Acid-resistant adhesive for lead-acid battery and preparation method thereof
By combining modified epoxy resin and specific fillers, the acid resistance of lead-acid battery adhesives is improved, the problem of insufficient acid resistance in the prior art is solved, and higher acid resistance and mechanical properties are achieved. It is suitable for lead-acid acid In-depth application of batteries.
Patent Information
- Application Number
- CN202311690514.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-11
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2043-12-11
AI Technical Summary
The lack of acid resistance of existing epoxy resin binders in the field of lead-acid batteries has limited their deep application. The existing improvement methods are relatively single, making it difficult to meet the industry's demand for further improvement of acid resistance.
By preparing modified epoxy resin, combined with raw materials such as silicone-capped polymer, spherical alumina, barium sulfate and quartz powder, a specific ratio and process flow is used to prepare an acid-resistant adhesive to improve its acid resistance to improve its acid resistance Performance and physical performance.
It significantly improves the acid resistance and mechanical properties of the adhesive, meets the requirements of lead-acid batteries for acid resistance and adhesion, and enhances its stability and applicability in an acidic environment.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of adhesives, and in particular relates to an acid-resistant adhesive for lead-acid batteries and a preparation method thereof. Background Art
[0002] Adhesives for lead-acid batteries are mainly used for bonding battery shells and covers and sealing poles. The shells of lead-acid batteries are generally made of ABS, and the poles of lead-acid batteries are generally made of lead and lead alloys. Therefore, adhesives for lead-acid batteries need to have strong adhesion to lead, EPDM rubber (safety valve material) and ABS. At the same time, since the seal between the shell and cover of lead-acid batteries is the key to the sealing of the entire battery, the adhesive layer formed by the adhesive between the shell and cover will directly contact the acid gas and acid liquid, so the adhesive needs to have excellent acid resistance.
[0003] In actual production, epoxy resin adhesives are the most widely used in the field of lead-acid batteries. Epoxy resin adhesives have the advantages of strong bonding, low shrinkage, good electrical insulation, high mechanical strength, and good alkali resistance. However, due to the presence of a large number of ether bond structures in the epoxy resin structure, it is easy to react with protons, resulting in poor acid resistance, which limits its in-depth application in the field of lead-acid batteries.
[0004] Chinese patent CN104946188B discloses a lead-acid battery sealant and a preparation method thereof, and Chinese patent CN109439252B discloses an epoxy resin sealant and a preparation method and application thereof. In the above prior art, bisphenol A epoxy resin and bisphenol A composite bisphenol F epoxy resin are used as resin base materials to improve the acid corrosion resistance of epoxy resin sealants. The improvement means for acid resistance are relatively common. Chinese patent CN110616057B discloses a preparation and use method of a sealant for assembly line batteries. In the patent, bisphenol A epoxy resin and bisphenol F epoxy resin are first selected for compounding as resin base materials, and then o-cresol glycidyl ether, a diluent with excellent acid resistance, is selected. Finally, a hyperbranched p-phenylenediamine polymer is added to the B component to achieve a significant improvement in acid resistance. The principle is to use the hyperbranched structure to cover the polar groups such as hydrophilic ether bonds that are easily affected by the acid environment to avoid direct contact with the acid environment, thereby improving its acid resistance to a certain extent.
[0005] In the prior art, the means for improving the acid resistance of epoxy resin adhesives are relatively simple, and with the continuous development of the lead-acid battery industry, the acid resistance of adhesives used for lead-acid batteries still needs to be further improved and enhanced. Summary of the invention
[0006] The invention provides an acid-resistant adhesive for lead-acid batteries and a preparation method thereof, and improves the applicability of the epoxy resin adhesive in lead-acid batteries by improving the acid resistance of the epoxy resin adhesive.
[0007] An object of the present invention is to provide an acid-resistant adhesive for lead-acid batteries;
[0008] Another object of the present invention is to provide a method for preparing the above acid-resistant adhesive.
[0009] The purpose of the present invention can be achieved by the following technical solutions:
[0010] An acid-resistant adhesive for lead-acid batteries, comprising a component A and a component B mixed in a mass ratio of 2.8-3.5:1;
[0011] The A component includes the following raw materials in parts by mass:
[0012] 70-75 parts of modified epoxy resin;
[0013] 15-20 parts of filler;
[0014] 12-15 parts of toughening agent;
[0015] 8-15 parts of diluent;
[0016] 2-4 parts of defoaming agent;
[0017] The B component, in parts by mass, includes the following raw materials:
[0018] Curing agent 55-70 parts;
[0019] 5-12 parts of accelerator;
[0020] 1-4 parts of coupling agent;
[0021] The modified epoxy resin is prepared by the following steps:
[0022] Add polycaprolactone triol to 1,1,1-trimethylolpropane with stirring, heat to 110-115°C, and stir to react for 3 hours. After the reaction is completed, cool to 60°C and introduce argon protection, then add dibutyltin dilaurate and isocyanatepropyltriethoxysilane, continue stirring until the -NCO reaction in the system is complete, stop the reaction, cool to room temperature, and stir to add epoxy resin, stir and mix for 24 hours to obtain a modified epoxy resin.
[0023] Furthermore, the usage ratio of the 1,1,1-trimethylolpropane, polycaprolactone triol, dibutyltin dilaurate, isocyanatepropyltriethoxysilane and epoxy resin is 8.5-11.2g:98-100g:0.1g:84-85g:225-250g.
[0024] Furthermore, the filler is a mixture of spherical alumina, barium sulfate and quartz powder in a mass ratio of 3-5:1-2:1.
[0025] Furthermore, the spherical alumina is a mixture of spherical alumina with gradient median particle sizes, which is a mixture of spherical alumina with a median particle size of 90-110 μm, spherical alumina with a median particle size of 40-70 μm and spherical alumina with a median particle size of 1.5-3.0 μm in a mass ratio of 5:2:1.
[0026] Furthermore, the toughening agent is one of amino-terminated liquid nitrile rubber and liquid polysulfide rubber.
[0027] Furthermore, the diluent is one of X-52 cresol glycidyl ether and LITE-2020.
[0028] Furthermore, the defoaming agent is one of BYK-1794, BYK-054 and BYK-A535.
[0029] Furthermore, the curing agent is one of NX-2003D, NX-2040, and Ancamine2280.
[0030] Furthermore, the accelerator is DMP-30 (2,4,6-tris(dimethylaminomethyl)phenol).
[0031] As a further embodiment of the present invention, a method for preparing an acid-resistant adhesive for a lead-acid battery comprises the following steps:
[0032] Weigh the raw materials in component A and component B respectively in parts by mass, add filler and toughening agent to the modified epoxy resin, stir and disperse at a speed of 800-1000r / min for 30min, then add diluent and defoaming agent, stir and disperse at 1000-1200r / min for 30min, place under vacuum degree of -0.1MPa vacuum degree condition for vacuum degassing for 1h to obtain component A, stir and disperse the curing agent, accelerator and coupling agent at a speed of 400-600r / min for 30min to obtain component B, mix component A and component B in a mass ratio of 2.8-3.5:1 to obtain.
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] The invention provides an acid-resistant adhesive for lead-acid batteries, which is prepared from modified epoxy resin, filler, toughening agent, diluent, curing agent and other raw materials.
[0035] Firstly, the modified epoxy resin prepared by the present invention is composited with an epoxy resin and a siloxane-terminated polymer. The epoxy resin is compositely modified by using a siloxane-terminated polymer synthesized by a nucleophilic addition reaction of isocyanatepropyltriethoxysilane and 1,1,1-trimethylolpropane. The network structure of the siloxane-terminated polymer helps to reduce the protonation corrosion of polar groups such as ether bonds in the epoxy resin by acid solution. The finally prepared adhesive has excellent acid resistance.
[0036] Then, the spherical alumina, barium sulfate and quartz powder in the filler are all inert acid-resistant fillers. The addition of inert acid-resistant fillers can improve the acid resistance of the adhesive. Among them, spherical alumina and barium sulfate can improve the physical properties of the adhesive, and quartz powder can improve the bonding durability. Compared with traditional fillers such as mica powder (the slip of mica powder will reduce the bonding performance of the adhesive) and calcium carbonate (calcium carbonate has poor acid resistance and will cause the adhesive to bubble under acidic conditions), it can significantly improve the acid resistance, physical properties and bonding of the adhesive. Among them, the spherical alumina with a gradient median particle size selected in the present invention can better achieve close stacking, while reducing the amount of filler, fully ensuring that the filler improves the acid resistance and physical properties of the adhesive. The amount of filler in the adhesive needs to be precisely controlled. Too much filler will affect the fluidity and lightness of the adhesive. Since the shell-cover gap of the lead-acid battery is narrow, only by ensuring that the adhesive has good fluidity can the production requirements be met. At the same time, the tightly stacked spherical alumina can achieve a uniform and comprehensive improvement in the acid resistance of the adhesive.
[0037] Next, the adhesive toughened with the amino-terminated liquid nitrile rubber in the toughening agent has a two-phase structure with better acid resistance and mechanical properties.
[0038] Then, the main component of LITE-2020 in the diluent is cardanol molecules, and the long hydrophobic fatty side chains of cardanol molecules give the adhesive extremely low viscosity and excellent acid resistance.
[0039] At the same time, the NX-2003D in the curing agent is a cashew nut shell oil modified phenolic amine curing agent. The curing system of NX-2003D has good mechanical strength, bonding strength and acid resistance.
[0040] Finally, the acid-resistant adhesive prepared by the present invention is a solvent-free adhesive. Although the solvent can reduce the viscosity of the adhesive, it is not easy to evaporate from the cured adhesive layer of the adhesive, which will cause more bubbles to be generated on the surface of the adhesive after curing, affecting the acid resistance of the adhesive. Solvent-free addition is also one of the improvements of the present invention to the existing acid-resistant adhesive used for lead-acid batteries. DETAILED DESCRIPTION
[0041] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] Example 1 Preparation of modified epoxy resin:
[0043] 8.5 g of 1,1,1-trimethylolpropane (TMP; analytical grade; purchased from Shanghai MacLean Biochemical Technology Co., Ltd.) was added to the reaction vessel, and then 98 g of polycaprolactone triol (PCL-308; Mn = 850; hydroxyl value = 190-200 KOHmg / g; acid value <1.5) was added to the reaction vessel with stirring. The reaction vessel was heated to 110°C at a heating rate of 15°C / min, and the reaction was stirred for 3 hours. After the reaction was completed, the temperature was lowered to 60°C, and argon was introduced into the reaction vessel for protection. Then, 0.1g of the catalyst dibutyltin dilaurate and 84g of isocyanatepropyltriethoxysilane (ICPTES; 95%; purchased from Shin-Etsu Chemical Co., Ltd.) were added, and the stirring was continued until the -NCO reaction in the system was complete. The reaction was stopped and cooled to room temperature. Then, 225g of epoxy resin (E-44 epoxy resin; epoxy equivalent weight was 210-240g / eq; viscosity was 30000-40000mPa•s; purchased from Nantong Xingchen Synthetic Materials Co., Ltd.) was added thereto with stirring, and the mixture was stirred for 24 hours to obtain a modified epoxy resin.
[0044] Example 2 Preparation of modified epoxy resin:
[0045] 10.5 g of 1,1,1-trimethylolpropane (TMP; analytical grade; purchased from Shanghai MacLean Biochemical Technology Co., Ltd.) was added to the reaction vessel, and then 99 g of polycaprolactone triol (PCL-308; Mn = 850; hydroxyl value = 190-200 KOHmg / g; acid value <1.5) was added to the reaction vessel with stirring. The reaction vessel was heated to 115°C at a heating rate of 15°C / min, and the reaction was stirred for 3 hours. After the reaction was completed, the temperature was lowered to 60°C, and argon was introduced into the reaction vessel for protection. Then, 0.1g of the catalyst dibutyltin dilaurate and 85g of isocyanatepropyltriethoxysilane (ICPTES; 95%; purchased from Shin-Etsu Chemical Co., Ltd.) were added, and the stirring was continued until the -NCO reaction in the system was complete. The reaction was stopped and cooled to room temperature. Then, 240g of epoxy resin (E-44 epoxy resin; epoxy equivalent weight was 210-240g / eq; viscosity was 30000-40000mPa•s; purchased from Nantong Xingchen Synthetic Materials Co., Ltd.) was added thereto with stirring, and the mixture was stirred for 24 hours to obtain a modified epoxy resin.
[0046] Example 3 Preparation of modified epoxy resin:
[0047] 11.2 g of 1,1,1-trimethylolpropane (TMP; analytical grade; purchased from Shanghai MacLean Biochemical Technology Co., Ltd.) was added to the reaction vessel, and then 100 g of polycaprolactone triol (PCL-308; Mn = 850; hydroxyl value = 190-200 KOHmg / g; acid value <1.5) was added to the reaction vessel with stirring. The reaction vessel was heated to 115°C at a heating rate of 15°C / min, and the reaction was stirred for 3 hours. After the reaction was completed, the temperature was lowered to 60°C, and argon was introduced into the reaction vessel for protection. Then, 0.1g of the catalyst dibutyltin dilaurate and 85g of isocyanatepropyltriethoxysilane (ICPTES; 95%; purchased from Shin-Etsu Chemical Co., Ltd.) were added, and the stirring was continued until the -NCO reaction in the system was complete. The reaction was stopped and cooled to room temperature. Then, 250g of epoxy resin (E-44 epoxy resin; epoxy equivalent weight was 210-240g / eq; viscosity was 30000-40000mPa•s; purchased from Nantong Xingchen Synthetic Materials Co., Ltd.) was added thereto with stirring, and the mixture was stirred for 24 hours to obtain a modified epoxy resin.
[0048] Example 4 An acid-resistant adhesive for lead-acid batteries is prepared by mixing component A and component B in a mass ratio of 2.8:1;
[0049] The A component includes the following raw materials in parts by mass:
[0050] 70 parts of the modified epoxy resin prepared in Example 1;
[0051] 15 parts of filler;
[0052] 12 parts of toughening agent;
[0053] 8 parts of diluent;
[0054] 2 parts of defoaming agent;
[0055] The B component, in parts by mass, includes the following raw materials:
[0056] 55 parts of curing agent;
[0057] 5 parts of accelerator;
[0058] 1 part of coupling agent.
[0059] The preparation method of the above acid-resistant adhesive comprises the following steps:
[0060] Weighing raw materials: weigh the raw materials in component A and component B respectively according to the above mass parts;
[0061] Preparation of component A: Add modified epoxy resin to stirring tank A, then add filler and toughening agent, stir and disperse at a speed of 800 r / min for 30 min, then add diluent and defoamer, stir and disperse at 1000 r / min for 30 min, place under vacuum degree -0.1 MPa vacuum degree condition for vacuum degassing for 1 h to obtain component A;
[0062] Preparation of component B: Add curing agent, accelerator and coupling agent to stirring kettle B, and stir and disperse at a speed of 400 r / min for 30 minutes to obtain component B;
[0063] Prepare the acid-resistant adhesive: mix component A and component B in a mass ratio of 2.8:1.
[0064] in:
[0065] a. Filler: The filler is spherical alumina (purchased from Forsman Technology (Beijing) Co., Ltd.), barium sulfate (200 mesh; purchased from Shandong Xiya Chemical Co., Ltd.), and quartz powder (200 mesh; purchased from Shandong Xiya Chemical Co., Ltd.) mixed in a mass ratio of 3:1:1. Among them, the spherical alumina is a mixture of spherical alumina with gradient median particle size, which is a mixture of spherical alumina with a median particle size of 90-110 μm, spherical alumina with a median particle size of 40-70 μm, and spherical alumina with a median particle size of 1.5-3.0 μm in a mass ratio of 5:2:1.
[0066] b. Toughening agent: The toughening agent is amino-terminated liquid nitrile rubber (ATBN; acrylonitrile content 18%), purchased from Shenzhen Jiadida Chemical Co., Ltd.
[0067] c. Diluent: The diluent is X-52 cresol glycidyl ether (hydroxyl value 3.0 mmol / g), purchased from Tianjin Synthetic Materials Industry Research Institute.
[0068] d. Defoaming agent: The defoaming agent is BYK-1794, purchased from BYK Chemical Company of Germany.
[0069] e. Curing agent: The curing agent is NX-2003D, purchased from Cardolite Chemical Co., Ltd. of Germany.
[0070] f. Accelerator: The accelerator is DMP-30 (2,4,6-tris(dimethylaminomethyl)phenol), purchased from Shandong Xiya Chemical Co., Ltd.
[0071] g. Coupling agent: The coupling agent is KH-550, purchased from Shanghai MacLean Biochemical Technology Co., Ltd.
[0072] Example 5 An acid-resistant adhesive for lead-acid batteries is prepared by mixing component A and component B in a mass ratio of 3:1;
[0073] The A component includes the following raw materials in parts by mass:
[0074] 72 parts of the modified epoxy resin prepared in Example 1;
[0075] 18 parts of filler;
[0076] 14 parts of toughening agent;
[0077] 12 parts of diluent;
[0078] 3 parts of defoaming agent;
[0079] The B component, in parts by mass, includes the following raw materials:
[0080] 65 parts of curing agent;
[0081] Accelerator 10 parts;
[0082] 2 parts of coupling agent.
[0083] The preparation method of the above acid-resistant adhesive comprises the following steps:
[0084] Weighing raw materials: weigh the raw materials in component A and component B respectively according to the above mass parts;
[0085] Preparation of component A: Add modified epoxy resin to stirring tank A, then add filler and toughening agent, stir and disperse at a speed of 1000 r / min for 30 minutes, then add diluent and defoamer, stir and disperse at 1200 r / min for 30 minutes, place under vacuum degree -0.1 MPa vacuum degree condition for vacuum degassing for 1 hour to obtain component A;
[0086] Preparation of component B: Add curing agent, accelerator and coupling agent to stirring kettle B, and stir and disperse at a speed of 600 r / min for 30 minutes to obtain component B;
[0087] Prepare the acid-resistant adhesive: mix component A and component B in a mass ratio of 3:1.
[0088] in:
[0089] a. Filler: The filler is spherical alumina (purchased from Forsman Technology (Beijing) Co., Ltd.), barium sulfate (200 mesh; purchased from Shandong Xiya Chemical Co., Ltd.), and quartz powder (200 mesh; purchased from Shandong Xiya Chemical Co., Ltd.) mixed in a mass ratio of 4:2:1. Among them, the spherical alumina is a mixture of spherical alumina with gradient median particle size, which is a mixture of spherical alumina with a median particle size of 90-110 μm, spherical alumina with a median particle size of 40-70 μm, and spherical alumina with a median particle size of 1.5-3.0 μm in a mass ratio of 5:2:1.
[0090] b. Toughening agent: The toughening agent is liquid polysulfide rubber (LP23 type; molecular weight 2500; mercaptan content 2.5%-3.5%), purchased from Toray Industries, Japan.
[0091] c. Diluent: The diluent was LITE-2020, purchased from Cardolite Chemical Co., Ltd.
[0092] d. Defoaming agent: The defoaming agent is BYK-054, purchased from BYK Chemical Company of Germany.
[0093] e. Curing agent: The curing agent is NX-2040, purchased from Cardolite Chemical Co., Ltd. of Germany.
[0094] f. Accelerator: The accelerator is DMP-30 (2,4,6-tris(dimethylaminomethyl)phenol), purchased from Shandong Xiya Chemical Co., Ltd.
[0095] g. Coupling agent: The coupling agent is KH-550, purchased from Shanghai MacLean Biochemical Technology Co., Ltd.
[0096] Example 6 An acid-resistant adhesive for lead-acid batteries, comprising component A and component B mixed in a mass ratio of 3.5:1;
[0097] The A component includes the following raw materials in parts by mass:
[0098] 75 parts of the modified epoxy resin prepared in Example 1;
[0099] 20 parts of filler;
[0100] 15 parts of toughening agent;
[0101] 15 parts of diluent;
[0102] 4 parts of defoamer;
[0103] The B component, in parts by mass, includes the following raw materials:
[0104] 70 parts of curing agent;
[0105] 12 parts of accelerator;
[0106] 4 parts of coupling agent.
[0107] The preparation method of the above acid-resistant adhesive comprises the following steps:
[0108] Weighing raw materials: weigh the raw materials in component A and component B respectively according to the above mass parts;
[0109] Preparation of component A: Add modified epoxy resin to stirring tank A, then add filler and toughening agent, stir and disperse at a speed of 1000 r / min for 30 minutes, then add diluent and defoamer, stir and disperse at 1200 r / min for 30 minutes, place under vacuum degree -0.1 MPa vacuum degree condition for vacuum degassing for 1 hour to obtain component A;
[0110] Preparation of component B: Add curing agent, accelerator and coupling agent to stirring kettle B, and stir and disperse at a speed of 600 r / min for 30 minutes to obtain component B;
[0111] Prepare the acid-resistant adhesive: mix component A and component B in a mass ratio of 3.5:1.
[0112] in:
[0113] a. Filler: The filler is a mixture of spherical alumina (purchased from Forsman Technology (Beijing) Co., Ltd.), barium sulfate (200 mesh; purchased from Shandong Xiya Chemical Co., Ltd.), and quartz powder (200 mesh; purchased from Shandong Xiya Chemical Co., Ltd.) in a mass ratio of 5:2:1. Among them, the spherical alumina is a mixture of spherical alumina with a gradient median particle size, which is a mixture of spherical alumina with a median particle size of 90-110 μm, spherical alumina with a median particle size of 40-70 μm, and spherical alumina with a median particle size of 1.5-3.0 μm in a mass ratio of 5:2:1.
[0114] b. Toughening agent: The toughening agent is amino-terminated liquid nitrile rubber (ATBN; acrylonitrile content 18%), purchased from Shenzhen Jiadida Chemical Co., Ltd.
[0115] c. Diluent: The diluent was LITE-2020, purchased from Cardolite Chemical Co., Ltd.
[0116] d. Defoaming agent: The defoaming agent is BYK-A535, purchased from BYK Chemical Company of Germany.
[0117] e. Curing agent: The curing agent is Ancamine 2280, purchased from Evonik Industries AG, Germany.
[0118] f. Accelerator: The accelerator is DMP-30 (2,4,6-tris(dimethylaminomethyl)phenol), purchased from Shandong Xiya Chemical Co., Ltd.
[0119] g. Coupling agent: The coupling agent is KH-550, purchased from Shanghai MacLean Biochemical Technology Co., Ltd.
[0120] Comparative Example 1 Comparative Example 1 is the control group of Example 5, except that the modified epoxy resin prepared in Example 1 in the raw materials of component A in Example 4 is replaced by epoxy resin (E-44 type epoxy resin; epoxy equivalent is 210-240 g / eq; viscosity is 30000-40000 mPa•s; purchased from Nantong Xingchen Synthetic Materials Co., Ltd.), and the other raw materials and their preparation process remain unchanged, and finally an acid-resistant adhesive is obtained.
[0121] Comparative Example 2 Comparative Example 2 is the control group of Example 5, except that the filler in Example 5 is removed, and the other raw materials and the preparation process remain unchanged, and finally an acid-resistant adhesive is obtained.
[0122] Comparative Example 3 Comparative Example 2 is the control group of Example 5, except that the spherical alumina in the filler in Example 5 is removed, and the other raw materials and the preparation process remain unchanged, and finally an acid-resistant adhesive is obtained.
[0123] In the process of preparing the acid-resistant adhesive of Example 4-Example 6 and Comparative Examples 1-Comparative Examples 3, component A and component B were mixed and stirred for 10 minutes according to the mass ratio to obtain six groups of acid-resistant adhesive solutions. The tensile shear strength and acid resistance of the six batches of acid-resistant adhesive solutions were measured. The specific process is as follows:
[0124] The tensile shear strength was tested with reference to GB / T7124-86, replacing the metal-to-metal overlap in the standard with overlap between selected substrates. The selected substrates were divided into three types, namely lead plate-lead plate (sample A), ABS substrate-ABS substrate (sample B) and EPDM substrate-EPDM substrate (sample C). The thickness of the adhesive layer on the bonding surface was 0.18-0.20mm. The rest of the process remained the same as in the standard. The adhesive layer was cured at room temperature. Six batches of acid-resistant adhesives each corresponded to three groups of test samples, and the tensile shear strength was tested by a testing machine;
[0125] The preparation of the test samples for acid resistance was the same as above. A total of 18 test samples in six batches were immersed in 40% H2SO4 / 25℃ / 168h. After being taken out and dried, the tensile shear strength was tested by a testing machine. The acid resistance was evaluated by the change rate of the tensile shear strength.
[0126] The test results are shown in Table 1 below:
[0127]
[0128] As can be seen from Table 1, the tensile shear strength data of Example 5 and Comparative Examples 1 to 3 show that the filler of the present invention can significantly improve the mechanical strength of the adhesive. The data before and after acid leaching of Example 5 and Comparative Examples 1 to 3 show that the modified epoxy resin prepared by the present invention can significantly improve the acid resistance of the adhesive, and the filler selected by the present invention can improve the acid resistance of the adhesive.
[0129] It should be noted that, in this article, terms such as "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or equipment that includes a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or equipment.
[0130] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the invention, and the scope of the invention is defined by the appended claims and their equivalents.
Claims
1. An acid-resistant adhesive for lead-acid batteries, characterized in that: It is made by mixing component A and component B in a mass ratio of 2.8-3.5:1; The A component includes the following raw materials in parts by mass: 70-75 parts of modified epoxy resin; 15-20 parts of filler; 12-15 parts of toughening agent; 8-15 parts of diluent; 2-4 parts of defoaming agent; The B component, in parts by mass, includes the following raw materials: Curing agent 55-70 parts; 5-12 parts of accelerator; 1-4 parts of coupling agent; The modified epoxy resin is prepared by the following steps: Add polycaprolactone triol to 1,1,1-trimethylolpropane with stirring, heat to 110-115°C, stir and react for 3 hours, cool to 60°C after the reaction is completed, and introduce argon protection, then add dibutyltin dilaurate and isocyanatepropyltriethoxysilane, continue stirring until -NCO in the system reacts completely, stop the reaction, cool to room temperature, stir and add epoxy resin, stir and mix for 24 hours to obtain a modified epoxy resin; The filler is a mixture of spherical alumina, barium sulfate and quartz powder in a mass ratio of 3-5:1-2:1; The spherical alumina is a mixture of spherical alumina with a gradient median particle size, which is a mixture of spherical alumina with a median particle size of 90-110 μm, spherical alumina with a median particle size of 40-70 μm and spherical alumina with a median particle size of 1.5-3.0 μm in a mass ratio of 5:2:1; The usage ratio of the 1,1,1-trimethylolpropane, polycaprolactone triol, dibutyltin dilaurate, isocyanatepropyltriethoxysilane and epoxy resin is 8.5-11.2g:98-100g:0.1g:84-85g:225-250g.
2. The acid-resistant adhesive for lead-acid batteries according to claim 1, characterized in that: The toughening agent is one of amino-terminated liquid nitrile rubber and liquid polysulfide rubber.
3. The acid-resistant adhesive for lead-acid batteries according to claim 1, characterized in that: The diluent is one of X-52 cresol glycidyl ether and LITE-2020.
4. The acid-resistant adhesive for lead-acid batteries according to claim 1, characterized in that: The defoamer is one of BYK-1794, BYK-054 and BYK-A535.
5. The acid-resistant adhesive for lead-acid batteries according to claim 1, characterized in that: The curing agent is one of NX-2003D, NX-2040 and Ancamine2280.
6. The acid-resistant adhesive for lead-acid batteries according to claim 1, characterized in that: The accelerator is DMP-30 (2,4,6-tris(dimethylaminomethyl)phenol).
7. The method for preparing an acid-resistant adhesive for lead-acid batteries according to claim 1, characterized in that: The following steps are involved: Weigh the raw materials in component A and component B respectively in parts by mass, add filler and toughening agent to the modified epoxy resin, stir and disperse at a speed of 800-1000r / min for 30min, then add diluent and defoaming agent, stir and disperse at 1000-1200r / min for 30min, place under vacuum degree of -0.1MPa vacuum degree condition for vacuum degassing for 1h to obtain component A, stir and disperse the curing agent, accelerator and coupling agent at a speed of 400-600r / min for 30min to obtain component B, mix component A and component B in a mass ratio of 2.8-3.5:1 to obtain.
Citation Information
Patent Citations
Lead-acid battery sealant and preparation method thereof
CN104946188B
An epoxy resin sealant, its preparation method and application
CN109439252B
A method for preparing and using a sealant for automated lead-acid batteries.
CN110616057B
Lead-acid storage battery sealing gum
CN102925093A
Lead-acid storage battery sealant and preparation method thereof
CN116554836A