Crystalline silicon films and their preparation methods, solar cells and their preparation methods

By introducing a first polycrystalline silicon portion with suitable crystallinity and hydrogen content into the crystalline silicon film, and using infrared heating and laser processing, the complex problem of wet etching caused by poor polycrystalline silicon film quality was solved, and efficient production of photovoltaic devices was achieved.

CN117558783BActive Publication Date: 2026-11-10LONGI SOLAR TECHNOLOGY (TAIZHOU) CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202310872152.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-07-14
Publication Date
2026-11-10
Estimated Expiration
2043-07-14

AI Technical Summary

Technical Problem

The existing polycrystalline silicon film is of poor quality, which makes the wet etching process complex and the process relatively complicated.

Method used

A crystalline silicon film is provided, comprising a first polycrystalline silicon portion extending through its thickness direction, having a crystallinity of 50% to 60%, a hydrogen content of 1% to 20%, and a porosity of 0.1% to 10%, formed by infrared heating and laser processing, simplifying the wet etching process.

Benefits of technology

It improves the photoelectric conversion efficiency of photovoltaic devices, simplifies the wet etching process, reduces the steps of setting and removing mask layers, and improves production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117558783B_ABST
    Figure CN117558783B_ABST
Patent Text Reader

Abstract

This invention provides a crystalline silicon film and its preparation method, and a solar cell and its preparation method, relating to the field of photovoltaic technology. The crystalline silicon film includes: at least one first polycrystalline silicon portion; the crystallinity of the first polycrystalline silicon portion is 50% to 60%; the hydrogen content in the first polycrystalline silicon portion is 1% to 20%; and the porosity of the first polycrystalline silicon portion is 0.1% to 10%. The first polycrystalline silicon portion has suitable crystallinity, suitable hydrogen content, and suitable porosity, resulting in a superior film quality, which is beneficial for improving the photoelectric conversion efficiency of photovoltaic devices. Furthermore, during wet etching, the superior quality first polycrystalline silicon portion experiences very slow etching rates in both alkaline and acidic wet etching agents, and the etching effect is negligible. Therefore, a mask layer is not required on the first polycrystalline silicon portion, reducing steps, simplifying the wet etching process, and improving production efficiency.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of photovoltaic technology, and in particular to crystalline silicon films and their preparation methods, and solar cells and their preparation methods. Background Technology

[0002] Polycrystalline silicon is widely used in the photovoltaic industry, and the quality of the polycrystalline silicon film layer plays an important role in the photoelectric conversion efficiency of photovoltaic devices.

[0003] However, the existing polysilicon film quality is poor, which makes the wet etching process more complicated. Summary of the Invention

[0004] This invention provides a crystalline silicon film layer and its preparation method, as well as a solar cell and its preparation method, aiming to solve the problem of poor film quality in existing polycrystalline silicon films, which leads to complex processes during wet etching.

[0005] In a first aspect, the present invention provides a crystalline silicon film layer, the crystalline silicon film layer comprising: at least one first polycrystalline silicon portion; the first polycrystalline silicon portion extending through the crystalline silicon film layer in the thickness direction; The crystallinity of the first polycrystalline silicon portion is 50% to 60%; The hydrogen content in the first polycrystalline silicon portion is 1% to 20%; The porosity of the first polycrystalline silicon portion is 0.1% to 10%.

[0006] In this embodiment of the invention, the first polycrystalline silicon portion extends through the crystalline silicon film layer along its thickness direction. The first polycrystalline silicon portion has suitable crystallinity, hydrogen content, and porosity, resulting in superior film quality, which is beneficial for improving the photoelectric conversion efficiency of photovoltaic devices. Furthermore, during wet etching, the superior quality first polycrystalline silicon portion exhibits very slow etching rates in both alkaline and acidic wet etching agents. The etching effect of these agents is negligible, thus eliminating the need for a mask layer on the first polycrystalline silicon portion. This reduces the steps involved in setting and removing the mask layer after wet etching, simplifying the wet etching process and improving production efficiency.

[0007] Optionally, the first polysilicon portion is a doped polysilicon portion, and the doping concentration of the doped first polysilicon portion is 5 × 10⁻⁶. 18 cm -3 Up to 1×10 20 cm -3 .

[0008] Optionally, the thickness variation of the crystalline silicon film is less than 5%.

[0009] Optionally, the crystalline silicon film layer further includes: at least one amorphous silicon portion; the amorphous silicon portion extends through the crystalline silicon film layer from its thickness direction; in the crystalline silicon film layer, the first polycrystalline silicon portion and the amorphous silicon portion are alternately distributed; the crystallinity of the amorphous silicon portion is lower than that of the first polycrystalline silicon portion, and the hydrogen content and porosity of the amorphous silicon portion are both greater than those of the first polycrystalline silicon portion.

[0010] A second aspect of the present invention provides a method for preparing any of the aforementioned crystalline silicon films, comprising: Provides amorphous silicon film; The amorphous silicon film is heated with infrared light until the temperature of the amorphous silicon film reaches a preset temperature. At least a portion of the amorphous silicon film is hydrogenated and crystallized using a laser. The portion affected by the laser forms a first polycrystalline silicon portion. The preset temperature is 5%-30% of the laser temperature. The infrared heating and laser action are performed simultaneously, or the infrared heating is performed first and then the laser action is performed.

[0011] Optionally, the power of the laser is from 20W to 200W; The preset temperature is 100℃ to 300℃.

[0012] Optionally, the laser spot shape is triangular.

[0013] Optionally, the provision of the amorphous silicon film layer includes: Provide substrate; On the first surface of the substrate, an amorphous silicon film with a crystallinity of 5%-40% and a porosity of 0.1% to 20% is formed by LPCVD. Alternatively, an amorphous silicon film with a crystallinity of 5%-30% and a porosity of 0.1% to 20% can be formed on the substrate using PECVD. In the PECVD method, the process parameters include at least one of the following five types: The RF power supply switching ratio is 1 / 5-4 / 5; The number of discharge cycles is 20,000 to 50,000. The discharge gas is a mixture of hydrogen, nitrogen, and argon; in the mixture, the volume concentration of hydrogen is 5%-70%, and the volume concentration of argon is 10%-80%. The power of the RF power supply is 5000W-15000W; The process temperature is 300°C-500°C.

[0014] Optionally, the provided substrate includes: The first surface of the substrate is polished to obtain a first surface with a reflectivity of 30%-50%.

[0015] A third aspect of the present invention provides a solar cell comprising: A silicon substrate, a tunneling oxide layer on the silicon substrate, and a first doped film layer on the tunneling oxide layer; the first doped film layer includes: at least one second polysilicon portion; the second polysilicon portion extends through the first doped film layer from the thickness direction of the first doped film layer; The crystallinity of the second polycrystalline silicon portion is greater than or equal to 60%; The hydrogen content in the second polycrystalline silicon portion is 1% to 20%; The porosity of the second polycrystalline silicon portion is 0.1% to 10%. Optionally, the first doped film layer is entirely composed of the second polycrystalline silicon portion; The surface of the silicon substrate away from the crystalline silicon film layer has a textured surface.

[0016] Optionally, the thickness difference of the first doped film layer is less than 5%.

[0017] A fourth aspect of the present invention provides a back-contact solar cell, comprising: Silicon substrate; The projection falls on a first region and a second region on the silicon substrate; the first region and the second region are alternately distributed; the first region includes: a tunneling oxide layer and a first transport layer stacked together; the crystallinity of the first transport layer is greater than or equal to 60%; the hydrogen content of the first transport layer is 1% to 20%; the porosity of the first transport layer is 0.1% to 10%; the second region includes a second transport layer; the first transport layer and the second transport layer have different doping types.

[0018] Optionally, the thickness difference of the first transmission layer is less than 5%.

[0019] A fifth aspect of the present invention provides a method for fabricating the aforementioned back-contact solar cell, comprising: A conductive substrate is provided; the conductive substrate comprises: a silicon substrate, a tunneling oxide layer and a crystalline silicon film layer sequentially stacked on the silicon substrate; the crystalline silicon film layer is any of the aforementioned crystalline silicon film layers, or the crystalline silicon film layer is prepared by any of the aforementioned methods for preparing crystalline silicon film layers; the crystalline silicon film layer comprises: at least one first polycrystalline silicon portion and at least one amorphous silicon portion; the amorphous silicon portion extends through the crystalline silicon film layer from its thickness direction; in the crystalline silicon film layer, the first polycrystalline silicon portion and the amorphous silicon portion are alternately distributed; In the absence of a mask layer covering each of the first polysilicon portions, the conductive substrate is wet-etched, each of the first polysilicon portions is retained in the wet etching, each of the amorphous silicon portions is removed in the wet etching, and the tunneling oxide layer or the second region of the silicon substrate is exposed. A second transport layer is formed on the exposed second region. Attached Figure Description

[0020] To more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings used in the description of the embodiments of the present invention will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0021] Figure 1 A schematic diagram of a planar structure of a crystalline silicon film layer is shown in an embodiment of the present invention; Figure 2 A schematic diagram of a planar structure of another crystalline silicon film layer in an embodiment of the present invention is shown; Figure 3 A partially enlarged schematic diagram of a first polysilicon portion according to an embodiment of the present invention is shown; Figure 4 A partially enlarged schematic diagram of a polycrystalline silicon film layer in the prior art is shown; Figure 5 A schematic diagram of crystallization and hydrogenation in an embodiment of the present invention is shown; Figure 6 A schematic diagram of crystallization and hydrogenation in the prior art is shown; Figure 7 A schematic diagram of a laser according to an embodiment of the present invention is shown; Figure 8 A schematic diagram of a laser in the prior art is shown; Figure 9 The diagram shows the hydrogen content and crystallinity distribution of the first polycrystalline silicon portion in various embodiments of the present invention.

[0022] Explanation of the attached drawing numbers: 1-Crystal silicon film, 11-First polycrystalline silicon portion, 12-Amorphous silicon portion, 111-Pore, 2-Amorphous silicon film, 31-Infrared light, 32-Laser. Detailed Implementation

[0023] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0024] Figure 1 A schematic diagram of a planar structure of a crystalline silicon film layer is shown in an embodiment of the present invention. Figure 2 A schematic diagram of another planar structure of a crystalline silicon film layer according to an embodiment of the present invention is shown. The present invention provides a crystalline silicon film layer 1, which includes at least one first polycrystalline silicon portion 11. The first polycrystalline silicon portion 11 extends through the crystalline silicon film layer 1 from its thickness direction. The number of first polycrystalline silicon portions in the crystalline silicon film layer 1 is not limited. The crystalline silicon film layer 1 may be composed entirely of the first polycrystalline silicon portions 11, or it may be composed of the first polycrystalline silicon portions 11 and amorphous silicon portions 12. In this embodiment of the present invention, no specific limitation is made. For example, refer to... Figure 1 As shown, the crystalline silicon film layer 1 is entirely composed of a first polycrystalline silicon portion 11, or it can be considered that the crystalline silicon film layer 1 is composed of one first polycrystalline silicon portion 11, which extends through the crystalline silicon film layer 1 from the thickness direction. Figure 1 , Figure 2 This is a schematic diagram of the planar structure of a crystalline silicon film. Therefore, Figure 1 , Figure 2 The thickness direction of the intermediate-crystalline silicon film 1 is perpendicular to the paper surface. For example, refer to... Figure 2 The crystalline silicon film layer 1 includes eight first polycrystalline silicon portions 11 and seven amorphous silicon portions 12. Each first polycrystalline silicon portion 11 extends through the crystalline silicon film layer 1 along its thickness direction, and each amorphous silicon portion 12 extends through the crystalline silicon film layer 1 along its thickness direction. The first polycrystalline silicon portion 11 extending through the crystalline silicon film layer 1 along its thickness direction can be defined as having at least one three-dimensional structure, which includes at least one point and at least one surface, located on two opposite surfaces along the thickness direction of the crystalline silicon film layer 1.

[0025] Figure 3 A partially enlarged schematic diagram of a first polysilicon portion according to an embodiment of the present invention is shown. Figure 4 A partially enlarged schematic diagram of a polycrystalline silicon film in the prior art is shown. (Refer to...) Figure 3 , Figure 4Compared with the prior art, in the present invention, the first polycrystalline silicon portion 11 has fewer pores 111 and smaller pore volume. Therefore, in the present invention, the first polycrystalline silicon portion 11 has lower porosity and is more compact.

[0026] More specifically, the crystallinity of the first polycrystalline silicon portion 11 is 50% to 60%, the hydrogen content in the first polycrystalline silicon portion 11 is 1% to 20%, and the porosity of the first polycrystalline silicon portion 11 is 0.1% to 10%. Since the crystallinity, hydrogen content, and porosity of the first polycrystalline silicon portion 11 are all within the aforementioned ranges, the film quality of the first polycrystalline silicon portion 11 is superior, which is beneficial for improving the photoelectric conversion efficiency of photovoltaic devices. Furthermore, during wet etching, the superior quality of the first polycrystalline silicon portion 11 exhibits very slow etching rates in both alkaline and acidic wet etching agents. The etching effect of alkaline and acidic wet etching agents on it is negligible. Therefore, it is unnecessary to place a mask layer on the first polycrystalline silicon portion 11, reducing the steps of placing mask layers on each first polycrystalline silicon portion 11 and the steps of removing the mask layer after wet etching, simplifying the wet etching process and improving production efficiency.

[0027] For example, refer to Figure 1 The crystalline silicon film layer 1 shown is entirely composed of a first polycrystalline silicon portion 11. The photovoltaic device includes the crystalline silicon film layer 1 and component A stacked together. During the texturing process on the surface of component A away from the crystalline silicon film layer 1, since the crystallinity, hydrogen content and porosity of the first polycrystalline silicon portion 11 are within the aforementioned ranges, the film quality of the first polycrystalline silicon portion 11 is superior. During the texturing process, the etching rate of the superior quality first polycrystalline silicon portion 11 in the texturing solution is very slow, and the etching of it by the texturing solution is negligible. Therefore, it is not necessary to set a mask layer on the crystalline silicon film layer 1, reducing the steps of setting a mask layer on the crystalline silicon film layer 1 and the steps of removing the mask layer after wet etching, simplifying the texturing process and improving production efficiency.

[0028] For example, refer to Figure 2The crystalline silicon film layer 1 shown is composed of 8 first polycrystalline silicon portions 11 and 7 amorphous silicon portions 12. Each first polycrystalline silicon portion 11 penetrates the crystalline silicon film layer 1 from the thickness direction of the crystalline silicon film layer 1, and each amorphous silicon portion 12 penetrates the crystalline silicon film layer 1 from the thickness direction of the crystalline silicon film layer 1. During the patterning process of the crystalline silicon film 1, since the crystallinity, hydrogen content, and porosity of the first polycrystalline silicon portion 11 are all within the aforementioned ranges, the film quality of the first polycrystalline silicon portion 11 is superior. During the patterning process, the etching rate of the superior quality first polycrystalline silicon portion 11 in the etching solution is very slow, and the etching effect of the etching solution on it is negligible. However, compared to the first polycrystalline silicon portion 11, the film quality of the amorphous silicon portion 12 is poor. In the etching solution, the seven amorphous silicon portions 12 will be completely etched, leaving only eight first polycrystalline silicon portions 11, thus achieving patterning. Therefore, it is not necessary to set a mask layer on each first polycrystalline silicon portion 11, reducing the steps of setting a mask layer on each first polycrystalline silicon portion 11 and the steps of removing the mask layer after patterning, simplifying the patterning process and improving production efficiency.

[0029] For example, the crystallinity of the first polycrystalline silicon portion 11 can be 50%, or 50.2%, or 52%, or 52.9%, or 53.7%, or 54.9%, or 55%, or 55.3%, or 57%, or 59%, or 60%, the hydrogen content in the first polycrystalline silicon portion 11 can be 1%, or 2.3%, or 4%, or 7%, or 9.7%, or 10.4%, or 10.5%, or 10.9%, or 12%, or 15%, or 20%, and the porosity of the first polycrystalline silicon portion 11 can be 0.1%, or 1%, or 3%, or 4.7%, or 5.05%, or 6%, or 7.5%, or 8%, or 9%, or 9.5%, or 10%.

[0030] It should be noted that the hydrogen content in a first polycrystalline silicon portion 11 can refer to the proportion of the total number of hydrogen bonds in the first polycrystalline silicon portion 11 to the total number of bonds in the first polycrystalline silicon portion 11. The crystallinity in a first polycrystalline silicon portion 11 can refer to the ratio of crystals in the first polycrystalline silicon portion 11. The porosity in a first polycrystalline silicon portion 11 can refer to the percentage of the total volume of pores in the first polycrystalline silicon portion 11 to the total volume of the first polycrystalline silicon portion 11. For crystallinity and porosity, a predetermined number of points can be selected in the first polycrystalline silicon portion 11, located at different positions within the first polycrystalline silicon portion 11. The crystallinity and porosity at each point are measured, and then the arithmetic mean of the crystallinity at all points is calculated to obtain the crystallinity of the first polycrystalline silicon portion 11. Similarly, the arithmetic mean of the porosity at all points is calculated to obtain the porosity of the first polycrystalline silicon portion 11. For crystallinity and porosity, the number of points selected can be the same or different, and each point can be representative of the first polycrystalline silicon portion 11. For example, if the first polycrystalline silicon portion 11 is rectangular, five points can be selected for both crystallinity and porosity, located at the four vertices of the rectangle and its geometric center. Alternatively, 30 points can be selected for both crystallinity and porosity, evenly distributed throughout the first polycrystalline silicon portion 11.

[0031] Optionally, the first polysilicon portion 11 is a doped polysilicon portion, and the doping concentration of the doped polysilicon portion is 5 × 10⁻⁶. 18 cm -3 Up to 1×10 20 cm -3 Specifically, the first polysilicon portion 11 has a superior film quality, thus enabling it to achieve a wider range of doping concentrations and making it suitable for a wider range of applications. For example, if the first polysilicon portion 11 is a doped polysilicon portion, the doping concentration of the doped polysilicon portion can be 5 × 10⁻⁶. 18 cm -3 or 8×10 18 cm -3 or 9.3×10 18 cm -3 or 1×10 19 cm -3 or 4×10 19 cm -3 or 5×10 19 cm -3 or 5.25×10 19 cm -3 or 6×10 19 cm -3 or 8×10 19 cm-3 or 9×10 19 cm -3 or 1×10 20 cm -3 .

[0032] It should be noted that the first polysilicon portion 11 can be N-type doped or P-type doped, and there is no limitation on this.

[0033] Optionally, the thickness variation of the crystalline silicon film 1 is less than 5%. The thickness variation of the crystalline silicon film 1 is calculated as follows: the first difference obtained by subtracting the average of the multiple thicknesses from the maximum thickness at multiple locations within the crystalline silicon film 1, divided by the average of the multiple thicknesses, yields a first quotient. Alternatively, the thickness variation of the crystalline silicon film 1 is calculated as follows: the second difference obtained by subtracting the minimum thickness from the average of the multiple thicknesses at multiple locations within the crystalline silicon film 1, divided by the average of the multiple thicknesses, yields a second quotient. A thickness variation of less than 5% in the crystalline silicon film 1 indicates good thickness uniformity across the crystalline silicon film 1. During etching, the thickest part of the crystalline silicon film 1 will not be excessively thick, and the etching time will not be excessively long, thus saving etching time and improving etching efficiency. Each first polycrystalline silicon portion is part of the crystalline silicon film layer, and each first polycrystalline silicon portion penetrates the crystalline silicon film layer from the thickness direction. Therefore, the thickness difference of each first polycrystalline silicon portion is basically equal to the thickness difference of the crystalline silicon film layer. The thickness difference of each first polycrystalline silicon portion is less than 5%, indicating that the thickness uniformity of each first polycrystalline silicon portion is good. During the etching process of each first polycrystalline silicon portion, the thickest part of each first polycrystalline silicon portion will not be too thick, and the etching time will not be too long. This can also save etching time and improve etching efficiency. When the crystalline silicon film layer includes amorphous silicon portions, each amorphous silicon portion is a part of the crystalline silicon film layer, and each amorphous silicon portion penetrates the crystalline silicon film layer from the thickness direction. Therefore, the thickness difference of each amorphous silicon portion is basically equal to the thickness difference of the crystalline silicon film layer, and the thickness difference of each amorphous silicon portion is less than 5%, indicating that the thickness uniformity of each amorphous silicon portion is good. During the etching process of each amorphous silicon portion, the thickest part of each amorphous silicon portion will not be too thick, and the etching time will not be too long, which can also save etching time and improve etching efficiency.

[0034] Optional, refer to Figure 2The crystalline silicon film layer 1 further includes at least one amorphous silicon portion 12, which extends through the crystalline silicon film layer 1 from its thickness direction. The first polycrystalline silicon portion 11 and the amorphous silicon portion 12 are alternately distributed in the crystalline silicon film layer 1. The crystallinity of the amorphous silicon portion 12 is lower than that of the first polycrystalline silicon portion 11. The hydrogen content and porosity of the amorphous silicon portion 12 are both greater than those of the first polycrystalline silicon portion 11. That is, compared to the first polycrystalline silicon portion 11, the film quality of the amorphous silicon portion 12 is relatively poor. When it is necessary to remove the amorphous silicon portion 12 from the crystalline silicon film layer 1 while retaining the first polycrystalline silicon portion 11, on the one hand, the relatively poor film quality of the amorphous silicon portion 12 allows for faster removal and reduces process time; on the other hand, the first polycrystalline silicon portion 11 has a higher crystallinity than the amorphous silicon portion 12. The film layer has good quality. When it is necessary to remove the amorphous silicon portion 12 in the crystalline silicon film layer 1 while retaining the first polycrystalline silicon portion 11, the etching rate of the first polycrystalline silicon portion 11 in both alkaline and acidic wet etching agents is very slow. The etching effect of alkaline and acidic wet etching agents on it is negligible. Therefore, it is unnecessary to form a mask layer on each of the first polycrystalline silicon portions 11, reducing the steps of setting mask layers on each of the first polycrystalline silicon portions 11 and the steps of removing the mask layer after wet etching, simplifying the wet etching process and improving production efficiency. It should be noted that the hydrogen content in an amorphous silicon portion 12 can refer to the proportion of the total number of hydrogen bonds in the amorphous silicon portion 12 to the total number of bonds in the amorphous silicon portion 12. The crystallinity in an amorphous silicon portion 12 can refer to the ratio of crystals in the amorphous silicon portion 12. The porosity in an amorphous silicon portion 12 can refer to the percentage of the total volume of pores in the amorphous silicon portion 12 to the total volume of the amorphous silicon portion 12.

[0035] It should be noted that the specific amount by which the crystallinity of the amorphous silicon portion 12 is lower than that of the first polycrystalline silicon portion 11, and the specific amount by which the hydrogen content and porosity of the amorphous silicon portion 12 are greater than those of the first polycrystalline silicon portion 11, are not specifically limited. The methods for determining the hydrogen content, crystallinity, and porosity of the amorphous silicon portion 12 can refer to the methods used for determining the hydrogen content, crystallinity, and porosity of the first polycrystalline silicon portion 11 described above; to avoid repetition, they will not be repeated here.

[0036] The present invention also provides a method for preparing any of the aforementioned crystalline silicon film layers 1. This method may include the following steps.

[0037] Step 101: Provide an amorphous silicon film layer.

[0038] The crystallinity of the amorphous silicon film is lower than that of the first polycrystalline silicon portion 11, while the hydrogen content and porosity of the amorphous silicon film are both greater than those of the first polycrystalline silicon portion 11. Here, the hydrogen content in the amorphous silicon film can refer to the proportion of the total number of hydrogen bonds in the amorphous silicon film to the total number of bonds in the amorphous silicon film. The crystallinity in the amorphous silicon film can refer to the ratio of crystals in the amorphous silicon film. The porosity in the amorphous silicon film can refer to the percentage of the total volume of pores in the amorphous silicon film to the total volume of the amorphous silicon film. The methods for determining the hydrogen content, crystallinity, and porosity of the amorphous silicon film can refer to the methods for determining the hydrogen content, crystallinity, and porosity of the first polycrystalline silicon portion 11 described above; to avoid repetition, they will not be repeated here.

[0039] Step 102: The amorphous silicon film layer is heated with infrared light until the temperature of the amorphous silicon film layer reaches a preset temperature. At least a portion of the amorphous silicon film layer is hydrogenated and crystallized using a laser. The portion affected by the laser forms a first polycrystalline silicon portion. The preset temperature is 5%-30% of the laser temperature. The infrared light heating and laser action are performed simultaneously, or the infrared light heating is performed first and then the laser action is performed.

[0040] Figure 5 A schematic diagram of crystallization and hydrogenation in an embodiment of the present invention is shown. Figure 6 A schematic diagram of crystallization and hydrogenation in the prior art is shown. In this invention, the main purpose of using infrared light 31 to heat the amorphous silicon film layer 2 is as follows: First, infrared light 31 causes virtually no damage and can provide a certain heat base for the amorphous silicon film layer 2, reducing the energy of the laser 32 and thus reducing laser damage. Second, hydrogen has a high absorption rate for infrared light 31, facilitating the slow release of hydrogen, which can significantly reduce porosity. Third, infrared light 31 can easily raise the temperature of the amorphous silicon film layer 2 to the preset temperature. That is, relative to… Figure 6 In the prior art shown, only laser 32 is used for crystallization and hydrogenation. In this invention, due to the auxiliary heating of infrared light 31, the energy of laser 32 can be reduced, which can reduce laser damage. In addition, hydrogen has a high absorption rate for infrared light 31, which is conducive to the slow release of hydrogen. At the same time, infrared light 31 can easily raise the temperature of amorphous silicon film layer 2 to the preset temperature.

[0041] It should be noted that in this invention, infrared light 31 is used to heat the entire amorphous silicon film layer 2. Compared to using only infrared light 31 to heat the parts requiring crystallization and hydrogenation, this method has several advantages: firstly, it eliminates the need for alignment, simplifying the heating process; secondly, the entire amorphous silicon film layer 2 is heated more uniformly, resulting in a more uniform stress distribution and reducing warping. For example, the amorphous silicon film layer 2 can be placed on an auxiliary platform, and the auxiliary platform can be heated to a preset temperature using infrared light.

[0042] The preset temperature is 5%-30% of the laser temperature. At this preset temperature, the laser and infrared light work well together, facilitating the slow release of hydrogen. This slow hydrogen release significantly reduces porosity. Simultaneously, this preset temperature is easily achievable by infrared light, and combined with the laser, it achieves good crystallization and hydrogenation effects with less laser damage. In this invention, the main purpose of combining laser and infrared light is to facilitate the slow release of hydrogen and reduce laser damage; the improvement in crystallization rate is not excessively limited. For example, this temperature can be 5%, 8%, 9%, 10%, 13.5%, 17%, 17.5%, 18%, 21%, 28%, or 30% of the laser temperature.

[0043] In the amorphous silicon film 1, the portion affected by the laser 32 forms the first polycrystalline silicon portion 11. The portion not affected by the laser 32 serves as the amorphous silicon portion.

[0044] Infrared light 31 heating and laser 32 action are performed simultaneously. That is, while infrared light 31 heats the amorphous silicon film layer 2, laser 32 is used to hydrogenate and crystallize at least a portion of the amorphous silicon film layer 2. Infrared light 31 heats the amorphous silicon film layer 2 to reach the aforementioned preset temperature. Infrared light 31 heating followed by laser 32 action means that infrared light 31 is first used to heat the amorphous silicon film layer 2 to the aforementioned preset temperature, and then laser 32 is used to hydrogenate and crystallize at least a portion of the amorphous silicon film layer 2.

[0045] Optionally, in this invention, the power of the laser 32 is between 20W and 200W. Lasers at this power facilitate the slow release of hydrogen. Slow hydrogen release can significantly reduce porosity and cause less laser damage. Simultaneously, the degree of crystallization and hydrogenation is more suitable. The preset temperature is between 100℃ and 300℃. Infrared light 31 can easily raise the temperature of the amorphous silicon film 2 to this preset temperature. Moreover, with the assistance of this preset temperature, laser damage is less, the hydrogen release rate is more suitable, and porosity can be further reduced.

[0046] For example, in this invention, the power of the laser 32 is 20W, 30W, 50W, 60W, 90W, 105W, 110W, 113W, 140W, 170W, or 200W. The preset temperature can be 100℃, 110℃, 140℃, 160℃, 190℃, 197℃, 200℃, 210℃, 260℃, 290℃, or 300℃.

[0047] It should be noted that the wavelength of infrared light 31 is not limited in this invention, and the wavelength of laser 32 and other wavelengths are also not limited. For example, the wavelength of infrared light 31 can be 50nm-3000nm. Laser 32 can be a nanosecond laser of 500-600nm. Alternatively, laser 32 can be green light with a pulse width of 10ns-100ns, a spot size of 20um-300um (micrometers), and a wavelength of 492nm-577nm.

[0048] Figure 7 A schematic diagram of a laser according to an embodiment of the present invention is shown. Figure 7 In the image, the black and white triangles distributed at the top and bottom are all triangular laser spots. Figure 8 A schematic diagram of a laser in the prior art is shown. (Refer to...) Figure 8 In existing technologies, square laser spots are commonly used in the photovoltaic field. However, the inventors discovered that square laser spots have a large number of sides, and each side inevitably contains burrs, making it difficult to stitch them into a regular shape during the assembly process. Furthermore, due to the numerous burrs, there are many laser-damaged areas with irregular distribution, making it difficult to remove laser-induced damage. Optionally, to address this problem, the inventors creatively adjusted the shape of the laser spot 32 to a triangle, such as... Figure 7 As shown, compared to a square, a triangle has fewer sides and fewer burrs, making it easier to assemble into a regular shape during the splicing process. Moreover, due to fewer burrs, the laser-damaged area is smaller and more regularly distributed, making it easier to remove laser-induced damage.

[0049] More specifically, the triangular laser spot can be an equilateral triangular laser spot, which makes it easier to stitch into a regular pattern during the splicing process. Moreover, there are fewer burrs, fewer laser-damaged areas, and a more regular distribution, making it easier to remove laser-induced damage.

[0050] Optionally, step 101 may include: providing a substrate. On a first surface of the substrate, an amorphous silicon film 2 with a crystallinity of 5%-40% and a porosity of 0.1%-20% is formed using LPCVD (Low Pressure Chemical Vapor Deposition). Alternatively, on the substrate, an amorphous silicon film 2 with a crystallinity of 5%-30% and a porosity of 0.1%-20% is formed using PECVD (Plasma Enhanced Chemical Vapor Deposition). In the PECVD method, the process parameters include at least one of the following five: RF power supply switching ratio of 1 / 5-4 / 5; discharge cycles of 20,000-50,000; discharge gas is a mixture of hydrogen, nitrogen, and argon; in this mixture, the volume concentration of hydrogen is 5%-70%, and the volume concentration of argon is 10%-80%; the RF power supply power is 5000W-15000W; and the process temperature is 300°C-500°C.

[0051] Specifically, the substrate is the deposition support for amorphous silicon film layer 2, and the material of the substrate is not specifically limited. Using LPCVD, due to the temperature during the LPCVD deposition process, the amorphous silicon film layer 2 exhibits a certain degree of crystallization, with a crystallization rate between 5% and 40% and a porosity between 0.1% and 20%. Because PECVD has a lower deposition temperature, the amorphous silicon film layer 2 has a lower crystallization rate, between 5% and 30%, and a porosity between 0.1% and 20%. In PECVD, adjusting the RF power switching ratio, using a smaller switching ratio and a denser switching frequency, achieves high-quality film deposition. Specifically, the switching ratio ranges from 1 / 5 to 4 / 5, and the number of discharge cycles ranges from 20,000 to 50,000. By adjusting the RF power switching ratio and the number of discharge cycles, a high-quality amorphous silicon film layer 2 with a thickness variation within 5% is obtained. And / or, in PECVD, the discharge gas is a mixture of hydrogen, nitrogen, and argon. In this mixed gas, the volume concentration of hydrogen is 5%-70%, and the volume concentration of argon is 10%-80%. This invention uses a mixture of nitrogen, argon, and hydrogen for discharge. Hydrogen molecules are small and ionize more easily into the amorphous silicon film layer 2. The nitrogen and argon gases assist in ionization; however, nitrogen and argon molecules are larger than hydrogen molecules and ionize less readily into the amorphous silicon film layer 2, thus reducing porosity. Furthermore, the use of nitrogen and argon ensures effective ionization. Simultaneously, when the substrate is silicon, nitrogen readily reacts with the silicon substrate, while argon is more expensive. Using both nitrogen and argon, with an argon volume concentration of 10%-80%, reduces cost and decreases the reaction with the silicon substrate compared to using only one of them. And / or, in the PECVD process, the power of the RF power supply is 5000W-15000W. The relatively low power of the RF power supply can reduce power consumption and appropriately reduce the crystallinity of the amorphous silicon film layer 2, thereby reducing the thickness variation of the amorphous silicon film layer 2. And / or, in the PECVD process, the process temperature is 300°C-500°C, which can reduce power consumption and appropriately reduce the crystallinity of the amorphous silicon film layer 2, thereby reducing the thickness variation of the amorphous silicon film layer 2. Since the thickness variation of the amorphous silicon film layer 2 is small, the thickest part will not be too thick, and the cleaning time for the amorphous silicon film layer 2 can be reduced by 10% to 50%.

[0052] For example, the substrate can be a silicon substrate. In the PECVD process, the RF power switching ratio can be 1 / 5, 1 / 4, 1 / 3, 2 / 5, 1 / 2, 3 / 5, 2 / 3, 3 / 4, or 4 / 5. The number of discharge cycles can be 20,000, 22,000, 29,000, 33,000, 34,000, 35,000, 37,000, 40,000, or 50,000. The discharge gas is a mixture of hydrogen, nitrogen, and argon. In this mixture, the volume concentration of hydrogen can be 5%, 10%, 19%, 26%, 35%, 37.5%, 50%, or 70%, and the volume concentration of argon can be 10%, 30%, 40%, 50%, 60%, 67.5%, 70%, or 80%. The power of the RF power supply can be 5000W, 6000W, 7000W, 9000W, 9600W, 10000W, 11000W, 13000W, 14000W, or 15000W. The process temperature can be 300°C, 310°C, 360°C, 390°C, 400°C, 405°C, 430°C, 480°C, or 500°C.

[0053] Optionally, the aforementioned provision of the substrate may include: polishing the first surface of the substrate to obtain a first surface with a reflectivity of 30%-50%, the first surface of the substrate being flatter, and on the flatter first surface, it is easier to obtain an amorphous silicon film layer 2 with better film quality.

[0054] For example, the first surface of the substrate is polished to obtain a first surface with a reflectivity of 30%, 32%, 39%, 40%, 41%, 46%, 49%, or 50%.

[0055] It should be noted that there are no specific limitations on the etchant used for polishing. For example, the etchant for polishing may include an alkaline solution and an etching additive, wherein the mass concentration of the alkaline solution and the mass concentration of the etching additive are both 1%-20%.

[0056] The present invention also provides a solar cell, comprising: a silicon substrate, a tunneling oxide layer on the silicon substrate, and a first doped film layer on the tunneling oxide layer. The first doped film layer here is a film layer formed under the influence of subsequent steps after any of the aforementioned crystalline silicon film layers 1 are formed during the formation of the solar cell. Alternatively, the first doped film layer here is a film layer formed under the influence of subsequent steps after crystalline silicon film layer 1 is prepared by any of the aforementioned methods for preparing crystalline silicon film layer 1 during the formation of the solar cell. Therefore, the structure of the first doped film layer in the solar cell is similar to the structure of the aforementioned crystalline silicon film layer, and the first doped film layer in the solar cell may include: at least one second polycrystalline silicon portion, the second polycrystalline silicon portion extending through the first doped film layer in the thickness direction. In this solar cell, after the crystalline silicon film layer 1 is formed, there is a high probability that the fabrication of other layers will involve heating processes. These heating processes may have a thermal impact on the first polycrystalline silicon portion 11. For example, electrode sintering may have a certain thermal impact on the crystalline silicon film layer 1. The thermal impact is mainly reflected in the increase of crystallinity, which may in turn increase the crystallinity of the first polycrystalline silicon portion 11. Therefore, the crystallinity of the first doped film layer in the solar cell is greater than or equal to 60%. For example, the crystallinity of the first polycrystalline silicon portion 11 of the crystalline silicon film layer 1 is 50% to 60%, while the crystallinity of the second polycrystalline silicon portion in this solar cell is 60% to 80%. The hydrogen content and porosity of the first polycrystalline silicon portion 11 are less affected by heat. Therefore, in this solar cell, the hydrogen content and porosity of the second polycrystalline silicon portion are basically the same as those of the first polycrystalline silicon portion 11. Thus, in this solar cell, the hydrogen content of the second polycrystalline silicon portion is 1% to 20%, and the porosity of the second polycrystalline silicon portion is 0.1% to 10%.

[0057] In the case where the first doped film layer is formed under the influence of subsequent steps after the crystalline silicon film layer 1 is prepared by any of the aforementioned methods for preparing crystalline silicon film layer 1 during the formation of a solar cell, the substrate in the aforementioned method for preparing crystalline silicon film layer 1 may be a silicon substrate and a tunneling oxide layer located on the silicon substrate.

[0058] In this solar cell, the second polycrystalline silicon portion has a higher crystallinity, a more suitable hydrogen content, and a more suitable porosity, resulting in a superior film quality and thus improving the photoelectric conversion efficiency of the solar cell. Other advantages of this solar cell can be found in the aforementioned descriptions of crystalline silicon film layer 1 or its preparation method, and they possess similar or comparable beneficial effects. To avoid repetition, these will not be elaborated upon here. The specific type of this solar cell is not limited.

[0059] Optionally, the first doped film layer is entirely composed of the second polycrystalline silicon portion, that is, referring to... Figure 1 The crystalline silicon film layer 1 is entirely composed of the first polycrystalline silicon portion 11. The surface of the silicon substrate away from the crystalline silicon film layer 1 has a textured structure. For the fabrication of this solar cell, after the crystalline silicon film layer 1 is set, the surface of the silicon substrate away from the crystalline silicon film layer 1 can be textured. During the texturing process, since the crystalline silicon film layer 1 is entirely composed of the first polycrystalline silicon portion 11, the quality of the crystalline silicon film layer 1 is superior. The crystalline silicon film layer 1 is basically not etched in the texturing solution. Therefore, there is no need to set a mask layer on the crystalline silicon film layer 1, which reduces the steps of setting the mask layer and the steps of removing the mask layer. The production steps of this solar cell are fewer and the production efficiency is higher.

[0060] Optionally, the thickness variation of the first doped film layer is less than 5%. Specifically, the first doped film layer here refers to the film layer formed under the influence of subsequent steps after any of the aforementioned crystalline silicon film layers 1 are formed during the formation of a solar cell. Alternatively, the first doped film layer here refers to the film layer formed under the influence of subsequent steps after crystalline silicon film layer 1 is prepared by any of the aforementioned methods during the formation of a solar cell. The influence of subsequent steps is mainly thermal, which has virtually no effect on the thickness variation. Therefore, the thickness variation of the first doped film layer is also less than 5%. The thickness variation of the first doped film layer being less than 5% indicates that the thickness uniformity of the first doped film layer is good. During the processing of each first doped film layer, the thickest part will not be too thick, and the processing time will not be too long, thus saving process time and improving production efficiency. The method for determining the thickness variation of the first doped film layer can refer to the method for determining the thickness variation of the crystalline silicon film layer mentioned above. To avoid repetition, it will not be repeated here.

[0061] The present invention also provides a back-contact solar cell, comprising: a silicon substrate, and a first region and a second region projected onto the silicon substrate. The first region and the second region are alternately distributed. The relative size of the first region and the second region is not limited. The first region may include: a tunneling oxide layer and a first transport layer stacked thereon. The relative positional relationship between the first transport layer and the tunneling oxide layer can be: the first transport layer is located on the surface of the silicon substrate near the tunneling oxide layer or on the silicon substrate, and the tunneling oxide layer is located on the first transport layer; or, the tunneling oxide layer is located on the silicon substrate, and the first transport layer is located on the tunneling oxide layer, i.e., the tunneling oxide layer is located between the silicon substrate and the first transport layer. The crystallinity of the first transport layer is greater than or equal to 60%, the hydrogen content of the first transport layer is 1% to 20%, and the porosity of the first transport layer is 0.1% to 10%. Here, the first transport layer is: a film layer formed after the amorphous silicon portion is removed following the formation of any of the aforementioned crystalline silicon film layers 1 during the formation of the back-contact solar cell, and under the influence of subsequent steps. Alternatively, the first transport layer here can be: after the crystalline silicon film 1 is prepared by any of the aforementioned methods for preparing crystalline silicon film 1 during the formation of the back contact solar cell, the amorphous silicon portion is removed, and the film is formed under the influence of subsequent steps. In this back contact solar cell, after the crystalline silicon film 1 is set, there is a high probability that there will be heating processes during the preparation of other layers. These heating processes may have a thermal impact on the first polycrystalline silicon portion 11. For example, electrode sintering may have a certain thermal impact on the crystalline silicon film 1. The thermal impact is mainly reflected in the increase of crystallinity, which may in turn increase the crystallinity of the first polycrystalline silicon portion 11. Therefore, the crystallinity of the first transport layer in the back contact solar cell is greater than or equal to 60%. For example, the crystallinity of the first polycrystalline silicon portion 11 of the crystalline silicon film 1 is 50% to 60%, while the crystallinity of the first transport layer in this back contact solar cell is 60% to 80%. The hydrogen content and porosity of the first polycrystalline silicon portion 11 are less affected by heat. Therefore, in this back contact solar cell, the hydrogen content and porosity of the first transport layer are basically the same as those of the first polycrystalline silicon portion 11. Thus, in this back contact solar cell, the hydrogen content of the first transport layer is 1% to 20%, and the porosity of the second polycrystalline silicon portion is 0.1% to 10%.

[0062] The second region may include a second transport layer. The first and second transport layers have different doping types; that is, one of the first and second transport layers is P-type doped, and the other is N-type doped. It should be noted that the presence of a tunneling oxide layer in the second region is not limited; for example, the second region may not have a tunneling oxide layer. If a tunneling oxide layer is present in the second region, the relative positional relationship between the second transport layer and the tunneling oxide layer is also not specifically limited.

[0063] This back-contact solar cell has similar or nearly identical beneficial effects to the aforementioned crystalline silicon film layer, which will not be repeated here to avoid repetition. The specific type of this back-contact solar cell is not limited.

[0064] Optionally, the thickness variation of the first transport layer is less than 5%. Specifically, the first transport layer here is: a film layer formed after the amorphous silicon portion is removed following the formation of any of the aforementioned crystalline silicon film layers 1 during the formation of the back contact solar cell, and under the influence of subsequent steps. Alternatively, the first transport layer here is: a film layer formed after the crystalline silicon film layer 1 is prepared by any of the aforementioned methods during the formation of the back contact solar cell, after the amorphous silicon portion is removed, and under the influence of subsequent steps. The influence of subsequent steps is mainly thermal, which has virtually no effect on the thickness variation; therefore, the thickness variation of the first transport layer is also less than 5%. The thickness uniformity of the first transport layer is good, ensuring that the thickest part is not excessively thick during processing, thus reducing processing time and improving production efficiency. The method for determining the thickness variation of the first transport layer can refer to the method for determining the thickness variation of the crystalline silicon film layer described above; to avoid repetition, it will not be repeated here.

[0065] The present invention also provides a method for preparing the aforementioned back-contact solar cell, comprising the following steps.

[0066] Step S1, providing a conductive substrate; the conductive substrate includes: a silicon substrate, a tunneling oxide layer and a crystalline silicon film layer sequentially stacked on the silicon substrate; the crystalline silicon film layer is any of the aforementioned crystalline silicon film layers, or the crystalline silicon film layer is prepared by any of the aforementioned methods for preparing crystalline silicon film layers; the crystalline silicon film layer includes: at least one first polycrystalline silicon portion and at least one amorphous silicon portion; the amorphous silicon portion extends through the crystalline silicon film layer from its thickness direction; in the crystalline silicon film layer, the first polycrystalline silicon portion and the amorphous silicon portion are alternately distributed.

[0067] The silicon substrate, tunneling oxide layer, and crystalline silicon film layer can all include: a first region projected onto the silicon substrate and a second region projected onto the silicon substrate, with the first and second regions alternating. In the crystalline silicon film layer, a first polycrystalline silicon portion is located within the first region, and an amorphous silicon portion is located within the second region. Both the amorphous silicon portion and the first polycrystalline silicon portion penetrate the crystalline silicon film layer along its thickness direction. The first polycrystalline silicon portion and the amorphous silicon portion are alternating, i.e., the crystalline silicon film layer 1 refers to... Figure 2 As shown.

[0068] In step S2, when each of the first polysilicon portions is not covered by a mask layer, the conductive substrate is wet-etched. Each of the first polysilicon portions is retained in the wet etching, and each of the amorphous silicon portions is removed in the wet etching, exposing the tunneling oxide layer or the second region of the silicon substrate.

[0069] In step S2, the first polysilicon portion retained during wet etching forms the first transport layer under the influence of subsequent steps.

[0070] Step S3: Form a second transport layer on the exposed second region.

[0071] That is, the crystalline silicon film layer 1 is referenced. Figure 2 As shown. During the wet etching process in step S2, because the first polycrystalline silicon portion 11 has superior quality, it is essentially not etched in the wet etching solution. Therefore, no mask layer needs to be set on each of the first polycrystalline silicon portions 11, reducing the steps of setting mask layers on each of the first polycrystalline silicon portions 11 and reducing the steps of removing mask layers. This results in fewer production steps and higher production efficiency for the back contact solar cell. It should be noted that during the wet etching process to remove the amorphous silicon portion in the crystalline silicon film layer, the underlying tunneling oxide layer may also be etched away. Therefore, the portion of the silicon substrate located in the second region may also be exposed. If the tunneling oxide layer in the second region is not etched away, the second region of the tunneling oxide layer is exposed, and a second transport layer is formed on the second region of the tunneling oxide layer. If the second region of the tunneling oxide layer is etched away, the second region of the silicon substrate is exposed, and a second transport layer can be formed on the second region of the tunneling oxide layer.

[0072] Optionally, the first transport layer can be a P-type doped transport layer, and the second transport layer can be an N-type doped transport layer, which can reduce the thermal impact.

[0073] The present application will be further explained below with reference to specific embodiments.

[0074] Example 1 A tunneling oxide layer is formed on a silicon substrate. Both the tunneling oxide layer and the silicon substrate include a first region and a second region, which are alternately distributed. The first surface of the tunneling oxide layer away from the silicon substrate includes a portion located in the first region and a portion located in the second region. On the tunneling oxide layer, a P-type doped amorphous silicon film 2 with a crystallinity of 5%-30%, a porosity of 0.1%-20%, and a hydrogen content of 30%-40% is formed using PECVD. The amorphous silicon film 2 is heated with infrared light until its temperature reaches a preset temperature of 100°C and held at that temperature. Then, a 20W laser is used to hydrogenate and crystallize multiple portions of the amorphous silicon film 2 located in the first region. The laser-treated portions form a first polycrystalline silicon portion 11, and the portions not treated by the laser form an amorphous silicon portion 12. That is, the portions of the amorphous silicon film 2 located in the second region form an amorphous silicon portion 12, resulting in a conductive substrate. The first polycrystalline silicon portion 11 and the amorphous silicon portion 12 both extend through the amorphous silicon film layer 2 along its thickness direction. In the crystalline silicon film layer 1, the first polycrystalline silicon portion 11 and the amorphous silicon portion 12 are alternately distributed, resulting in a crystalline silicon film layer 1 as shown in the figure. Figure 2 As shown. In the PECVD method: the RF power supply switching ratio is 3 / 5, the number of discharge cycles is 40,000, and the discharge gas is a mixture of hydrogen, nitrogen, and argon. In the mixture, the volume concentration of hydrogen is 40%, the volume concentration of argon is 43%, and the volume concentration of nitrogen is 17%. The RF power supply has a power of 10,000W, and the process temperature is 400°C.

[0075] Without a mask layer covering each of the first polysilicon portions 11, the conductive substrate is wet-etched. The wet etchant consists of alkali and additives, and the etching time is 15 to 20 minutes. The first polysilicon portions 11 are largely unetched during the wet etching process and are mostly preserved. The amorphous silicon portions 12 are removed during the wet etching, exposing the second region of the tunneling oxide layer. Then, a mixed acid cleaning process is performed for 15-20 minutes. The mixed acid can include HF, HNO3, H2SO4, etc. The purpose of the mixed acid is to neutralize the alkali in the wet etchant and etch away the portion of the tunneling oxide layer located in the second region, exposing the second region of the silicon substrate.

[0076] An N-type doped second transport layer is formed on the second region exposed on the silicon substrate.

[0077] Compared to existing technologies that involve forming a relatively uniform polycrystalline silicon film and then removing the polycrystalline silicon film in the second region using a laser, firstly, in Example 1, the laser only serves for hydrogenation and crystallization, and with the assistance of infrared light, the laser power is lower, resulting in less laser damage; secondly, in Example 1, the laser-acting area is as follows... Figure 2It is only the first polysilicon portion 11. However, in the prior art, laser is used to remove the second region. Since the second region needs to form another doped second transport layer and also needs to leave an insulating region that mainly plays an insulating role, the second region is larger, that is, the laser action area is larger. In other words, compared with the prior art, the laser action area in this application is also smaller, and the laser damage is further greatly reduced.

[0078] Example 2 Infrared light is used to heat the amorphous silicon film layer 2 until the temperature of the amorphous silicon film layer 2 reaches the preset temperature of 130°C and is maintained at that temperature. Then, a 30W laser is used to hydrogenate and crystallize multiple parts of the amorphous silicon film layer 2.

[0079] The rest of Example 2 is the same as Example 1.

[0080] Example 3 Infrared light is used to heat the amorphous silicon film layer 2 until the temperature of the amorphous silicon film layer 2 reaches the preset temperature of 170°C and is maintained at that temperature. Then, a 40W laser is used to hydrogenate and crystallize multiple parts of the amorphous silicon film layer 2.

[0081] The rest of Example 3 is the same as Example 1.

[0082] Example 4 Infrared light is used to heat the amorphous silicon film layer 2 until the temperature of the amorphous silicon film layer 2 reaches the preset temperature of 200℃ and is maintained at that temperature. Then, a 50W laser is used to hydrogenate and crystallize multiple parts of the amorphous silicon film layer 2.

[0083] The rest of Example 4 is the same as Example 1.

[0084] Example 5 Infrared light is used to heat the amorphous silicon film layer 2 until the temperature of the amorphous silicon film layer reaches the preset temperature of 230℃ and is maintained at that temperature. Then, a 60W laser is used to hydrogenate and crystallize multiple parts of the amorphous silicon film layer 2.

[0085] The rest of Example 5 is the same as that of Example 1.

[0086] Example 6 Infrared light is used to heat the amorphous silicon film layer 2 until the temperature of the amorphous silicon film layer 2 reaches the preset temperature of 270°C and is maintained at that temperature. Then, a 70W laser is used to hydrogenate and crystallize multiple parts of the amorphous silicon film layer 2.

[0087] The rest of Example 6 is the same as that of Example 1.

[0088] Figure 9This document illustrates the hydrogen content and crystallinity distribution of the first polycrystalline silicon portion in various embodiments of the present invention. For the amorphous silicon film 2 formed by PECVD in Examples 1 to 6, no laser crystallization or hydrogenation is performed; instead, the wet etchant used in Examples 1 to 6 is directly applied, and cleaning is carried out under the same etching conditions. The cleaning parameters are shown in the second row of Table 1 below. The crystallinity and hydrogen content of the first polycrystalline silicon portion 11 in the crystalline silicon film 1 formed after laser crystallization and hydrogenation in Examples 1 to 6 are measured. The measurement results are shown in Table 1 and below. Figure 9 . Figure 9 In the text, G1 represents Example 1, G2 represents Example 2, G3 represents Example 3, G4 represents Example 4, G5 represents Example 5, and G6 represents Example 6.

[0089] Table 1: Partial Process Parameters and Measurement Results

[0090] Referring to the second row of Table 1, for the amorphous silicon film 2 formed by PECVD in Examples 1 to 6, no laser crystallization and hydrogenation are performed. Instead, the wet etchant used in Examples 1 to 6 is directly applied, and cleaning is carried out under the same etching conditions. The cleaning is basically completed in 6-12 minutes. As can be seen from Examples 1 to 6 and Table 1, for the crystalline silicon film 1 formed after laser crystallization and hydrogenation in Examples 1 to 6, when the wet etchant used in Examples 1 to 6 is applied and cleaning is carried out under the same etching conditions for 15-20 minutes, the various first polycrystalline silicon portions 11 are basically not etched during the wet etching process and are mostly preserved. The specific reason is that, in this invention, by combining infrared light-assisted heating and laser, the temperature of the assisted heating and the laser power are perfectly matched, resulting in a suitable crystallinity of the first polycrystalline silicon portion 11. This facilitates the slow release of hydrogen, which can significantly reduce porosity. Consequently, a first polycrystalline silicon portion 11 with excellent film quality can be obtained. Without the need for mask layers on each of the first polycrystalline silicon portions 11, the high-quality first polycrystalline silicon portions 11 are basically not etched in the etchant and are largely preserved. This reduces the steps of setting and removing mask layers on each of the first polycrystalline silicon portions 11, resulting in fewer process steps and higher production efficiency.

[0091] From Table 1 and Figure 9 As can be seen, in this invention, by combining infrared light-assisted heating and laser, the temperature of the assisted heating and the laser power are perfectly matched, and the crystallinity of the first polycrystalline silicon part 11 remains basically stable. It does not increase continuously with the increase of laser power. The hydrogen content is released slowly, which reduces the hydrogen content and also reduces the porosity.

[0092] It should be noted that, for the sake of simplicity, the method embodiments are all described as a series of actions. However, those skilled in the art should understand that the embodiments of this application are not limited to the described order of actions, because according to the embodiments of this application, some steps can be performed in other orders or simultaneously. Secondly, those skilled in the art should also understand that the embodiments described in the specification are all preferred embodiments, and the actions involved are not necessarily essential to the embodiments of this application.

[0093] It should be noted that, in this document, the terms "comprising," "including," or any other variations thereof are intended to cover non-exclusive inclusion, such that a process, method, article, or apparatus that comprises a list of elements includes not only those elements but also other elements not expressly listed, or elements inherent to such a process, method, article, or apparatus. Unless otherwise specified, an element defined by the phrase "comprising one..." does not exclude the presence of other identical elements in the process, method, article, or apparatus that includes that element.

[0094] Through the above description of the embodiments, those skilled in the art can clearly understand that the methods of the above embodiments can be implemented by means of software plus necessary general-purpose hardware platforms. Of course, they can also be implemented by hardware, but in many cases the former is a better implementation method. Based on this understanding, the technical solution of the present invention, or the part that contributes to the prior art, can be embodied in the form of a software product. This computer software product is stored in a storage medium (such as ROM / RAM, magnetic disk, optical disk) and includes several instructions to cause a terminal (which may be a mobile phone, computer, server, air conditioner, or network device, etc.) to execute the methods described in the various embodiments of the present invention.

[0095] The embodiments of the present invention have been described above with reference to the accompanying drawings. However, the present invention is not limited to the specific embodiments described above. The specific embodiments described above are merely illustrative and not restrictive. Those skilled in the art can make many other forms under the guidance of the present invention without departing from the spirit and scope of the claims. All of these forms are within the protection scope of the present invention.

Claims

1. A crystalline silicon film layer, characterized in that, The crystalline silicon film layer includes: at least one first polycrystalline silicon portion; the first polycrystalline silicon portion extends through the crystalline silicon film layer from its thickness direction. The crystallinity of the first polycrystalline silicon portion is 50% to 60%; The hydrogen content in the first polycrystalline silicon portion is 1% to 20%; The porosity of the first polycrystalline silicon portion is 0.1% to 10%; Wherein, the crystallization rate of the first polycrystalline silicon portion refers to the ratio of crystals in the first polycrystalline silicon portion; The hydrogen content in the first polycrystalline silicon portion refers to the proportion of the total number of hydrogen bonds in the first polycrystalline silicon portion to the total number of all bonds in the first polycrystalline silicon portion. The porosity of the first polycrystalline silicon portion refers to the percentage of the total volume of pores in the first polycrystalline silicon portion to the total volume of the first polycrystalline silicon portion.

2. The crystalline silicon film layer according to claim 1, characterized in that, The first polycrystalline silicon portion is a doped polycrystalline silicon portion, and the doping concentration of the doped polycrystalline silicon portion is 5 × 10⁻⁶. 18 cm -3 Up to 1×10 20 cm -3 .

3. The crystalline silicon film layer according to claim 1, characterized in that, The thickness variation of the crystalline silicon film is less than 5%.

4. The crystalline silicon film layer according to any one of claims 1 to 3, characterized in that, The crystalline silicon film layer further includes: at least one amorphous silicon portion; the amorphous silicon portion extends through the crystalline silicon film layer from its thickness direction; in the crystalline silicon film layer, the first polycrystalline silicon portion and the amorphous silicon portion are alternately distributed; the crystallization rate of the amorphous silicon portion is lower than that of the first polycrystalline silicon portion, and the hydrogen content and porosity of the amorphous silicon portion are both greater than those of the first polycrystalline silicon portion.

5. A method for preparing a crystalline silicon film layer according to any one of claims 1 to 4, characterized in that, include: Provides amorphous silicon films; The amorphous silicon film is heated with infrared light until the temperature of the amorphous silicon film reaches a preset temperature. At least a portion of the amorphous silicon film is hydrogenated and crystallized using a laser. The portion affected by the laser forms a first polycrystalline silicon portion. The preset temperature is 5%-30% of the laser temperature. The infrared heating and laser action are performed simultaneously, or the infrared heating is performed first and then the laser action is performed.

6. The method for preparing a crystalline silicon film according to claim 5, characterized in that, The power of the laser is 20W to 200W; The preset temperature is 100℃ to 300℃.

7. The method for preparing a crystalline silicon film according to claim 5 or 6, characterized in that, The laser spot is triangular in shape.

8. The method for preparing a crystalline silicon film according to claim 5 or 6, characterized in that, The provision of the amorphous silicon film layer includes: Provide substrate; On the first surface of the substrate, an amorphous silicon film with a crystallinity of 5%-40% and a porosity of 0.1% to 20% is formed by LPCVD. Alternatively, an amorphous silicon film with a crystallinity of 5%-30% and a porosity of 0.1% to 20% can be formed on the substrate using PECVD. In the PECVD method, the process parameters include at least one of the following five types: The RF power supply switching ratio is 1 / 5-4 / 5; The number of discharge cycles is 20,000 to 50,000. The discharge gas is a mixture of hydrogen, nitrogen, and argon; in the mixture, the volume concentration of hydrogen is 5%-70%, and the volume concentration of argon is 10%-80%. The power of the RF power supply is 5000W-15000W; The process temperature is 300°C-500°C.

9. The method for preparing a crystalline silicon film according to claim 8, characterized in that, The substrate provided includes: The first surface of the substrate is polished to obtain a first surface with a reflectivity of 30%-50%.

10. A solar cell, characterized in that, include: A silicon substrate, a tunneling oxide layer on the silicon substrate, and a first doped film layer on the tunneling oxide layer; The first doped film layer includes: at least one second polysilicon portion; the second polysilicon portion extends through the first doped film layer from the thickness direction. The crystallinity of the second polycrystalline silicon portion is greater than or equal to 60%; The hydrogen content in the second polycrystalline silicon portion is 1% to 20%; The porosity of the second polycrystalline silicon portion is 0.1% to 10%; The first doped film layer is formed from a crystalline silicon film layer as described in any one of claims 1 to 4, or a crystalline silicon film layer prepared by any one of the methods described in claims 5 to 9.

11. The solar cell according to claim 10, characterized in that, The first doped film layer is entirely composed of the second polycrystalline silicon portion; The surface of the silicon substrate away from the first doped film layer has a textured surface.

12. The solar cell according to claim 10 or 11, characterized in that, The thickness difference of the first doped film layer is less than 5%.

13. A back-contact solar cell, characterized in that, include: Silicon substrate; The projection falls on the first and second regions on the silicon substrate; The first region and the second region are alternately distributed; the first region includes: a tunneling oxide layer and a first transport layer stacked together; the crystallinity of the first transport layer is greater than or equal to 60%; the hydrogen content of the first transport layer is 1% to 20%; the porosity of the first transport layer is 0.1% to 10%; the second region includes a second transport layer; the first transport layer and the second transport layer have different doping types; The first transport layer is formed from a crystalline silicon film layer as described in any one of claims 1 to 4, or a crystalline silicon film layer prepared by any one of the methods described in claims 5 to 9.

14. The back-contact solar cell according to claim 13, characterized in that, The thickness difference of the first transmission layer is less than 5%.

15. A method for fabricating a back-contact solar cell according to claim 13 or 14, characterized in that, include: Provide a conductive substrate; The conductive substrate includes: a silicon substrate, a tunneling oxide layer and a crystalline silicon film layer sequentially stacked on the silicon substrate; the crystalline silicon film layer includes: at least one first polycrystalline silicon portion and at least one amorphous silicon portion; the amorphous silicon portion penetrates the crystalline silicon film layer from the thickness direction; in the crystalline silicon film layer, the first polycrystalline silicon portion and the amorphous silicon portion are alternately distributed; In the absence of a mask layer covering each of the first polysilicon portions, the conductive substrate is wet-etched, each of the first polysilicon portions is retained in the wet etching to form a first transport layer, each of the amorphous silicon portions is removed in the wet etching, and the tunneling oxide layer or the second region of the silicon substrate is exposed. A second transport layer is formed on the exposed second region.

Citation Information

Patent Citations

  • Method for forming thin semiconductor film, method for fabricating semiconductor device, system for executing these methods and electrooptic device

    US20030148565A1

  • Laser-irradiation method and laser-irradiation device

    US6455359B1