Preparation method and application of novel triarylamine monomer containing quinoline structure and polymer thereof

By introducing a quinoxaline-structured triarylamine monomer into polyamide and polymerizing it with a dicarboxylic acid monomer, the problem of low solubility of polyamide in organic solvents was solved, resulting in a polymer with high solubility and significant electrochromic properties, as well as good thermal stability and cycling stability.

CN117603448BActive Publication Date: 2026-11-10HEILONGJIANG UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311307623.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-10-11
Publication Date
2026-11-10
Estimated Expiration
2043-10-11

AI Technical Summary

Technical Problem

Polyamides have low solubility in organic solvents, resulting in poor film formation, difficulty in processing, small band structure variation, and limited color options.

Method used

A triarylamine monomer with a quinoxaline structure was polymerized with a commercially available diacid monomer to form a polyamide. The solubility and electrochromic properties were improved by designing a DA structure.

Benefits of technology

It improves the solubility and film-forming properties of the polymer, provides significant electrochromic properties with obvious color changes, good thermal stability, and excellent cycling stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117603448B_ABST
    Figure CN117603448B_ABST
Patent Text Reader

Abstract

The application relates to a novel quinoxaline-structure-containing triarylamine monomer and polymer, and a preparation method and application thereof. In order to solve the problems of low solubility in an organic solvent, difficulty in film forming, poor cycle stability, narrow color change range and single function of an existing polyamide material, two hydrogens in a benzene ring para-position of a quinoxaline are subjected to dibromine substitution, a novel quinoxaline-structure-containing triphenylamine precursor is obtained by reacting with 4-methoxy-4'-nitro diphenylamine, a diamine monomer is obtained by reducing the nitro group, and a novel soluble polyamide is formed by polymerization of the diamine monomer with a diacid. Meanwhile, the polymer has excellent electrochromic performance, including excellent cycle stability, fast switching time, high optical contrast and low voltage start. The application is expected to be applied to the fields of intelligent windows, rearview mirrors and electronic tags in the fields of buildings and automobiles.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a triarylamine monomer containing a quinoxaline structure, its polymer, its preparation method, and its application. Background Technology

[0002] Electrochromic materials are a class of materials whose color changes when an electric field is applied. Due to their rich color variations, they are widely used in smart windows, electronic displays, tunable mirrors, and optical devices. Quinoxaline and its derivatives are a class of nitrogen-containing heterocyclic aromatic compounds with high electron affinity, good thermal stability, photochemical stability, and fluorescence properties. Therefore, their application as optoelectronic materials has attracted much attention. This patent introduces a monomer structure containing this unit into a polyamide structure, aiming to obtain a novel multifunctional polyamide with strong stability and combining electrochromic and other electrochemical properties. Summary of the Invention

[0003] To address the problems of poor film formation, difficult processing, limited bandgap variation, and limited color of polyamides due to their low solubility in organic solvents, this invention proposes a triphenylamine polymer containing a quinoxaline structure, its preparation method, and its application in electrochromic processes. The triarylamine monomer containing the quinoxaline structure is polymerized with commercially available diacid monomers (diacids can be 1,4-cyclohexanedicarboxylic acid, 4,4'-diphenyl ether dicarboxylic acid, terephthalic acid, 4,4'-dicarboxylic acid biphenyl sulfone, phthalic acid, adipic acid, 2,6-naphthalenedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 4,4'-dicarboxylic acid biphenyl sulfone, etc.).

[0004] The structural formula of polyamide P1 obtained by polymerizing a triarylamine monomer containing a quinoxaline structure with 1,4-cyclohexanedicarboxylic acid is as follows:

[0005] The structural formula of polyamide P2 obtained by polymerizing a triarylamine monomer containing a quinoxaline structure with 4,4'-diphenyl ether dicarboxylic acid is as follows:

[0006] The structural formula of polyamide P3 obtained by polymerizing a triarylamine monomer containing a quinoxaline structure with terephthalic acid is as follows:

[0007] The structural formula of polyamide P4 obtained by polymerizing a triarylamine monomer containing a quinoxaline structure with 4,4'-dicarboxylic acid biphenyl sulfone is as follows: In the above structural formula, n is an integer from 10 to 16.

[0008] The method for preparing triarylamine polymers containing a quinoxaline structure according to the present invention is carried out according to the following steps:

[0009] I. Synthesis of N 1 N 1 '-(dibenzo[a,c]phenazine-10,13-diyl)bis(N 1 (4-Methoxyphenyl)benzene-1,4-diamine) monomer:

[0010] ① Under a nitrogen atmosphere, a mixture of 4-methoxyaniline, 4-fluoronitrobenzene, triethylamine and anhydrous dimethyl sulfoxide was placed in a three-necked flask and stirred at 90°C for 36 hours. The mixture was then refluxed. After the reaction was completed, the reaction solution was cooled to room temperature and poured into cold water to precipitate. The precipitate was filtered to obtain an orange solid crude product. The product was then recrystallized, and an orange needle-like crystalline product was filtered out. The product was then dried under vacuum to obtain 4-methoxy-4'-nitrodiphenylamine, which was named M1.

[0011] The volume ratio of anhydrous dimethyl sulfoxide to the molar amount of 4-methoxyaniline in step 1① is (100-150) mL: 13 mmol.

[0012] The molar ratio of 4-fluoronitrobenzene to triethylamine in step 1① is 1:2;

[0013] The molar ratio of 4-fluoronitrobenzene to 4-methoxyaniline in step 1① is 2:1;

[0014] The ratio of the volume of cold water to the amount of 4-methoxyaniline monomer mentioned in step 1① is (400-450) mL: 10 mmol;

[0015] The temperature of the cold water mentioned in step 1① is 0~5℃;

[0016] The vacuum drying temperature in step 1① is 45℃, the vacuum drying time is 48 hours, and the vacuum drying pressure is -30~-29KPa;

[0017] ② Under a nitrogen atmosphere, anhydrous ethanol and 4,7-dibromobenzothiadiazole were added to a three-necked flask. The reaction mixture was placed in an ice-water bath, and sodium borohydride was added in batches while stirring. The reaction mixture was then placed in an ice bath with stirring. After the gas stopped escaping, the ice bath was removed, and the reaction mixture was stirred at room temperature for 20 hours. After the reaction was complete, the ethanol was removed by rotary evaporation, followed by extraction. The organic phase was then washed with brine, and anhydrous MgSO4 was added to the organic phase for drying. The organic phase was then filtered, the solvent was removed by vacuum evaporation, and the mixture was dried in a vacuum oven to obtain a pale yellow solid product, 3,6-dibromo-1,2-phenylenediamine monomer, named M2.

[0018] The volume ratio of anhydrous ethanol to the amount of 4,7-dibromobenzothiadiazole in step 1② is (50-80) mL: 15 mmol.

[0019] The molar ratio of 4,7-dibromobenzothiadiazole to sodium borohydride in step 1② is 3:1;

[0020] The volume ratio of anhydrous ethanol to sodium borohydride in step 1② is (50-80) mL: 0.51 mmol;

[0021] The vacuum drying temperature described in step 1② is 55℃, the vacuum drying time is 48 hours, and the vacuum drying pressure is -30~-29KPa;

[0022] ③ At room temperature, M2 and phenanthrene-9,10-dione were dissolved in acetic acid. A precipitate gradually formed in the reaction flask. The reaction mixture was refluxed at 100°C for 24 hours. After the reaction was completed, it was cooled to room temperature and neutralized with sodium bicarbonate. The precipitate was collected by filtration and washed with ethanol. The crystallized product was placed in a vacuum drying oven to obtain a yellow solid product, 10,13-dibromodibenzo[a,c]phenazine, named M3.

[0023] The molar ratio of M2 to phenanthrene-9,10-dione mentioned in step 1③ is 1:1;

[0024] The volume ratio of acetic acid to the amount of M2 in step 1③ is (50-80) mL: 2.1 mmol;

[0025] The volume ratio of acetic acid to phenanthrene-9,10-dione in step 1③ is (50-80) mL: 2.1 mmol;

[0026] The mass ratio of sodium bicarbonate to water in step 1③ is 4g:100mL;

[0027] The vacuum drying temperature described in step 1③ is 45℃, the vacuum drying time is 36 hours, and the vacuum drying pressure is -30~-29KPa;

[0028] ④ Under a nitrogen atmosphere, M1, M3, 18-crown-6 ether, copper powder, potassium carbonate, and o-dichlorobenzene were placed in a three-necked flask and heated to 180°C. The mixture was then refluxed and reacted for 36 hours. After the reaction was completed, the mixture was filtered while hot, and the filtrate was poured into petroleum ether to precipitate a brick-red precipitate. The brick-red precipitate was purified by column chromatography, and the purified product was vacuum dried to obtain a brick-red powder, which was named M4.

[0029] The molar ratio of M1 to M3 mentioned in step 1, ④ is 1:2.5;

[0030] The molar ratio of M1 to 18-crown-6 ether in step 1④ is 1:1;

[0031] In step 1, ④, the molar ratio of M1 to copper powder is 1:8;

[0032] In step 1, ④, the molar ratio of M1 to potassium carbonate is 1:8;

[0033] The volume ratio of o-dichlorobenzene to the amount of M1 in step 1④ is (20–30) mL: 1 mmol;

[0034] The volume ratio of petroleum ether to the amount of M1 in step 1, ④ is (150–200) mL: 1 mmol;

[0035] The vacuum drying temperature described in step 1④ is 45℃, the vacuum drying time is 48 hours, and the vacuum drying pressure is -30~-29KPa;

[0036] ⑤ Under a nitrogen atmosphere, M4, anhydrous ethanol, and Pd / C were added to a three-necked flask. When the temperature reached 80°C, hydrazine hydrate was added dropwise to the flask using a constant-pressure funnel at a rate of 1-2 drops per second. The temperature was raised to reflux, and the reaction was allowed to proceed for 12 hours. After the reaction was complete, the palladium on carbon was removed by hot filtration. The filtrate was poured into distilled water, and an appropriate amount of sodium chloride was added to precipitate a solid. The solid phase was filtered off and washed with ethanol to obtain a pale blue precipitate, which was then dried under vacuum to obtain N. 1 N 1 '-(dibenzo[a,c]phenazine-10,13-diyl)bis(N 1 -(4-methoxyphenyl)benzene-1,4-diamine), named M5;

[0037] The volume ratio of anhydrous ethanol to the amount of M4 in step 1, ⑤ is (80-100) mL: 14 mmol;

[0038] The mass ratio of Pd / C to the molar amount of M4 mentioned in step 1, ⑤ is (1-1.5) g: 7 mmol;

[0039] The volume ratio of hydrazine hydrate to the amount of M4 in step 1, ⑤ is 3 mL: 1 mmol;

[0040] In step 1, ⑤, the heating rate when the solution is refluxed is 10°C per minute.

[0041] The temperature of the cold water mentioned in step 1, ⑤ is 0℃;

[0042] The volume ratio of the filtrate to cold water in step 1, ⑤ is 1:5;

[0043] In step 1, ⑤, the Pd / C is a material with palladium supported on a carbon support, and the mass fraction of Pd in ​​the Pd / C is 10%.

[0044] The vacuum drying temperature described in step 1, ⑤ is 30℃, the vacuum drying time is 48 to 64 hours, and the vacuum drying pressure is -30 to -29 kPa.

[0045] II. Preparation of polyamides containing quinoxalin and triarylamine groups:

[0046] The mixture contains M5, diacid monomers (1,4-cyclohexanedicarboxylic acid, 4,4'-diphenyl ether dicarboxylic acid, terephthalic acid, 4,4'-dicarboxylic biphenyl sulfone), triphenyl phosphite, calcium chloride, pyridine, and N-methylpyrrolidone. The mixture is then stirred at 120°C for 8 hours. After cooling to room temperature, methanol is added, the precipitate is collected by filtration, and the precipitate is thoroughly washed with methanol. Finally, the precipitate is extracted separately with methanol and acetone using a Soxhlet extractor. The molar ratio of M5 to the diacid monomer in step two is 1:1; The volume ratio of triphenyl phosphite to the molar amount of M5 in step two is 1.1 mL: 1 mmol;

[0047] The volume ratio of pyridine to the molar amount of M5 in step two is 0.6 mL: 1 mmol;

[0048] The volume ratio of N-methylpyrrolidone to the amount of M5 in step two is 3 mL: 1 mmol;

[0049] The mass ratio of calcium chloride to N-methylpyrrolidone in step two is 0.15 g : 1.5 mL;

[0050] In step two, the volume ratio of methanol and acetone to the molar amount of M5 is 250 mL: 1 mmol.

[0051] The dicarboxylic acid monomers are 1,4-cyclohexanedicarboxylic acid, 4,4'-diphenyl ether dicarboxylic acid, terephthalic acid, and 4,4'-dicarboxylic biphenyl sulfone, and the polymers prepared are P1, P2, P3, and P4, respectively.

[0052] The triarylamine polyamide containing the quinoxaline structure in this invention can be used as an electrochromic active layer in multiple fields such as smart windows and rearview mirrors.

[0053] This invention aims to prepare polyamides with excellent chemical stability and good electrochromic properties, addressing the problems of poor processability and cycling stability leading to short service life. By designing and introducing a triphenylamine structure into the polymer, the original poor solubility of the polymer can be improved, facilitating coating processing. Furthermore, it provides the polymer with nitrogen atoms as redox centers, endowing it with electrochromic properties. Quinoxaline derivatives possess high electron affinity and good thermal stability, and can form a DA structure with triarylamines, resulting in a lower band structure and higher color absorbance, which helps improve the overall electrochromic performance of the polymer. Combining these advantages, a triarylamine polyamide containing a quinoxaline structure is prepared, exhibiting strong antioxidant properties, good solubility, and film-forming properties. The invention also provides a method for preparing and applying this triarylamine polyamide containing a quinoxaline structure.

[0054] The present invention has the following beneficial effects:

[0055] I. Triarylamine compounds typically have a non-planar molecular configuration. The central nitrogen atom loses electrons under an electric field to form a cationic free radical. Due to the strong superelectron conjugation effect, the free radical exhibits high stability. This free radical characteristic gives triphenylamine and its derivatives excellent hole transport properties and high mobility. The triarylamine polymer containing the quinoxaline structure in this invention has a lower energy band due to the introduction of the quinoxaline group, resulting in a more pronounced color change due to increased absorbance. Simultaneously, the introduction of the propeller-shaped triarylamine unit improves the polymer's solubility. Therefore, the triarylamine polymer containing the quinoxaline structure prepared in this invention increases the solubility of the polyamide by introducing two triphenylamine structures into one monomer unit, making it easily soluble in polar solvents, with 0.1–0.2 g soluble per 1 mL of organic solvent. The quinoxaline structure provides an electron-withdrawing group (A), which forms a DA structure with the electron-donating group (D) of triphenylamine, causing a decrease in energy level and a more pronounced color change. Due to the increased thermal stability caused by the rigid structure, the thermal decomposition temperature of the triarylamine polymers containing the quinoxaline structure is in the range of 398-432℃ when the weight loss is 10% under a nitrogen atmosphere. When the temperature is heated to 800℃, the carbon residue of the above polymers is greater than 63%.

[0056] II. The polymer of this invention has excellent electrochromic properties.

[0057] Electrochromism is a phenomenon in which the color or optical properties of a material are reversibly changed by applying an electric field. Under the influence of an applied electric field, the movement of electrons or the transfer of charge leads to changes in the molecular structure or electronic energy levels of the material, thereby causing a color change. The triarylamine polyamide of this invention, containing quinoxaline directly bonded to nitrogen atoms, possesses charge transport active sites. By applying a certain voltage to the polymer, electron transfer occurs within the polymer, resulting in a color change. The polymer of this invention exhibits significant color changes within a voltage range of 0.5–1.4 V; the coloring time is 3.0–3.8 s, and the bleaching time is 1.0–2.5 s; it is deep blue when colored and nearly colorless when bleached, exhibiting high contrast during electrochromism, reaching up to 50%; the triarylamine polyamide containing quinoxaline directly bonded to triphenylamine prepared by this invention shows good cycling stability, with no significant change in optical contrast after 900 cycles, demonstrating excellent electrochromic stability. Attached Figure Description

[0058] Figure 1 The infrared spectra of the triphenylamine polymers containing quinoxaline structures prepared in Examples 1, 2, 3, and 4 are shown.

[0059] Figure 2 N used in the preparation of the polymer in Example 1 1 N 1 '-(dibenzo[a,c]phenazine-10,13-diyl)bis(N 1 The proton NMR spectrum of (4-methoxyphenyl)benzene-1,4-diamine monomer;

[0060] Figure 3-6 The above are the proton NMR spectra of the triarylamine polymers containing quinoxaline structures prepared in Examples 1 to 4;

[0061] Figure 7 Cyclic voltammetry diagrams of the triarylamine polyamide polymers containing quinoxaline structures prepared in Examples 1 to 4;

[0062] Figure 8-11 Electrochromic images of the triarylamine polymers containing quinoxaline structures prepared in Examples 1 to 4;

[0063] Figure 12 Thermogravimetric curves of the triarylamine polymers containing quinoxaline structures prepared in Examples 1 to 4 are shown.

[0064] Figure 13-16 Electrochromic stability diagrams of the triarylamine polymers containing quinoxaline structures prepared in Examples 1 to 4;

[0065] Figure 17-20Electrochromic response time diagrams of the triarylamine polymers containing quinoxaline structures prepared in Examples 1 to 4; Detailed Implementation

[0066] The technical solution of the present invention is not limited to the specific embodiments listed below, but also includes any reasonable combination of the specific embodiments.

[0067] Specific Implementation Method 1: In this implementation method, the triaromatic amine polyamides P1, P2, P3, and P4 containing the quinoxaline structure are as follows:

[0068] The structural formula of triarylamine polyamide P1 containing a quinoxaline structure is as follows:

[0069] The structural formula of triarylamine polyamide P2 containing the quinoxaline structure is as follows:

[0070] The structural formula of triarylamine polyamide P3 containing the quinoxaline structure is as follows:

[0071] The structural formula of triarylamine polyamide P4 containing the quinoxaline structure is as follows: In the formula, n is an integer from 10 to 16.

[0072] This embodiment has the following beneficial effects:

[0073] 1. In this embodiment, a triarylamine moiety is introduced into the polyamide, thereby increasing the solubility of the polyamide. Due to its propeller structure, the triarylamine structure is easily soluble in polar solvents, and 0.1 to 0.2 grams of the polymer can be dissolved in 1 ml of polar solution.

[0074] II. The polymer of this invention has excellent electrochromic properties.

[0075] The present invention relates to a triarylamine polyamide polymer containing quinoxaline directly bonded to a nitrogen atom, which contains active sites for electron transport and electron transition. When a certain voltage is applied to the polymer, electron transitions occur within the polymer, resulting in a color change. The polymer of the present invention exhibits significant color changes within a voltage range of 0.5–1.4 V; the coloring time is 3.0–3.8 s, and the bleaching time is 1.0–2.5 s; it is deep blue when colored and nearly colorless when bleached, exhibiting high contrast during electrochromic reaction, up to 50%; the polyamide containing quinoxaline directly bonded to a triarylamine prepared by the present invention demonstrates good cycling stability. After 900 cycles, the optical contrast remains essentially unchanged, with optimal cycling stability reaching 1500 cycles while retaining 80% of the original optical contrast, exhibiting excellent electrochromic stability.

[0076] Specific Implementation Method Two: The preparation method of the triarylamine polyamide containing the quinoxaline structure in this implementation method is carried out according to the following steps:

[0077] I. Synthesis of N 1 N 1 '-(dibenzo[a,c]phenazine-10,13-diyl)bis(N 1 (4-Methoxyphenyl)benzene-1,4-diamine) monomer:

[0078] ① Under a nitrogen atmosphere, a mixture of 4-methoxyaniline, 4-fluoronitrobenzene, triethylamine and anhydrous dimethyl sulfoxide was placed in a three-necked flask and stirred at 90°C for 36 hours. The mixture was then refluxed. After the reaction was completed, the reaction solution was cooled to room temperature and poured into cold water to precipitate. The precipitate was filtered to obtain an orange solid crude product. The product was then recrystallized, and an orange needle-like crystalline product was filtered out. The product was then dried under vacuum to obtain 4-methoxy-4'-nitrodiphenylamine, which was named M1.

[0079] The volume ratio of anhydrous dimethyl sulfoxide to the molar amount of 4-methoxyaniline in step 1① is (100-150) mL: 13 mmol.

[0080] The molar ratio of 4-fluoronitrobenzene to triethylamine in step 1① is 1:2;

[0081] The molar ratio of 4-fluoronitrobenzene to 4-methoxyaniline in step 1① is 2:1;

[0082] The ratio of the volume of cold water to the amount of 4-methoxyaniline monomer mentioned in step 1① is (400-450) mL: 10 mmol; The temperature of the cold water is 0–5℃;

[0083] The temperature of the cold water mentioned in step 1① is 0~5℃; the temperature of vacuum drying is 45℃, the vacuum drying time is 48 hours, and the vacuum drying pressure is -30~-29KPa;

[0084] ② Under a nitrogen atmosphere, anhydrous ethanol and 4,7-dibromobenzothiadiazole were added to a three-necked flask. The reaction mixture was placed in an ice-water bath, and sodium borohydride was added in batches while stirring. The reaction mixture was then placed in an ice bath with stirring. After the gas stopped escaping, the ice bath was removed, and the reaction mixture was stirred at room temperature for 20 hours. After the reaction was complete, the ethanol was removed by rotary evaporation, followed by extraction. The organic phase was then washed with brine, and anhydrous MgSO4 was added to the organic phase for drying. The organic phase was then filtered, the solvent was removed by vacuum evaporation, and the mixture was dried in a vacuum oven to obtain a pale yellow solid product, 3,6-dibromo-1,2-phenylenediamine monomer, named M2.

[0085] The volume ratio of anhydrous ethanol to the amount of 4,7-dibromobenzothiadiazole in step 1② is (50-80) mL: 15 mmol.

[0086] The molar ratio of 4,7-dibromobenzothiadiazole to sodium borohydride in step 1② is 3:1;

[0087] The volume ratio of anhydrous ethanol to sodium borohydride in step 1② is (50-80) mL: 0.51 mmol;

[0088] The vacuum drying temperature described in step 1② is 55℃, the vacuum drying time is 48 hours, and the vacuum drying pressure is -30~-29KPa;

[0089] ③ At room temperature, M2 and phenanthrene-9,10-dione were dissolved in acetic acid. A precipitate gradually formed in the reaction flask. The reaction mixture was refluxed at 100°C for 24 hours. After the reaction was completed, it was cooled to room temperature and neutralized with sodium bicarbonate. The precipitate was collected by filtration and washed with ethanol. The crystallized product was placed in a vacuum drying oven to obtain a yellow solid product, 10,13-dibromodibenzo[a,c]phenazine, named M3.

[0090] The molar ratio of M2 to phenanthrene-9,10-dione mentioned in step 1③ is 1:1;

[0091] The volume ratio of acetic acid to the amount of M2 in step 1③ is (50-80) mL: 2.1 mmol;

[0092] The volume ratio of acetic acid to phenanthrene-9,10-dione in step 1③ is (50-80) mL: 2.1 mmol;

[0093] The mass ratio of sodium bicarbonate to water in step 1③ is 4g:100mL;

[0094] The vacuum drying temperature described in step 1③ is 45℃, the vacuum drying time is 36 hours, and the vacuum drying pressure is -30~-29KPa;

[0095] ④ Under a nitrogen atmosphere, M1, M3, 18-crown-6 ether, copper powder, potassium carbonate, and o-dichlorobenzene were placed in a three-necked flask and heated to 180°C. The mixture was then refluxed and reacted for 36 hours. After the reaction was completed, the mixture was filtered while hot, and the filtrate was poured into petroleum ether to precipitate a brick-red precipitate. The brick-red precipitate was purified by column chromatography, and the purified product was vacuum dried to obtain a brick-red powder, which was named M4.

[0096] The molar ratio of M1 to M3 mentioned in step 1, ④ is 1:2.5;

[0097] The molar ratio of M1 to 18-crown-6 ether in step 1④ is 1:1;

[0098] In step 1, ④, the molar ratio of M1 to copper powder is 1:8;

[0099] In step 1, ④, the molar ratio of M1 to potassium carbonate is 1:8;

[0100] The volume ratio of o-dichlorobenzene to the amount of M1 in step 1④ is (20–30) mL: 1 mmol;

[0101] The volume ratio of petroleum ether to the amount of M1 in step 1, ④ is (150–200) mL: 1 mmol;

[0102] The vacuum drying temperature described in step 1④ is 45℃, the vacuum drying time is 48 hours, and the vacuum drying pressure is -30~-29KPa;

[0103] ⑤ Under a nitrogen atmosphere, M4, anhydrous ethanol, and Pd / C were added to a three-necked flask. When the temperature reached 80°C, hydrazine hydrate was added dropwise to the flask using a constant-pressure funnel at a rate of 1-2 drops per second. The temperature was raised to reflux, and the reaction was allowed to proceed for 12 hours. After the reaction was complete, the palladium on carbon was removed by hot filtration. The filtrate was poured into distilled water, and an appropriate amount of sodium chloride was added to precipitate a solid. The solid phase was filtered off and washed with ethanol to obtain a pale blue precipitate, which was then dried under vacuum to obtain N. 1 N 1 '-(dibenzo[a,c]phenazine-10,13-diyl)bis(N 1 -(4-methoxyphenyl)benzene-1,4-diamine), named M5;

[0104] The volume ratio of anhydrous ethanol to the amount of M4 in step 1, ⑤ is (80-100) mL: 14 mmol;

[0105] The mass ratio of Pd / C to the molar amount of M4 mentioned in step 1, ⑤ is (1-1.5) g: 7 mmol;

[0106] The volume ratio of hydrazine hydrate to the amount of M4 in step 1, ⑤ is 3 mL: 1 mmol;

[0107] In step 1, ⑤, the heating rate when the solution is refluxed is 10°C per minute.

[0108] The volume ratio of the filtrate to cold water in step 1, ⑤ is 1:5;

[0109] In step 1, ⑤, the Pd / C is a material with palladium supported on a carbon support, and the mass fraction of Pd in ​​the Pd / C is 10%.

[0110] The vacuum drying temperature described in step 1, ⑤ is 30℃, the vacuum drying time is 48 to 64 hours, and the vacuum drying pressure is -30 to -29 kPa.

[0111] II. Preparation of polyamides containing quinoxalin and triarylamine groups:

[0112] The mixture contains M5, diacid monomers (1,4-cyclohexanedicarboxylic acid, 4,4'-diphenyl ether dicarboxylic acid, terephthalic acid, 4,4'-dicarboxylic biphenyl sulfone), triphenyl phosphite, calcium chloride, pyridine, and N-methylpyrrolidone. The mixture is then stirred at 120°C for 8 hours. After cooling to room temperature, methanol is added, the precipitate is collected by filtration, and the precipitate is thoroughly washed with methanol. Finally, the precipitate is extracted separately with methanol and acetone using a Soxhlet extractor.

[0113] The molar ratio of M5 to the diacid monomer in step two is 1:1;

[0114] The volume ratio of triphenyl phosphite to the molar amount of M5 in step two is 1.1 mL: 1 mmol;

[0115] The volume ratio of pyridine to the molar amount of M5 in step two is 0.6 mL: 1 mmol;

[0116] The volume ratio of N-methylpyrrolidone to the amount of M5 in step two is 3 mL: 1 mmol;

[0117] The mass ratio of calcium chloride to N-methylpyrrolidone in step two is 0.15 g : 1.5 mL;

[0118] In step two, the volume ratio of methanol and acetone to the molar amount of M5 is 250 mL: 1 mmol.

[0119] In this implementation method, step 1④ uses a thin-layer chromatography method with a solvent of ethyl acetate and petroleum ether in a volume ratio of 1:4.

[0120] The dicarboxylic acid monomers obtained in this embodiment are 1,4-cyclohexanedicarboxylic acid, 4,4'-diphenyl ether dicarboxylic acid, terephthalic acid, and 4,4'-dicarboxylic biphenyl sulfone.

[0121] Specific Implementation Method 3: This implementation method describes the application of triarylamine polyamide polymers containing quinoxaline structures as electrochromic layers in electrochromic devices.

[0122] Specific Implementation Method Four: This implementation method differs from Specific Implementation Method Three in that the application of the triarylamine polyamide polymer containing a quinoxaline structure as the electrochromic layer in the electrochromic device is carried out according to the following steps: The triarylamine polyamide polymer containing a quinoxaline structure is used as the electrochromic layer in the electrochromic device. The electrochromic layer is coated on a conductive substrate to prepare an electrochromic device. The electrochromic layer produces electrochromic changes under the action of an external electric field. Everything else is the same as in Specific Implementation Method Three.

[0123] Specific Implementation Method Five: This implementation method differs from Specific Implementation Methods Three or Four in that the conductive substrate is conductive glass. Other steps and parameters are the same as in Specific Implementation Methods Three or Four.

[0124] Specific Implementation Method Six: This implementation method differs from Specific Implementation Methods Three to Five in that the voltage of the applied electric field is 0 to 1.50V. Other steps and parameters are the same as in Specific Implementation Methods Three to Six.

[0125] The beneficial effects of the present invention are verified using the following embodiments:

[0126] Example 1: The structural formulas of triarylamine polyamide P1 containing the quinoxaline structure are as follows: In the formula, n is 11.

[0127] I. Synthesis of N 1 N 1 '-(dibenzo[a,c]phenazine-10,13-diyl)bis(N 1 (4-Methoxyphenyl)benzene-1,4-diamine) monomer:

[0128] ① Under a nitrogen atmosphere, a mixture of 4-methoxyaniline, 4-fluoronitrobenzene, triethylamine and anhydrous dimethyl sulfoxide was placed in a three-necked flask and stirred at 90°C for 36 hours. The mixture was then refluxed. After the reaction was completed, the reaction solution was cooled to room temperature and poured into cold water to precipitate. The precipitate was filtered to obtain an orange solid crude product. The product was then recrystallized, and an orange needle-like crystalline product was filtered out. The product was then dried under vacuum to obtain 4-methoxy-4'-nitrodiphenylamine, which was named M1.

[0129] The volume ratio of anhydrous dimethyl sulfoxide to the molar amount of 4-methoxyaniline in step 1① is (100-150) mL: 13 mmol.

[0130] The molar ratio of 4-fluoronitrobenzene to triethylamine in step 1① is 1:2;

[0131] The molar ratio of 4-fluoronitrobenzene to 4-methoxyaniline in step 1① is 2:1;

[0132] The ratio of the volume of cold water to the amount of 4-methoxyaniline monomer mentioned in step 1① is (400-450) mL: 10 mmol;

[0133] The temperature of the cold water mentioned in step 1① is 0~5℃;

[0134] The vacuum drying temperature in step 1① is 45℃, the vacuum drying time is 48 hours, and the vacuum drying pressure is -30~-29KPa;

[0135] ② Under a nitrogen atmosphere, anhydrous ethanol and 4,7-dibromobenzothiadiazole were added to a three-necked flask. The reaction mixture was placed in an ice-water bath, and sodium borohydride was added in batches while stirring. The reaction mixture was then placed in an ice bath with stirring. After the gas stopped escaping, the ice bath was removed, and the reaction mixture was stirred at room temperature for 20 hours. After the reaction was complete, the ethanol was removed by rotary evaporation, followed by extraction. The organic phase was then washed with brine, and anhydrous MgSO4 was added to the organic phase for drying. The organic phase was then filtered, the solvent was removed by vacuum evaporation, and the mixture was dried in a vacuum oven to obtain a pale yellow solid product, 3,6-dibromo-1,2-phenylenediamine monomer, named M2.

[0136] The volume ratio of anhydrous ethanol to the amount of 4,7-dibromobenzothiadiazole in step 1② is (50-80) mL: 15 mmol.

[0137] The molar ratio of 4,7-dibromobenzothiadiazole to sodium borohydride in step 1② is 3:1;

[0138] The volume ratio of anhydrous ethanol to sodium borohydride in step 1② is (50-80) mL: 0.51 mmol;

[0139] The vacuum drying temperature described in step 1② is 55℃, the vacuum drying time is 48 hours, and the vacuum drying pressure is -30~-29KPa;

[0140] ③ At room temperature, M2 and phenanthrene-9,10-dione were dissolved in acetic acid. A precipitate gradually formed in the reaction flask. The reaction mixture was refluxed at 100°C for 24 hours. After the reaction was completed, it was cooled to room temperature and neutralized with sodium bicarbonate. The precipitate was collected by filtration and washed with ethanol. The crystallized product was placed in a vacuum drying oven to obtain a yellow solid product, 10,13-dibromodibenzo[a,c]phenazine, named M3.

[0141] The molar ratio of M2 to phenanthrene-9,10-dione mentioned in step 1③ is 1:1;

[0142] The volume ratio of acetic acid to the amount of M2 in step 1③ is (50-80) mL: 2.1 mmol;

[0143] The volume ratio of acetic acid to phenanthrene-9,10-dione in step 1③ is (50-80) mL: 2.1 mmol;

[0144] The mass ratio of sodium bicarbonate to water in step 1③ is 4g:100mL;

[0145] The vacuum drying temperature described in step 1③ is 45℃, the vacuum drying time is 36 hours, and the vacuum drying pressure is -30~-29KPa;

[0146] ④ Under a nitrogen atmosphere, M1, M3, 18-crown-6 ether, copper powder, potassium carbonate, and o-dichlorobenzene were placed in a three-necked flask and heated to 180°C. The mixture was then refluxed and reacted for 36 hours. After the reaction was completed, the mixture was filtered while hot, and the filtrate was poured into petroleum ether to precipitate a brick-red precipitate. The brick-red precipitate was purified by column chromatography, and the purified product was vacuum dried to obtain a brick-red powder, which was named M4.

[0147] The molar ratio of M1 to M3 mentioned in step 1, ④ is 1:2.5;

[0148] The molar ratio of M1 to 18-crown-6 ether in step 1④ is 1:1;

[0149] In step 1, ④, the molar ratio of M1 to copper powder is 1:8;

[0150] In step 1, ④, the molar ratio of M1 to potassium carbonate is 1:8;

[0151] The volume ratio of o-dichlorobenzene to the amount of M1 in step 1④ is (20–30) mL: 1 mmol;

[0152] The volume ratio of petroleum ether to the amount of M1 in step 1, ④ is (150–200) mL: 1 mmol;

[0153] The vacuum drying temperature described in step 1④ is 45℃, the vacuum drying time is 48 hours, and the vacuum drying pressure is -30~-29KPa;

[0154] ⑤ Under a nitrogen atmosphere, M4, anhydrous ethanol, and Pd / C were added to a three-necked flask. When the temperature reached 80°C, hydrazine hydrate was added dropwise to the flask using a constant-pressure funnel at a rate of 1–2 drops per second. The temperature was raised to reflux, and the reaction was allowed to proceed for 12 hours. After the reaction was complete, the palladium on carbon was removed by hot filtration. The filtrate was poured into distilled water, and an appropriate amount of sodium chloride was added to precipitate a solid. The solid phase was filtered off and washed with ethanol to obtain a pale blue precipitate, which was then dried under vacuum to obtain N. 1 N 1 '-(dibenzo[a,c]phenazine-10,13-diyl)bis(N 1 -(4-methoxyphenyl)benzene-1,4-diamine), named M5;

[0155] The volume ratio of anhydrous ethanol to the amount of M4 in step 1, ⑤ is (80-100) mL: 14 mmol;

[0156] The mass ratio of Pd / C to the molar amount of M4 mentioned in step 1, ⑤ is (1-1.5) g: 7 mmol;

[0157] The volume ratio of hydrazine hydrate to the amount of M4 in step 1, ⑤ is 3 mL: 1 mmol;

[0158] In step 1, ⑤, the heating rate when the solution is refluxed is 10°C per minute.

[0159] The temperature of the cold water mentioned in step 1, ⑤ is 0℃;

[0160] The volume ratio of the filtrate to cold water in step 1, ⑤ is 1:5;

[0161] In step 1, ⑤, the Pd / C is a material with palladium supported on a carbon support, and the mass fraction of Pd in ​​the Pd / C is 10%.

[0162] The vacuum drying temperature described in step 1, ⑤ is 30℃, the vacuum drying time is 48 to 64 hours, and the vacuum drying pressure is -30 to -29 kPa.

[0163] II. Preparation of polyamides containing quinoxalin and triarylamine groups:

[0164] A mixture containing M5, 1,4-cyclohexanedicarboxylic acid, triphenyl phosphite, calcium chloride, pyridine, and N-methylpyrrolidone was stirred at 120°C for 8 hours. After cooling to room temperature, methanol was added, the precipitate was collected by filtration, and the mixture was thoroughly washed with methanol. Finally, the polymer P1 was obtained by extraction with methanol and acetone using a Soxhlet extractor.

[0165] The molar ratio of M5 to the diacid monomer in step two is 1:1;

[0166] The volume ratio of triphenyl phosphite to the molar amount of M5 in step two is 1.1 mL: 1 mmol;

[0167] The volume ratio of pyridine to the molar amount of M5 in step two is 0.6 mL: 1 mmol;

[0168] The volume ratio of N-methylpyrrolidone to the amount of M5 in step two is 3 mL: 1 mmol;

[0169] The mass ratio of calcium chloride to N-methylpyrrolidone in step two is 0.15 g : 1.5 mL;

[0170] In step two, the volume ratio of methanol and acetone to the molar amount of M5 is 250 mL: 1 mmol.

[0171] Example 2: The structural formulas of triarylamine polyamide P2 containing the quinoxaline structure are as follows: In the formula, n is 10.

[0172] I. Synthesis of N 1 N 1 '-(dibenzo[a,c]phenazine-10,13-diyl)bis(N 1 (4-Methoxyphenyl)benzene-1,4-diamine) monomer:

[0173] ① Under a nitrogen atmosphere, a mixture of 4-methoxyaniline, 4-fluoronitrobenzene, triethylamine and anhydrous dimethyl sulfoxide was placed in a three-necked flask and stirred at 90°C for 36 hours. The mixture was then refluxed. After the reaction was completed, the reaction solution was cooled to room temperature and poured into cold water to precipitate. The precipitate was filtered to obtain an orange solid crude product. The product was then recrystallized, and an orange needle-like crystalline product was filtered out. The product was then dried under vacuum to obtain 4-methoxy-4'-nitrodiphenylamine, which was named M1.

[0174] The volume ratio of anhydrous dimethyl sulfoxide to the molar amount of 4-methoxyaniline in step 1① is (100-150) mL: 13 mmol.

[0175] The molar ratio of 4-fluoronitrobenzene to triethylamine in step 1① is 1:2;

[0176] The molar ratio of 4-fluoronitrobenzene to 4-methoxyaniline in step 1① is 2:1;

[0177] The ratio of the volume of cold water to the amount of 4-methoxyaniline monomer mentioned in step 1① is (400-450) mL: 10 mmol;

[0178] The temperature of the cold water mentioned in step 1① is 0~5℃;

[0179] The vacuum drying temperature in step 1① is 45℃, the vacuum drying time is 48 hours, and the vacuum drying pressure is -30~-29KPa;

[0180] ② Under a nitrogen atmosphere, anhydrous ethanol and 4,7-dibromobenzothiadiazole were added to a three-necked flask. The reaction mixture was placed in an ice-water bath, and sodium borohydride was added in batches while stirring. The reaction mixture was then placed in an ice bath with stirring. After the gas stopped escaping, the ice bath was removed, and the reaction mixture was stirred at room temperature for 20 hours. After the reaction was complete, the ethanol was removed by rotary evaporation, followed by extraction. The organic phase was then washed with brine, and anhydrous MgSO4 was added to the organic phase for drying. The organic phase was then filtered, the solvent was removed by vacuum evaporation, and the mixture was dried in a vacuum oven to obtain a pale yellow solid product, 3,6-dibromo-1,2-phenylenediamine monomer, named M2.

[0181] The volume ratio of anhydrous ethanol to the amount of 4,7-dibromobenzothiadiazole in step 1② is (50-80) mL: 15 mmol.

[0182] The molar ratio of 4,7-dibromobenzothiadiazole to sodium borohydride in step 1② is 3:1;

[0183] The volume ratio of anhydrous ethanol to sodium borohydride in step 1② is (50-80) mL: 0.51 mmol;

[0184] The vacuum drying temperature described in step 1② is 55℃, the vacuum drying time is 48 hours, and the vacuum drying pressure is -30~-29KPa;

[0185] ③ At room temperature, M2 and phenanthrene-9,10-dione were dissolved in acetic acid. A precipitate gradually formed in the reaction flask. The reaction mixture was refluxed at 100°C for 24 hours. After the reaction was completed, it was cooled to room temperature and neutralized with sodium bicarbonate. The precipitate was collected by filtration and washed with ethanol. The crystallized product was placed in a vacuum drying oven to obtain a yellow solid product, 10,13-dibromodibenzo[a,c]phenazine, named M3.

[0186] The molar ratio of M2 to phenanthrene-9,10-dione mentioned in step 1③ is 1:1;

[0187] The volume ratio of acetic acid to the amount of M2 in step 1③ is (50-80) mL: 2.1 mmol;

[0188] The volume ratio of acetic acid to phenanthrene-9,10-dione in step 1③ is (50-80) mL: 2.1 mmol;

[0189] The mass ratio of sodium bicarbonate to water in step 1③ is 4g:100mL;

[0190] The vacuum drying temperature described in step 1③ is 45℃, the vacuum drying time is 36 hours, and the vacuum drying pressure is -30~-29KPa;

[0191] ④ Under a nitrogen atmosphere, M1, M3, 18-crown-6 ether, copper powder, potassium carbonate, and o-dichlorobenzene were placed in a three-necked flask and heated to 180°C. The mixture was then refluxed and reacted for 36 hours. After the reaction was completed, the mixture was filtered while hot, and the filtrate was poured into petroleum ether to precipitate a brick-red precipitate. The brick-red precipitate was purified by column chromatography, and the purified product was vacuum dried to obtain a brick-red powder, which was named M4.

[0192] The molar ratio of M1 to M3 mentioned in step 1, ④ is 1:2.5;

[0193] The molar ratio of M1 to 18-crown-6 ether in step 1④ is 1:1;

[0194] In step 1, ④, the molar ratio of M1 to copper powder is 1:8;

[0195] In step 1, ④, the molar ratio of M1 to potassium carbonate is 1:8;

[0196] The volume ratio of o-dichlorobenzene to the amount of M1 in step 1④ is (20–30) mL: 1 mmol;

[0197] The volume ratio of petroleum ether to the amount of M1 in step 1, ④ is (150–200) mL: 1 mmol;

[0198] The vacuum drying temperature described in step 1④ is 45℃, the vacuum drying time is 48 hours, and the vacuum drying pressure is -30~-29KPa;

[0199] ⑤ Under a nitrogen atmosphere, M4, anhydrous ethanol, and Pd / C were added to a three-necked flask. When the temperature reached 80°C, hydrazine hydrate was added dropwise to the flask using a constant-pressure funnel at a rate of 1–2 drops per second. The temperature was raised to reflux, and the reaction was allowed to proceed for 12 hours. After the reaction was complete, the palladium on carbon was removed by hot filtration. The filtrate was poured into distilled water, and an appropriate amount of sodium chloride was added to precipitate a solid. The solid phase was filtered off and washed with ethanol to obtain a pale blue precipitate, which was then dried under vacuum to obtain N. 1 N 1 '-(dibenzo[a,c]phenazine-10,13-diyl)bis(N 1 -(4-methoxyphenyl)benzene-1,4-diamine), named M5;

[0200] The volume ratio of anhydrous ethanol to the amount of M4 in step 1, ⑤ is (80-100) mL: 14 mmol;

[0201] The mass ratio of Pd / C to the molar amount of M4 mentioned in step 1, ⑤ is (1-1.5) g: 7 mmol;

[0202] The volume ratio of hydrazine hydrate to the amount of M4 in step 1, ⑤ is 3 mL: 1 mmol;

[0203] In step 1, ⑤, the heating rate when the solution is refluxed is 10°C per minute.

[0204] The temperature of the cold water mentioned in step 1, ⑤ is 0℃;

[0205] The volume ratio of the filtrate to cold water in step 1, ⑤ is 1:5;

[0206] In step 1, ⑤, the Pd / C is a material with palladium supported on a carbon support, and the mass fraction of Pd in ​​the Pd / C is 10%.

[0207] The vacuum drying temperature described in step 1, ⑤ is 30℃, the vacuum drying time is 48 to 64 hours, and the vacuum drying pressure is -30 to -29 kPa.

[0208] II. Preparation of polyamides containing quinoxalin and triarylamine groups:

[0209] A mixture containing M5, 4,4'-diphenyl ether dicarboxylic acid, triphenyl phosphite, calcium chloride, pyridine, and N-methylpyrrolidone was stirred at 120°C for 8 hours. After cooling to room temperature, methanol was added, the precipitate was collected by filtration, and thoroughly washed with methanol. Finally, the polymer P2 was obtained by extraction with methanol and acetone using a Soxhlet extractor.

[0210] The molar ratio of M5 to the diacid monomer in step two is 1:1;

[0211] The volume ratio of triphenyl phosphite to the molar amount of M5 in step two is 1.1 mL: 1 mmol;

[0212] The volume ratio of pyridine to the molar amount of M5 in step two is 0.6 mL: 1 mmol;

[0213] The volume ratio of N-methylpyrrolidone to the amount of M5 in step two is 3 mL: 1 mmol;

[0214] The mass ratio of calcium chloride to N-methylpyrrolidone in step two is 0.15 g : 1.5 mL;

[0215] In step two, the volume ratio of methanol and acetone to the molar amount of M5 is 250 mL: 1 mmol.

[0216] Example 3: The structural formulas of triarylamine polyamide P3 containing the quinoxaline structure are as follows: In the formula, n is 16.

[0217] I. Synthesis of N 1 N 1 '-(dibenzo[a,c]phenazine-10,13-diyl)bis(N 1 (4-Methoxyphenyl)benzene-1,4-diamine) monomer:

[0218] ① Under a nitrogen atmosphere, a mixture of 4-methoxyaniline, 4-fluoronitrobenzene, triethylamine and anhydrous dimethyl sulfoxide was placed in a three-necked flask and stirred at 90°C for 36 hours. The mixture was then refluxed. After the reaction was completed, the reaction solution was cooled to room temperature and poured into cold water to precipitate. The precipitate was filtered to obtain an orange solid crude product. The product was then recrystallized, and an orange needle-like crystalline product was filtered out. The product was then dried under vacuum to obtain 4-methoxy-4'-nitrodiphenylamine, which was named M1.

[0219] The volume ratio of anhydrous dimethyl sulfoxide to the molar amount of 4-methoxyaniline in step 1① is (100-150) mL: 13 mmol.

[0220] The molar ratio of 4-fluoronitrobenzene to triethylamine in step 1① is 1:2;

[0221] The molar ratio of 4-fluoronitrobenzene to 4-methoxyaniline in step 1① is 2:1;

[0222] The ratio of the volume of cold water to the amount of 4-methoxyaniline monomer mentioned in step 1① is (400-450) mL: 10 mmol;

[0223] The temperature of the cold water mentioned in step 1① is 0~5℃;

[0224] The vacuum drying temperature in step 1① is 45℃, the vacuum drying time is 48 hours, and the vacuum drying pressure is -30~-29KPa;

[0225] ② Under a nitrogen atmosphere, anhydrous ethanol and 4,7-dibromobenzothiadiazole were added to a three-necked flask. The reaction mixture was placed in an ice-water bath, and sodium borohydride was added in batches while stirring. The reaction mixture was then placed in an ice bath with stirring. After the gas stopped escaping, the ice bath was removed, and the reaction mixture was stirred at room temperature for 20 hours. After the reaction was complete, the ethanol was removed by rotary evaporation, followed by extraction. The organic phase was then washed with brine, and anhydrous MgSO4 was added to the organic phase for drying. The organic phase was then filtered, the solvent was removed by vacuum evaporation, and the mixture was dried in a vacuum oven to obtain a pale yellow solid product, 3,6-dibromo-1,2-phenylenediamine monomer, named M2.

[0226] The volume ratio of anhydrous ethanol to the amount of 4,7-dibromobenzothiadiazole in step 1② is (50-80) mL: 15 mmol.

[0227] The molar ratio of 4,7-dibromobenzothiadiazole to sodium borohydride in step 1② is 3:1;

[0228] The volume ratio of anhydrous ethanol to sodium borohydride in step 1② is (50-80) mL: 0.51 mmol;

[0229] The vacuum drying temperature described in step 1② is 55℃, the vacuum drying time is 48 hours, and the vacuum drying pressure is -30~-29KPa;

[0230] ③ At room temperature, M2 and phenanthrene-9,10-dione were dissolved in acetic acid. A precipitate gradually formed in the reaction flask. The reaction mixture was refluxed at 100°C for 24 hours. After the reaction was completed, it was cooled to room temperature and neutralized with sodium bicarbonate. The precipitate was collected by filtration and washed with ethanol. The crystallized product was placed in a vacuum drying oven to obtain a yellow solid product, 10,13-dibromodibenzo[a,c]phenazine, named M3.

[0231] The molar ratio of M2 to phenanthrene-9,10-dione mentioned in step 1③ is 1:1;

[0232] The volume ratio of acetic acid to the amount of M2 in step 1③ is (50-80) mL: 2.1 mmol;

[0233] The volume ratio of acetic acid to phenanthrene-9,10-dione in step 1③ is (50-80) mL: 2.1 mmol;

[0234] The mass ratio of sodium bicarbonate to water in step 1③ is 4g:100mL;

[0235] The vacuum drying temperature described in step 1③ is 45℃, the vacuum drying time is 36 hours, and the vacuum drying pressure is -30~-29KPa;

[0236] ④ Under a nitrogen atmosphere, M1, M3, 18-crown-6 ether, copper powder, potassium carbonate, and o-dichlorobenzene were placed in a three-necked flask and heated to 180°C. The mixture was then refluxed and reacted for 36 hours. After the reaction was completed, the mixture was filtered while hot, and the filtrate was poured into petroleum ether to precipitate a brick-red precipitate. The brick-red precipitate was purified by column chromatography, and the purified product was vacuum dried to obtain a brick-red powder, which was named M4.

[0237] The molar ratio of M1 to M3 mentioned in step 1, ④ is 1:2.5;

[0238] The molar ratio of M1 to 18-crown-6 ether in step 1④ is 1:1;

[0239] In step 1, ④, the molar ratio of M1 to copper powder is 1:8;

[0240] In step 1, ④, the molar ratio of M1 to potassium carbonate is 1:8;

[0241] The volume ratio of o-dichlorobenzene to the amount of M1 in step 1④ is (20–30) mL: 1 mmol;

[0242] The volume ratio of petroleum ether to the amount of M1 in step 1, ④ is (150–200) mL: 1 mmol;

[0243] The vacuum drying temperature described in step 1④ is 45℃, the vacuum drying time is 48 hours, and the vacuum drying pressure is -30~-29KPa;

[0244] ⑤ Under a nitrogen atmosphere, M4, anhydrous ethanol, and Pd / C were added to a three-necked flask. When the temperature reached 80°C, hydrazine hydrate was added dropwise to the flask using a constant-pressure funnel at a rate of 1–2 drops per second. The temperature was raised to reflux, and the reaction was allowed to proceed for 12 hours. After the reaction was complete, the palladium on carbon was removed by hot filtration. The filtrate was poured into distilled water, and an appropriate amount of sodium chloride was added to precipitate a solid. The solid phase was filtered off and washed with ethanol to obtain a pale blue precipitate, which was then dried under vacuum to obtain N. 1 N 1 '-(dibenzo[a,c]phenazine-10,13-diyl)bis(N 1 -(4-methoxyphenyl)benzene-1,4-diamine), named M5;

[0245] The volume ratio of anhydrous ethanol to the amount of M4 in step 1, ⑤ is (80-100) mL: 14 mmol;

[0246] The mass ratio of Pd / C to the molar amount of M4 mentioned in step 1, ⑤ is (1-1.5) g: 7 mmol;

[0247] The volume ratio of hydrazine hydrate to the amount of M4 in step 1, ⑤ is 3 mL: 1 mmol;

[0248] In step 1, ⑤, the heating rate when the solution is refluxed is 10°C per minute.

[0249] The temperature of the cold water mentioned in step 1, ⑤ is 0℃;

[0250] The volume ratio of the filtrate to cold water in step 1, ⑤ is 1:5;

[0251] In step 1, ⑤, the Pd / C is a material with palladium supported on a carbon support, and the mass fraction of Pd in ​​the Pd / C is 10%.

[0252] The vacuum drying temperature described in step 1, ⑤ is 30℃, the vacuum drying time is 48 to 64 hours, and the vacuum drying pressure is -30 to -29 kPa.

[0253] II. Preparation of polyamides containing quinoxalin and triarylamine groups:

[0254] The mixture containing M5, terephthalic acid, triphenyl phosphite, calcium chloride, pyridine, and N-methylpyrrolidone was stirred at 120°C for 8 hours. After cooling to room temperature, methanol was added, the precipitate was collected by filtration, and the mixture was thoroughly washed with methanol. Finally, the polymer P3 was obtained by extraction with methanol and acetone using a Soxhlet extractor.

[0255] The molar ratio of M5 to the diacid monomer in step two is 1:1;

[0256] The volume ratio of triphenyl phosphite to the molar amount of M5 in step two is 1.1 mL: 1 mmol;

[0257] The volume ratio of pyridine to the molar amount of M5 in step two is 0.6 mL: 1 mmol;

[0258] The volume ratio of N-methylpyrrolidone to the amount of M5 in step two is 3 mL: 1 mmol;

[0259] The mass ratio of calcium chloride to N-methylpyrrolidone in step two is 0.15 g : 1.5 mL;

[0260] In step two, the volume ratio of methanol and acetone to the molar amount of M5 is 250 mL: 1 mmol.

[0261] Example 4: The structural formulas of triarylamine polyamide P4 containing the quinoxaline structure are as follows: In the formula, n is 11.

[0262] I. Synthesis of N 1 N 1 '-(dibenzo[a,c]phenazine-10,13-diyl)bis(N 1 (4-Methoxyphenyl)benzene-1,4-diamine) monomer:

[0263] ① Under a nitrogen atmosphere, a mixture of 4-methoxyaniline, 4-fluoronitrobenzene, triethylamine and anhydrous dimethyl sulfoxide was placed in a three-necked flask and stirred at 90°C for 36 hours. The mixture was then refluxed. After the reaction was completed, the reaction solution was cooled to room temperature and poured into cold water to precipitate. The precipitate was filtered to obtain an orange solid crude product. The product was then recrystallized, and an orange needle-like crystalline product was filtered out. The product was then dried under vacuum to obtain 4-methoxy-4'-nitrodiphenylamine, which was named M1.

[0264] The volume ratio of anhydrous dimethyl sulfoxide to the molar amount of 4-methoxyaniline in step 1① is (100-150) mL: 13 mmol.

[0265] The molar ratio of 4-fluoronitrobenzene to triethylamine in step 1① is 1:2;

[0266] The molar ratio of 4-fluoronitrobenzene to 4-methoxyaniline in step 1① is 2:1;

[0267] The ratio of the volume of cold water to the amount of 4-methoxyaniline monomer mentioned in step 1① is (400-450) mL: 10 mmol;

[0268] The temperature of the cold water mentioned in step 1① is 0~5℃;

[0269] The vacuum drying temperature in step 1① is 45℃, the vacuum drying time is 48 hours, and the vacuum drying pressure is -30~-29KPa;

[0270] ② Under a nitrogen atmosphere, anhydrous ethanol and 4,7-dibromobenzothiadiazole were added to a three-necked flask. The reaction mixture was placed in an ice-water bath, and sodium borohydride was added in batches while stirring. The reaction mixture was then placed in an ice bath with stirring. After the gas stopped escaping, the ice bath was removed, and the reaction mixture was stirred at room temperature for 20 hours. After the reaction was complete, the ethanol was removed by rotary evaporation, followed by extraction. The organic phase was then washed with brine, and anhydrous MgSO4 was added to the organic phase for drying. The organic phase was then filtered, the solvent was removed by vacuum evaporation, and the mixture was dried in a vacuum oven to obtain a pale yellow solid product, 3,6-dibromo-1,2-phenylenediamine monomer, named M2.

[0271] The volume ratio of anhydrous ethanol to the amount of 4,7-dibromobenzothiadiazole in step 1② is (50-80) mL: 15 mmol.

[0272] The molar ratio of 4,7-dibromobenzothiadiazole to sodium borohydride in step 1② is 3:1;

[0273] The volume ratio of anhydrous ethanol to sodium borohydride in step 1② is (50-80) mL: 0.51 mmol;

[0274] The vacuum drying temperature described in step 1② is 55℃, the vacuum drying time is 48 hours, and the vacuum drying pressure is -30~-29KPa;

[0275] ③ At room temperature, M2 and phenanthrene-9,10-dione were dissolved in acetic acid. A precipitate gradually formed in the reaction flask. The reaction mixture was refluxed at 100°C for 24 hours. After the reaction was completed, it was cooled to room temperature and neutralized with sodium bicarbonate. The precipitate was collected by filtration and washed with ethanol. The crystallized product was placed in a vacuum drying oven to obtain a yellow solid product, 10,13-dibromodibenzo[a,c]phenazine, named M3.

[0276] The molar ratio of M2 to phenanthrene-9,10-dione mentioned in step 1③ is 1:1;

[0277] The volume ratio of acetic acid to the amount of M2 in step 1③ is (50-80) mL: 2.1 mmol;

[0278] The volume ratio of acetic acid to phenanthrene-9,10-dione in step 1③ is (50-80) mL: 2.1 mmol;

[0279] The mass ratio of sodium bicarbonate to water in step 1③ is 4g:100mL;

[0280] The vacuum drying temperature described in step 1③ is 45℃, the vacuum drying time is 36 hours, and the vacuum drying pressure is -30~-29KPa;

[0281] ④ Under a nitrogen atmosphere, M1, M3, 18-crown-6 ether, copper powder, potassium carbonate, and o-dichlorobenzene were placed in a three-necked flask and heated to 180°C. The mixture was then refluxed and reacted for 36 hours. After the reaction was completed, the mixture was filtered while hot, and the filtrate was poured into petroleum ether to precipitate a brick-red precipitate. The brick-red precipitate was purified by column chromatography, and the purified product was vacuum dried to obtain a brick-red powder, which was named M4.

[0282] The molar ratio of M1 to M3 mentioned in step 1, ④ is 1:2.5;

[0283] The molar ratio of M1 to 18-crown-6 ether in step 1④ is 1:1;

[0284] In step 1, ④, the molar ratio of M1 to copper powder is 1:8;

[0285] In step 1, ④, the molar ratio of M1 to potassium carbonate is 1:8;

[0286] The volume ratio of o-dichlorobenzene to the amount of M1 in step 1④ is (20–30) mL: 1 mmol;

[0287] The volume ratio of petroleum ether to the amount of M1 in step 1, ④ is (150–200) mL: 1 mmol;

[0288] The vacuum drying temperature described in step 1④ is 45℃, the vacuum drying time is 48 hours, and the vacuum drying pressure is -30~-29KPa;

[0289] ⑤ Under a nitrogen atmosphere, M4, anhydrous ethanol, and Pd / C were added to a three-necked flask. When the temperature reached 80°C, hydrazine hydrate was added dropwise to the flask using a constant-pressure funnel at a rate of 1–2 drops per second. The temperature was raised to reflux, and the reaction was allowed to proceed for 12 hours. After the reaction was complete, the palladium on carbon was removed by hot filtration. The filtrate was poured into distilled water, and an appropriate amount of sodium chloride was added to precipitate a solid. The solid phase was filtered off and washed with ethanol to obtain a pale blue precipitate, which was then dried under vacuum to obtain N. 1 N 1 '-(dibenzo[a,c]phenazine-10,13-diyl)bis(N 1 -(4-methoxyphenyl)benzene-1,4-diamine), named M5;

[0290] The volume ratio of anhydrous ethanol to the amount of M4 in step 1, ⑤ is (80-100) mL: 14 mmol;

[0291] The mass ratio of Pd / C to the molar amount of M4 mentioned in step 1, ⑤ is (1-1.5) g: 7 mmol;

[0292] The volume ratio of hydrazine hydrate to the amount of M4 in step 1, ⑤ is 3 mL: 1 mmol;

[0293] In step 1, ⑤, the heating rate when the solution is refluxed is 10°C per minute.

[0294] The temperature of the cold water mentioned in step 1, ⑤ is 0℃;

[0295] The volume ratio of the filtrate to cold water in step 1, ⑤ is 1:5;

[0296] In step 1, ⑤, the Pd / C is a material with palladium supported on a carbon support, and the mass fraction of Pd in ​​the Pd / C is 10%.

[0297] The vacuum drying temperature described in step 1, ⑤ is 30℃, the vacuum drying time is 48 to 64 hours, and the vacuum drying pressure is -30 to -29 kPa.

[0298] II. Preparation of polyamides containing quinoxalin groups and triarylamines:

[0299] The mixture containing M5, 4,4'-dicarboxylic acid biphenyl sulfone, triphenyl phosphite, calcium chloride, pyridine, and N-methylpyrrolidone was stirred at 120°C for 8 hours. After cooling to room temperature, methanol was added, the precipitate was collected by filtration, and the mixture was thoroughly washed with methanol. Finally, the polymer P4 was obtained by Soxhlet extraction using methanol and acetone, respectively.

[0300] The molar ratio of M5 to the diacid monomer in step two is 1:1;

[0301] The volume ratio of triphenyl phosphite to the molar amount of M5 in step two is 1.1 mL: 1 mmol;

[0302] The volume ratio of pyridine to the molar amount of M5 in step two is 0.6 mL: 1 mmol;

[0303] The volume ratio of N-methylpyrrolidone to the amount of M5 in step two is 3 mL: 1 mmol;

[0304] The mass ratio of calcium chloride to N-methylpyrrolidone in step two is 0.15 g : 1.5 mL;

[0305] In step two, the volume ratio of methanol and acetone to the molar amount of M5 is 250 mL: 1 mmol.

[0306] Figure 1 Infrared spectra of the triphenylamine polymers containing quinoxaline structures prepared in Examples 1 to 4; from Figure 1 The infrared spectra of the four triphenylamine polymers containing quinoxaline structures show a value of 3300 cm⁻¹. -1 and 1670cm -1 Two amide bands exhibit characteristic absorption peaks. In summary, Figure 1 Examples one through four demonstrate the synthesis of triphenylamine polymers containing a quinoxaline structure;

[0307] Figure 2 N prepared in Example 1 1 N 1 '-(dibenzo[a,c]phenazine-10,13-diyl)bis(N 1 The proton NMR spectrum of (4-methoxyphenyl)benzene-1,4-diamine monomer;

[0308] Figure 3-6 The above are the proton NMR spectra of the triarylamine polymers P1-P4 containing quinoxaline structures prepared in Examples 1 to 4; from Figure 3-6 The chemical shift δ is 9.73–10.67, which can be attributed to the chemical shift of H on the amide group, indicating that the three amine polymers containing quinoxaline structure were synthesized in Examples 1 to 4.

[0309] The triphenylamine polymers P1-P4 containing quinoxaline structure were coated into films, and their properties were tested.

[0310] Figure 7 Cyclic voltammograms of the triarylamine polyamide polymers containing benzophenthiazine structures prepared in Examples 1 to 4; from Figure 7 It can be seen that polymer P1 showed two oxidation peaks at 0.61V and 0.88V, and two reduction peaks at 0.37V and 0.62V; polymer P2 showed two oxidation peaks at 0.57V and 0.84V, and two reduction peaks at 0.40V and 0.65V; polymer P3 showed two oxidation peaks at 0.69V and 1.04V, and two reduction peaks at 0.38V and 0.60V; polymer P4 showed two oxidation peaks at 0.66V and 0.91V, and two reduction peaks at 0.48V and 0.75V. This indicates that the triarylamine polymers containing quinoxaline structure prepared in Examples 1 to 4 underwent redox reactions under applied voltage conditions, and the triarylamine polyamide polymers containing quinoxaline structure produced color changes during the redox process. This indicates that the triarylamine polymers containing quinoxaline structure prepared in Examples 1 to 4 possess electrochromic properties.

[0311] Figure 8-11 Electrochromic images of the triarylamine polymers containing quinoxaline structures prepared in Examples 1 to 4 are shown. The electrochromic properties of the polyamides were determined by testing the changes in UV-Vis and NIR spectra under increasing applied potential. Taking the electrochromic properties of P4 as an example, as the potential increases, the absorption intensity at 338 nm and 1251 nm gradually decreases, while the absorption intensity at 660 nm and 890 nm increases sharply, and the color of the film changes from colorless to deep blue. When the applied voltage reaches 0.9 V, the absorption intensity of P4 continues to increase. When the voltage is applied to 1.4 V, the absorption of P4 reaches its maximum, and the color of the film is deep blue. After increasing the oxidation potential above 1.4 V, the absorption at 660 nm and 890 nm no longer increases, indicating that the triarylamine TPA is completely oxidized to TPA. + .

[0312] Figure 12 Thermogravimetric curves of the triarylamine polymers containing quinoxaline structures prepared in Examples 1 to 4 are shown. Figure 12 It can be seen that the thermal decomposition temperatures of the aforementioned triarylamine polymers containing quinoxaline structures under a nitrogen atmosphere with a 10% weight loss are in the range of 398-432℃, indicating that these polymers have good thermal stability. When heated to 800℃, the residual carbon content of these polymers is all greater than 63%, which is due to the high content of aromatic structures in the polymers. This further demonstrates that the polymers have good thermal stability and can operate in high-temperature environments, such as in the aerospace field.

[0313] The coloring decolorization time of polymer films was tested using the step voltage method. The specific method is as follows: voltages of -0.3 to 0.9V were applied to films P1 to P4 respectively, and the cycle time was maintained for 10s. The changes in polyamide transmittance were determined under the conditions of wavelengths of 895nm / 888nm / 893nm / 893nm respectively.

[0314] Figure 13 The figure shows the dynamic curve of the transmittance of the P1 thin film at a wavelength of 895 nm under a voltage range of -0.3 to 0.9 V. The optical contrast of P1 is 41%, and the optical contrast remains basically unchanged after 600 cycles, demonstrating excellent electrochromic stability. Figure 14 The figure shows the dynamic curve of the transmittance of the P2 thin film at a wavelength of 888 nm under a voltage range of -0.3 to 0.9 V. The optical contrast of P2 is 40%, and the optical contrast remains basically unchanged after 1000 cycles, demonstrating excellent electrochromic stability. Figure 15The figure shows the dynamic curve of the transmittance of the P3 thin film at a wavelength of 893 nm under a voltage range of -0.3 to 0.9 V. The optical contrast of P3 is 48%, and the optical contrast remains basically unchanged after 800 cycles, demonstrating excellent electrochromic stability. Figure 16 The figure shows the dynamic curve of the transmittance of the P3 film at a wavelength of 890 nm under a voltage range of -0.3 to 0.9 V. The P4 film has an optical contrast of 50%, and its optical contrast remains essentially unchanged after 1500 cycles, exhibiting excellent electrochromic stability.

[0315] The switching response time of the electrochromic process is defined as the time it takes for the transmittance to reach 90% of the full change after a voltage is applied; this data represents its response speed. Figure 17 The redox process of the P1 film during the step test was calculated to be 3.2 s for coloring and 1.1 s for fading. Figure 18 The redox process of the P2 film during the step test was calculated to be 1.0 s for coloring and 3.0 s for fading. Figure 19 The redox process of the P3 film during the step test was calculated to be 1.6 s for coloring and 3.3 s for fading. Figure 20 The redox process of the P4 film during the step test was calculated to have a coloring time of 1.8 s and a fading time of 3.8 s. Among them, the P2 film had the fastest response speed, exhibiting excellent coloring and fading response times.

Claims

1. A polyamide P1 polymerized from a triarylamine monomer containing a quinoxaline structure and a commercially available diacid monomer, namely 1,4-cyclohexanedicarboxylic acid, characterized in that, The structural formula of polyamide P1 is as follows: In the above structural formula, n is an integer from 10 to 16.

2. The application of polyamide P1 as an electrochromic layer in an electrochromic device as described in claim 1 in electrochromic applications.

3. The application according to claim 2, characterized in that... The application of polyamide P1 as an electrochromic layer in electrochromic devices is carried out according to the following steps: Polyamide P1 is used as the electrochromic layer in the electrochromic device. The electrochromic layer is coated on a conductive substrate to prepare the electrochromic device. The electrochromic layer produces electrochromic changes under the action of an external electric field.

4. The application according to claim 3, characterized in that: The conductive substrate is ITO conductive glass.

5. The application according to claim 3, characterized in that: The voltage of the applied electric field is 0 ~ 2.2 V.

Citation Information

Patent Citations

  • Method for preparing polyimide porous diaphragm

    CN109473605A

  • Synthesis method of dinitro-substituted quinoxaline, heat-resistant polyimide and preparation method of same

    CN111909102A