpentine condenser, a nitrogen inlet tube, a silica gel drying tube, and a thermometer. The resulting mixture was stirred at 75°C for 3 hours under a nitrogen atmosphere, and the predetermined amine equivalent was confirmed to have been reached. Subsequently, after lowering the temperature of the reaction mixture to 40°C, 33.1 parts by weight of triethylamine were added to obtain a polyurethane polymer solution. Then, 500 g of water was added to a reaction vessel equipped with a homogenizer capable of high-speed stirring, and the temperature was adjusted to 25°C. The resulting mixture was passed through a homogenizer for 2000 min... -1 While stirring and mixing, a polyurethane polymer solution was added to obtain an aqueous dispersion. The solvent methyl ethyl ketone was then removed under reduced pressure. The concentration was adjusted with water to prepare a solution containing 35% by mass of polyurethane resin (A-5) with an acid value of 55.0 mg KOH / g.
[0125] Polymerization of polyurethane resin A-6
[0126] 45.0 parts by weight of hydrogenated m-xylene diisocyanate, 20.0 parts by weight of 1,6-hexanediol, 1491.0 parts by weight of polyethylene glycol with a number average molecular weight of 2000, and 110 parts by weight of methyl ethyl ketone as solvent were placed in a four-necked flask equipped with a stirrer, a serpentine condenser, a nitrogen inlet tube, a silica gel drying tube, and a thermometer. The resulting mixture was stirred at 75°C for 3 hours under a nitrogen atmosphere, and the predetermined amine equivalent was confirmed to have been reached.
[0127] Subsequently, after lowering the temperature of the reaction mixture to 40°C, a polyurethane polymer solution was obtained. 500 g of water was added to a reaction vessel equipped with a homogenizer capable of high-speed stirring, and the temperature was adjusted to 25°C. The resulting mixture was then passed through a homogenizer for 2000 min... -1 While stirring and mixing, a polyurethane polymer solution is added to obtain an aqueous dispersion.
[0128] The solvent methyl ethyl ketone was then removed under reduced pressure. The concentration was adjusted with water to prepare a solution containing 35% by mass of polyurethane resin (A-6) with an acid value of 0.2 mg KOH / g.
[0129] Polymerization of polyurethane resin A-7
[0130] 43.8 parts by weight of hydrogenated diphenylmethane diisocyanate, 12.9 parts by weight of dimethylolbutyric acid, 153.4 parts by weight of polycarbonate diol (derived from 1,6-hexanediol) with a number average molecular weight of 2000, and 110 parts by weight of methyl ethyl ketone as solvent were placed in a four-necked flask equipped with a stirrer, a serpentine condenser, a nitrogen inlet tube, a silica gel drying tube, and a thermometer. The resulting mixture was stirred at 75°C for 3 hours under a nitrogen atmosphere, and the predetermined amine equivalent was confirmed to have been reached. Subsequently, after the temperature of the reaction mixture was lowered to 40°C, 8.8 parts by weight of triethylamine were added to obtain a polyurethane polymer solution. Then, 500 g of water was added to a reaction vessel equipped with a homogenizer capable of high-speed stirring, and the temperature was adjusted to 25°C. The resulting mixture was passed through a homogenizer for 2000 min... -1 While stirring and mixing, a polyurethane polymer solution was added to obtain an aqueous dispersion. The solvent methyl ethyl ketone was then removed under reduced pressure. The concentration was adjusted with water to prepare a solution containing 35% by mass of polyurethane resin (A-7) with an acid value of 23.1 mg KOH / g.
[0131] Polymerization of polyurethane resin A-8
[0132] 68.0 parts by weight of hydrogenated diphenylmethane diisocyanate, 19.8 parts by weight of dimethylolpropionic acid, 148.0 parts by weight of polycarbonate diol (derived from 1,6-hexanediol) with a number average molecular weight of 2000, and 110 parts by weight of methyl ethyl ketone as solvent were placed in a four-necked flask equipped with a stirrer, a serpentine condenser, a nitrogen inlet tube, a silica gel drying tube, and a thermometer. The resulting mixture was stirred at 75°C for 2 hours under a nitrogen atmosphere, and the predetermined amine equivalent was confirmed to have been reached. Subsequently, 6.6 parts by weight of 2-butanone oxime were added, and the reaction was stirred for another hour. After the temperature of the reaction solution was lowered to 40°C, 15.7 parts by weight of triethylamine were added to obtain a polyurethane polymer solution. Subsequently, 500 g of water was added to a reaction vessel equipped with a homogenizer capable of high-speed stirring, and the temperature was adjusted to 25°C. The resulting mixture was passed through a homogenizer for 2000 min... -1 While stirring, a polyurethane polymer solution was added to obtain an aqueous dispersion. 1.1 parts by weight of a 10% by weight aqueous solution of ethylenediamine was added while stirring. The solvent methyl ethyl ketone was then removed under reduced pressure. The concentration was adjusted with water to prepare a solution containing 35% by weight of polyurethane resin (A-8) with an acid value of 32.0 mg KOH / g.
[0133] Synthesis of crosslinking agent B-1
[0134] 59.5 parts by weight of hexamethylene diisocyanate, 10.7 parts by weight of neopentyl glycol, 11.0 parts by weight of dimethylolbutyric acid, and 20.0 parts by weight of N-methylpyrrolidone as solvent were placed in a flask equipped with a stirrer, thermometer, and reflux condenser. The resulting mixture was stirred at 80°C for 3 hours under a nitrogen atmosphere, and the predetermined amine equivalent was confirmed to have been reached. Subsequently, 29.9 parts by weight of 2-butanone oxime were added dropwise to the reaction solution, and the reaction mixture was maintained at 80°C for 1 hour under a nitrogen atmosphere. The reaction mixture was then subjected to infrared spectroscopy, and the isocyanate group absorption peak was confirmed to have disappeared. The temperature of the reaction mixture was then lowered to 40°C, and 7.9 parts by weight of triethylamine were added. After stirring for 1 hour, an appropriate amount of water was added to prepare a solution of end-capped isocyanate crosslinking agent (B-1) with a solid content of 40% by weight. The acid value of the solid component of the crosslinking agent (B-1) was 37.6 mg KOH / g.
[0135] Synthesis of crosslinking agent B-2
[0136] 66.6 parts by mass of a polyisocyanate compound with an isocyanurate structure (Duranate TPA, manufactured by Asahi Kasei Corporation) prepared using hexamethylene diisocyanate as a raw material and 17.5 parts by mass of N-methylpyrrolidone were placed in a flask equipped with a stirrer, thermometer, and reflux condenser, and 21.7 parts by mass of 3,5-dimethylpyrazole were added dropwise. The resulting mixture was maintained at 70°C for 1 hour under a nitrogen atmosphere. 9.0 parts by mass of dimethylolpropionic acid were added dropwise. After infrared spectroscopy of the reaction mixture and confirmation that the isocyanate group absorption peak had disappeared, 6.3 parts by mass of N,N-dimethylethanolamine were added. After stirring for 1 hour, an appropriate amount of water was added to prepare a solution of a 40% by mass end-capped isocyanate crosslinking agent (B-2). The acid value of the solid component of the crosslinking agent (B-2) was 41.2 mg KOH / g.
[0137] Synthesis of crosslinking agent B-3
[0138] 150.0 parts by weight of water and 250.0 parts by weight of methoxypropanol were placed in a flask equipped with a stirrer, thermometer, and reflux condenser. The resulting mixture was heated to 80°C under a nitrogen atmosphere. While maintaining the temperature in the flask at 80°C, a monomer mixture comprising 126.0 parts by weight of methyl methacrylate, 210.0 parts by weight of 2-isopropenyl-2-oxazoline, and 53.0 parts by weight of triethylamine methacrylate, and a polymerization initiator solution consisting of 18.0 parts by weight of 2,2'-azobis(2-amidinylpropane) dihydrochloride as a polymerization initiator and 170.0 parts by weight of water was added dropwise over 2 hours. After the addition, the reaction mixture was stirred at 80°C for 5 hours and then cooled to room temperature. An appropriate amount of water was added to prepare a solution of oxazoline crosslinking agent (B-3) with a solids content of 40% by weight. The solid component of the crosslinking agent (B-3) has an acid value of 39.8 mg KOH / g.
[0139] Preparation of crosslinking agent B-4
[0140] 65.0 parts by weight of a polyisocyanate compound with an isocyanurate structure prepared using adipate isocyanate as a raw material (Duranate TPA, manufactured by Asahi Kasei Corporation), 17.5 parts by weight of N-methylpyrrolidone, 29.2 parts by weight of 3,5-dimethylpyrazole, and 21.9 parts by weight of polyethylene glycol monomethyl ether with a number average molecular weight of 500 were placed in a flask equipped with a stirrer, thermometer, and reflux condenser. The resulting mixture was maintained at 70°C for 2 hours under a nitrogen atmosphere. Then, 4.0 parts by weight of trimethylolpropane were added dropwise. After infrared spectroscopy of the reaction mixture and confirmation that the isocyanate group absorption peak had disappeared, 280.0 parts by weight of water were added. An appropriate amount of water was added to prepare a solution of end-capped polyisocyanate crosslinking agent (B-4) with a solid content of 40% by weight. The acid value of the solid component of the crosslinking agent (B-4) was 0.0 mg KOH / g.
[0141] Synthesis of crosslinking agent B-5
[0142] 66.04 parts by weight of a polyisocyanate compound (Duranate TPA, manufactured by Asahi Kasei Corporation) with an isocyanurate structure prepared using hexamethylene diisocyanate as a raw material and 17.50 parts by weight of N-methylpyrrolidone were placed in a flask equipped with a stirrer, thermometer, and reflux condenser, and 25.19 parts by weight of 3,5-dimethylpyrazole were added dropwise. The resulting mixture was maintained at 70°C for 1 hour under a nitrogen atmosphere. Then, 5.27 parts by weight of dimethylolpropionic acid were added dropwise. After infrared spectroscopy of the reaction mixture and confirmation that the isocyanate group absorption peak had disappeared, 5.59 parts by weight of N,N-dimethylethanolamine and 132.5 parts by weight of water were added. An appropriate amount of water was added to prepare a solution of a 40% by weight end-capped polyisocyanate crosslinking agent (B-5). The acid value of the solid component of the crosslinking agent (B-5) was 22.8 mg KOH / g.
[0143] Synthesis of crosslinking agent B-6
[0144] 59.5 parts by mass of hexamethylene diisocyanate, 6.8 parts by mass of neopentyl glycol, 16.6 parts by mass of dimethylolbutyric acid, and 20.0 parts by mass of N-methylpyrrolidone as solvent were placed in a flask equipped with a stirrer, thermometer, and reflux condenser. The resulting mixture was stirred at 80°C for 3 hours under a nitrogen atmosphere, and the predetermined amine equivalent was confirmed to be reached. Subsequently, 30.3 parts by mass of 2-butanone oxime were added dropwise to the reaction mixture, and the reaction mixture was maintained at 80°C for 1 hour under a nitrogen atmosphere. The reaction mixture was then subjected to infrared spectroscopy, and the isocyanate group absorption peak was confirmed to have disappeared. The temperature of the reaction mixture was then lowered to 40°C, and 11.9 parts by mass of triethylamine were added. After stirring for 1 hour, an appropriate amount of water was added to prepare a solution of end-capped isocyanate crosslinking agent (B-6) with a solid content of 40% by mass. The acid value of the solid component of the crosslinking agent (B-6) was 55.4 mg KOH / g.
[0145] Preparation of polyester resin C-1
[0146] 194.2 parts by weight of dimethyl terephthalate, 184.5 parts by weight of dimethyl isophthalate, 14.8 parts by weight of sodium 5-sulfoisophthalate, 233.5 parts by weight of diethylene glycol, 136.6 parts by weight of ethylene glycol, and 0.2 parts by weight of tetrabutyl titanate were placed in a stainless steel autoclave equipped with a stirrer, thermometer, and partial reflux condenser. The transesterification reaction was carried out at 160–220 °C for 4 hours. Subsequently, the temperature was raised to 255 °C, and the pressure within the reaction system was gradually reduced. Then, the reaction was carried out under reduced pressure of 30 Pa for 1 hour and 30 minutes to obtain copolyester resin (C-1). The obtained polyester resin (C-1) was pale yellow and transparent. The specific viscosity of polyester resin (C-1) was determined to be 0.70 dl / g.
[0147] In addition, 15 parts by mass of polyester resin (C-1) and 15 parts by mass of ethylene glycol n-butyl ether were placed in a reactor equipped with a stirrer, thermometer, and reflux condenser. The resulting mixture was heated and stirred at 110°C to dissolve the resin. After the resin was completely dissolved, 70 parts by mass of water were gradually added to the polyester solution while stirring. After the addition, the resulting liquid was cooled to room temperature while stirring. An appropriate amount of water was added to prepare a solution of polyester resin (C-1) with a solid content of 30% by mass. The acid value of the solid component of polyester resin (C-1) was 0.9 mg KOH / g.
[0148] Preparation of polyester resin C-2
[0149] 194.2 parts by weight of dimethyl terephthalate, 194.2 parts by weight of dimethyl isophthalate, 233.5 parts by weight of diethylene glycol, 136.6 parts by weight of ethylene glycol, and 0.2 parts by weight of tetrabutyl titanate were placed in a stainless steel autoclave equipped with a stirrer, thermometer, and partial reflux condenser. The transesterification reaction was carried out at 160–220 °C for 4 hours. Subsequently, the temperature was raised to 255 °C, and the pressure within the reaction system was gradually reduced. The reaction was then carried out under reduced pressure of 30 Pa for 1 hour. Meanwhile, nitrogen gas was introduced into the system to release the pressure while the system was cooled to 200 °C. 28.0 parts by weight of trimellitic anhydride were added to the system while stirring, and the addition reaction was carried out for another 2 hours to obtain polyester resin (C-2). The obtained polyester resin (C-2) was pale yellow and transparent. The specific viscosity of polyester resin (C-2) was determined to be 0.35 dl / g.
[0150] In addition, 15 parts by mass of polyester resin (C-2) and 15 parts by mass of tetrahydrofuran were placed in a reactor equipped with a stirrer, thermometer, and reflux condenser. The resulting mixture was heated at 70°C and stirred to dissolve the resin. After the resin was completely dissolved, 31 parts by mass of triethylamine and 70 parts by mass of water were gradually added to the polyester solution while stirring. After the addition, the pressure in the reaction system was reduced to remove the tetrahydrofuran, and the resulting mixture was cooled to room temperature. An appropriate amount of water was added to prepare a solution of polyester resin (C-2) with a solids content of 30% by mass. The acid value of the solids component of polyester resin (C-2) was 37.4 mg KOH / g.
[0151] Preparation of acrylic resin D-1
[0152] Forty parts of propylene glycol monomethyl ether were placed in a flask equipped with a stirrer, thermometer, and reflux condenser. While heating the flask to maintain the temperature at 100°C, a mixture of 60.0 parts by weight of n-butyl acrylate, 42.0 parts by weight of methyl methacrylate, 2.9 parts by weight of 2-hydroxyethyl methacrylate, 5.7 parts by weight of acrylic acid, and 5 parts by weight of azobisisobutyronitrile was added dropwise over 3 hours. After the addition, the resulting mixture was aged at the same temperature for 2 hours. Then, the temperature of the reaction mixture was lowered to 40°C, and 8.4 parts by weight of triethylamine and 165 parts by weight of water were added while stirring. After continuing stirring for another hour, an appropriate amount of water was added to prepare a solution of acrylic resin (D-1) with a solid content of 35% by weight. The acid value of the solid component of acrylic resin (D-1) was 40.1 mg KOH / g.
[0153] Preparation of polyester resin E-1 for substrate
[0154] Preparation of antimony trioxide solution
[0155] Antimony trioxide (manufactured by Sigma-Aldrich Japan) and ethylene glycol were placed in a flask and stirred at 150°C for 4 hours to dissolve the antimony trioxide. The resulting solution was then cooled to room temperature to prepare a 20 g / L solution of antimony trioxide in ethylene glycol.
[0156] Polymerization of polyester resin E-1 for substrate
[0157] High-purity terephthalic acid and ethylene glycol were placed in a 2-liter stainless steel autoclave equipped with a stirrer at a molar ratio of 1:2. Triethylamine was added at a rate of 0.3 mol% relative to the acid content. Esterification was carried out simultaneously with distillation of water from the reaction system at 250°C and 0.25 MPa to obtain a mixture of bis(2-hydroxyethyl) terephthalate and oligomers with an esterification rate of approximately 95% (hereinafter referred to as the BHET mixture). Subsequently, a solution of antimony trioxide in ethylene glycol, acting as a polymerization catalyst, was added to the BHET mixture at a rate of 0.04 mol% (based on antimony atoms) relative to the acid content of the polyester. The resulting mixture was then stirred for 10 minutes at atmospheric pressure and 250°C under a nitrogen atmosphere. Subsequently, while heating to 280°C over 60 minutes, the pressure of the reaction system was gradually reduced to 13.3 Pa (0.1 Torr), and a polycondensation reaction was further carried out at 280°C and 13.3 Pa for 68 minutes to obtain a polyester resin (E-1) with an intrinsic viscosity (IV) (solvent: phenol / tetrachloroethane = 60 / 40) of 0.61 dl / g and which is substantially free of particles.
[0158] Preparation of polyester resin E-2 for substrate
[0159] Preparation example of aluminum compound solution
[0160] A 20 g / L aqueous solution of basic aluminum acetate (aluminum diacetate; manufactured by Sigma-Aldrich Japan) and an equal volume (volume ratio) of ethylene glycol were placed in a flask and stirred at room temperature for 6 hours. Then, the reaction system was stirred at 70–90 °C and under reduced pressure (133 Pa) for several hours, and water was distilled off to prepare a 20 g / L solution of aluminum compound in ethylene glycol.
[0161] Example of preparation of phosphorus compound solution
[0162] Diethyl 3,5-di-tert-butyl-4-hydroxybenzylphosphonate (Irganox 1222, manufactured by BASF), which is a phosphorus compound, was placed in a flask and heated with stirring at a liquid temperature of 160°C for 25 hours under a nitrogen atmosphere to prepare a 50 g / L solution of the phosphorus compound in ethylene glycol.
[0163] Preparation of a mixture of aluminum compound solution and phosphorus compound solution
[0164] The aluminum compound solution in ethylene glycol obtained in the "Preparation Example of Aluminum Compound Solution" section above and the phosphorus compound solution in ethylene glycol obtained in the "Preparation Example of Phosphorus Compound Solution" section above were placed in a flask and mixed at room temperature to achieve a molar ratio of aluminum atoms to phosphorus atoms of 1:2. The mixture was stirred for 1 day to prepare a catalyst solution.
[0165] Polymerization of polyester resin E-2 for substrate
[0166] Except that a mixture of aluminum compound solution and phosphorus compound solution was used instead of antimony trioxide solution as the polycondensation catalyst, and the mixture was added in the same manner as in polyester resin (E-1) with aluminum and phosphorus content added in amounts of 0.014 mol% and 0.028 mol% respectively relative to the acid content of the polyester; the polymerization time was changed to 68 minutes to obtain polyester resin (E-2) with an intrinsic viscosity (IV) of 0.61 dl / g and substantially free of particles.
[0167] Example 1
[0168] (1) Preparation of coating solution
[0169] The following coating components were mixed in a mixed solvent of water and isopropanol (mass ratio: 80 / 20) to prepare a coating solution with a mass ratio of polyurethane resin solution (A-1) / crosslinking agent (B-1) solution of 70 / 30 based on solid content.
[0170]
[0171] (2) Preparation of laminated polyester film
[0172] As a membrane material polymer, polyester resin (E-1) pellets were dried at 135°C for 6 hours under reduced pressure of 133 Pa. The dried pellets were then fed into an extruder and melt-extruded into sheets at approximately 280°C. The resulting product was then rapidly cooled, bonded, and cured on a rotating cooling metal roller with its surface temperature maintained at 20°C, thereby obtaining unstretched PET sheets.
[0173] Unstretched PET sheets are heated to 100°C using a set of heated rollers and an infrared heater, and then stretched longitudinally by 3.5 times using rollers with different circumferential speeds, thereby obtaining a uniaxially stretched PET film.
[0174] Subsequently, the coating liquid was applied to achieve a final (after biaxial stretching) coating weight of 0.13 g / m² after drying. 2An appropriate amount of coating solution was applied to one surface of a PET film. After the coating solution dried, the film was stretched 4.0 times its original length in the width direction at 110°C, and then heated at 230°C for 5 seconds while maintaining the width direction of the film. Furthermore, the film was subjected to a 3% relaxation treatment in the width direction, thereby obtaining a laminated polyester film with a thickness of 100 μm. Table 1 shows the evaluation results.
[0175] Example 2
[0176] Except for changing the polyurethane resin to polyurethane resin (A-2) and changing the ratio of polyurethane resin to crosslinking agent to 60 / 40 (mass ratio), the laminated polyester film was obtained in the same manner as in Example 1.
[0177] Example 3
[0178] Except for changing the polyurethane resin to polyurethane resin (A-3) and changing the ratio of polyurethane resin to crosslinking agent to 50 / 50 (mass ratio), the laminated polyester film was obtained in the same manner as in Example 1.
[0179] Example 4
[0180] Except for changing the crosslinking agent to crosslinking agent (B-2) and changing the ratio of polyurethane resin to crosslinking agent to 60 / 40 (mass ratio), the laminated polyester film was obtained in the same manner as in Example 1.
[0181] Example 5
[0182] Except for changing the crosslinking agent to crosslinking agent (B-3) and changing the ratio of polyurethane resin to crosslinking agent to 60 / 40 (mass ratio), the laminated polyester film was obtained in the same manner as in Example 1.
[0183] Example 6
[0184] In addition to using a crosslinking agent (B-4) in addition to polyurethane resin (A-1) and crosslinking agent (B-1), and changing the component ratio to (A-1) / (B-1) / (B-4) = 55 / 35 / 10 (mass ratio), a laminated polyester film was obtained in the same manner as in Example 1.
[0185] Example 7
[0186] In addition to using polyester resin (C-1) in addition to polyurethane resin (A-1) and crosslinking agent (B-1), and changing the component ratio to (A-1) / (B-1) / (C-1) = 36 / 24 / 40 (mass ratio), a laminated polyester film was obtained in the same manner as in Example 1.
[0187] Example 8
[0188] In addition to using polyester resin (C-1) in addition to polyurethane resin (A-1) and crosslinking agent (B-1), and changing the component ratio to (A-1) / (B-1) / (C-1) = 24 / 16 / 60 (mass ratio), a laminated polyester film was obtained in the same manner as in Example 1.
[0189] Example 9
[0190] Except that the polyester resin pellets (E-2) were used as the membrane material polymer, the laminated polyester film was obtained in the same manner as in Example 1.
[0191] Example 10
[0192] Except for changing the polyurethane resin to polyurethane resin (A-8), the laminated polyester film was obtained in the same manner as in Example 1.
[0193] Comparative Example 1
[0194] The laminated polyester film was obtained in the same manner as in Example 1, except that only polyurethane resin (A-1) was used without crosslinking agent (B-1).
[0195] Comparative Example 2
[0196] The laminated polyester film was obtained in the same manner as in Example 1, except that only the crosslinking agent (B-1) was used and the polyurethane resin (A-1) was not used.
[0197] Comparative Example 3
[0198] Except for changing the polyurethane resin to polyurethane resin (A-4), the laminated polyester film was obtained in the same manner as in Example 1.
[0199] Comparative Example 4
[0200] Except for changing the polyurethane resin to polyurethane resin (A-5) and changing the ratio of polyurethane resin to crosslinking agent to 60 / 40 (mass ratio), the laminated polyester film was obtained in the same manner as in Example 1.
[0201] Comparative Example 5
[0202] Except for changing the polyurethane resin to polyurethane resin (A-6) and changing the ratio of polyurethane resin to crosslinking agent to 50 / 50 (mass ratio), the laminated polyester film was obtained in the same manner as in Example 1.
[0203] Comparative Example 6
[0204] Except for changing the polyurethane resin to polyurethane resin (A-7) and the crosslinking agent to crosslinking agent (B-5), the laminated polyester film was obtained in the same manner as in Example 1.
[0205] Comparative Example 7
[0206] Except for changing the crosslinking agent to crosslinking agent (B-5) and changing the ratio of polyurethane resin to crosslinking agent to 75 / 25 (mass ratio), the laminated polyester film was obtained in the same manner as in Example 1.
[0207] Comparative Example 8
[0208] Except for changing the crosslinking agent to crosslinking agent (B-6), the laminated polyester film was obtained in the same manner as in Example 1.
[0209] Comparative Example 9
[0210] The laminated polyester film was obtained in the same manner as in Example 1, except that polyurethane resin (C-2) was used instead of polyurethane resin (A-1).
[0211] Comparative Example 10
[0212] The laminated polyester film was obtained in the same manner as in Example 1, except that an acrylic resin (D-1) was used instead of a polyurethane resin (A-1).
[0213] Table 1 summarizes the evaluation results of the embodiments and comparative examples.
[0214] As shown in Table 1, the laminated polyester films obtained in the examples are satisfactory in terms of haze, tack resistance, adhesion to UV-curable inks, adhesion to hard coatings, and resistance to damp heat. In contrast, the laminated polyester films obtained in Comparative Examples 1 to 10 are unsatisfactory in at least one aspect of the above evaluation items.
[0215]
[0216] Industrial availability
[0217] According to the present invention, laminated polyester films suitable for use in all fields such as optics, packaging and labeling applications can be provided.
Claims
1. A laminated polyester film, wherein, The polyester film has a coating layer on at least one surface. The coating layer comprises a composition containing: a polyurethane resin having carboxyl groups and an acid value of 30-45 mgKOH / g, a crosslinking agent having carboxyl groups and an acid value of 30-45 mgKOH / g, and a polyester resin containing dicarboxylic acid and a branched diol or a diol having one or more ether bonds as constituent components. The crosslinking agent with a carboxyl group is an oxazoline compound or an isocyanate compound with a carboxyl group in the molecule.
2. The laminated polyester film according to claim 1, wherein Crosslinking agents with carboxyl groups are isocyanate compounds that have carboxyl groups in their molecules.
3. The laminated polyester film according to claim 2, wherein Isocyanate compounds containing a carboxyl group in the molecule are end-capped isocyanate compounds containing a carboxyl group in the molecule.
4. The laminated polyester film according to claim 1, wherein A polyurethane resin having a carboxyl group is a polyurethane resin synthesized from at least a carboxyl-containing polyol component and a polyisocyanate component, and a chain extender used as needed.
5. The laminated polyester film according to claim 4, wherein The carboxyl-containing polyol component is selected from at least one of the following groups: carboxyl-containing polyalkylene glycols, carboxyl-containing acrylic polyols, carboxyl-containing polyolefin polyols, carboxyl-containing polyester polyols, 2,2-dimethylolpropionic acid, 2,2-dimethylolbutyric acid, and 2,2-dimethylolvalerate.
6. The laminated polyester film according to claim 4, wherein The polyisocyanate component is selected from at least one of the group consisting of xylene diisocyanate, alicyclic diisocyanate and aliphatic diisocyanate.
7. The laminated polyester film according to claim 1, wherein The weight ratio of the carboxyl-containing polyurethane resin to the carboxyl-containing crosslinking agent in the composition is 90 / 10 to 10 / 90.
8. The laminated polyester film according to claim 1, wherein The thickness of the coating layer ranges from 0.001 to 2.00 μm.
9. The laminated polyester film according to claim 1, wherein The haze of the laminated polyester film is below 2.5%.
10. The laminated polyester film according to claim 1, wherein A UV-curable resin is present on the coating layer of the laminated polyester film.
11. A method for manufacturing a laminated polyester film having a coating layer and a polyester film, comprising the following steps: A composition is coated on at least one side of a polyester film and heat-treated to form a coating layer. The composition contains a polyurethane resin having carboxyl groups and an acid value of 30-45 mgKOH / g, a crosslinking agent having carboxyl groups and an acid value of 30-45 mgKOH / g, and a polyester resin containing dicarboxylic acid and a branched diol or a diol having one or more ether bonds as constituent components. The crosslinking agent with a carboxyl group is an oxazoline compound or an isocyanate compound with a carboxyl group in the molecule.
Citation Information
Patent Citations
Easily adhesive film
JP2009220376A
Non-water-based for plastic film provided with active energy line curing film and plastic film provided with active energy line curing film
CN102408823A
Water-based coating substrate treatment agent which serves as primer, surface-treated metal material, and precoated metal material
JP2010065211A