A high weather-resistant titanium dioxide, its preparation method and application
By using multilayer silicon oxide film coating technology, the problem of limited use of titanium dioxide under specific pH conditions has been solved, achieving high weather resistance and good dispersibility over a wide pH range, making it suitable for titanium dioxide applications in both acidic and alkaline systems.
Patent Information
- Application Number
- CN202311673858.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-07
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-12-07
AI Technical Summary
In existing technologies, the silicon coating technology for titanium dioxide involves water washing to dilute the material, which limits its use in specific pH environments. Furthermore, zirconium coating is costly and struggles to exhibit good weather resistance in acidic and alkaline systems.
The process employs a multi-layer silicon coating technology, which includes the coating of dense and porous silicon oxide films. By controlling the pH value and temperature, it ensures that sodium silicate forms a continuous dense and porous oxide film on the surface of titanium dioxide. Combined with an alcoholysis organic treatment agent, the dispersibility and weather resistance of titanium dioxide are improved.
The prepared titanium dioxide exhibits excellent weather resistance and dispersibility over a wide pH range, making it suitable for both acidic and alkaline systems. This solves the problem of water washing not affecting the product, thus improving the applicability and performance of the titanium dioxide.
Smart Images

Figure CN117624941B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of titanium dioxide, and in particular to a high weather-resistant titanium dioxide, its preparation method, and its application. Background Technology
[0002] Titanium dioxide possesses relatively stable physical and chemical properties and is widely used in industries such as coatings, rubber, papermaking, inks, plastics, food additives, and pharmaceutical dyeing. However, titanium dioxide also exhibits photochemical activity; in the presence of water in the air, oxygen atoms excited by ultraviolet light can degrade organic media such as coatings. To improve its performance, surface coating treatment is necessary. This is used to improve inherent defects in titanium dioxide products or alter the surface properties of its molecular particles. Inorganic surface treatment involves coating titanium dioxide particles with a film, preventing direct contact with organic media, thus shielding against photocatalysis and enhancing the chemical resistance of titanium dioxide. Different surface treatment agents, treatment amounts, and treatment methods will all have varying degrees of impact on the properties of titanium dioxide. The most commonly used inorganic surface treatment agents are hydrated oxides of aluminum and silicon. The Al2O3 / SiO2 series is considered the most basic coating method. Aluminum coating forms a protective layer on the surface of titanium dioxide, isolating it from direct contact with organic media. However, aluminum coating has a drawback. Because alumina is an amphoteric oxide, it can react with both acids and alkalis. Therefore, the use of silicon-aluminum coated titanium dioxide products is limited in certain environmental systems. The role of the silicon coating is to form a film on the surface of titanium dioxide, isolating the titanium dioxide particles from the medium, reducing the contact area between titanium dioxide and the medium, blocking the photoactivation sites on TiO2, effectively protecting titanium dioxide from ultraviolet radiation, and reducing its photochemical activity.
[0003] Titanium dioxide is generally not coated alone because current silicon coating technology dilutes the material through water washing. It is usually coated simultaneously with aluminum coating. Alumina is an amphoteric oxide, so the use of aluminum-coated titanium dioxide products is limited in acidic systems.
[0004] Chinese Patent Publication No. CN111100481A discloses a method for coating dense alumina onto the surface of titanium dioxide, belonging to the field of analytical testing technology. This invention provides a method for coating dense alumina onto the surface of titanium dioxide, comprising: mixing titanium dioxide, water, and a dispersant; slurrying and dispersing to obtain a pre-coating slurry; diluting the pre-coating slurry with water; adjusting the pH and temperature of the slurry; adding sodium aluminate and dilute acid; then controlling the pH for a first and second ripening; followed by sieving, filtering, washing, and organic treatment; and finally drying and pulverizing to obtain uniform and dense aluminum-coated titanium dioxide. This patent includes both silicon coating and aluminum coating. The aluminum coating can react with both acids and alkalis, and the resulting titanium dioxide has strict pH requirements during use.
[0005] Zirconium coating, specifically zirconium oxide coating, can improve the weather resistance of titanium dioxide, but zirconium is expensive. Therefore, zirconium coating is generally not used. Even if zirconium coating is used, the coating amount is small, and the outer layer does not contain aluminum salts or other components, so it does not significantly alter the surface properties of the powder. Summary of the Invention
[0006] The technical problem to be solved by the present invention is to provide a method for preparing titanium dioxide with high weather resistance, which addresses the shortcomings of the existing technology. The titanium dioxide prepared is unaffected by water washing, has high purity, and has good dispersibility.
[0007] This invention also provides a highly weather-resistant titanium dioxide and its application, suitable for use in acidic and alkaline systems, exhibiting excellent weather resistance.
[0008] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is: a method for preparing high weather-resistant titanium dioxide, comprising the following steps:
[0009] S1. Prepare titanium dioxide slurry;
[0010] S2. Heat the titanium dioxide slurry in S1 to 85-90℃, control the pH to 10-10.5, add sodium silicate solution to react, and let it mature for 2-3 hours.
[0011] S3. Add sodium silicate solution to the titanium dioxide slurry obtained in S2, and then add dilute acid dropwise to make the pH of the slurry finally 5.0-6.0, and the maturation time is 60-90 minutes.
[0012] S4. Cool the titanium dioxide slurry obtained in S3 to 60-70℃, then add sodium silicate solution to adjust the pH to 6.0-7.0, and let it mature for 30-60 minutes.
[0013] S5. Cool the titanium dioxide slurry obtained in S4 to 50-60℃, then add sodium silicate solution to adjust the pH to 5.5-6.5, and let it mature for 30-60 minutes.
[0014] S6. Wash the titanium dioxide slurry obtained in S5 with water, filter it to obtain a filter cake, dry the filter cake, and then add an alcoholysis organic treatment agent and stir to obtain the final product.
[0015] In S2, the pH is 10-10.5 and the temperature is 85-90℃, forming a dense and uniform silica film. In S3, acid neutralization causes silicon to precipitate as "active silicon" in the form of Si(OH)4 on the surface of TiO2 particles, forming a continuous and dense film. Amorphous hydrated silicon oxide is firmly bonded to the TiO2 surface in the form of hydroxyl groups. S2 and S3 interact to form a dense, continuous film with strong adhesion to titanium dioxide.
[0016] S4 and S5 contain two layers of loose silicon film, which not only ensures that the titanium dioxide is not affected by water washing and guarantees the purity of the titanium dioxide, but also further improves the weather resistance of titanium dioxide.
[0017] The alcoholysis organic treatment agent in S6 improves the dispersion performance of titanium dioxide.
[0018] In a preferred embodiment of the present invention, the weight of sodium silicate solution in S2, calculated as SiO2, is 2.0-3.0% of the weight of titanium dioxide slurry;
[0019] The sodium silicate solution in S2 is added over a period of 20-30 minutes.
[0020] Add dilute acid to S2 to adjust the pH, wherein the weight concentration of the dilute acid is 2-8%.
[0021] The sodium silicate solution in S2 accounts for 2.0-3.0% of the weight of the titanium dioxide slurry. The sodium silicate solution in S2 is added over a period of 20-30 minutes to ensure good dispersion of sodium silicate in the titanium dioxide slurry at low concentrations, thus avoiding localized high concentrations or high pH values.
[0022] In step S2, first add an alkaline solution to adjust the pH to 10, then add a sodium silicate solution, and simultaneously add dilute acid to control the pH to 10.0-10.5. The weight of the titanium dioxide slurry is based on the weight of TiO2, and the same applies below. The time for adding the sodium silicate solution in step S2 is the total time required to add the sodium silicate solution.
[0023] In a preferred embodiment of the present invention, the weight of sodium silicate solution in S3, calculated as SiO2, is 0.5-1.0% of the weight of titanium dioxide slurry.
[0024] The sodium silicate solution in S3 is added over a period of 20-35 minutes.
[0025] The dilute acid mentioned in S3 is dilute sulfuric acid;
[0026] The weight concentration of the dilute acid mentioned in S3 is 2-8%;
[0027] The dilute acid mentioned in S3 is added over a period of 3-4 hours;
[0028] The pH control process in S3 is as follows:
[0029] Acidification pH 10-9.5 9.5-9.0 9.0-8.5 8.5-8.0 8.0-7.0 7.0-6.0 6.0-5.5 % of total time 45-50 30-35 10-15 3-5 2-3 1-2 0.5-1
[0030] The above parameters ensure that all silicic acid is deposited on the titanium dioxide surface, improving the SiO2 coating rate. The pH control process ensures that silicon forms a dense oxide film on the titanium dioxide surface, and the addition time of dilute sulfuric acid is controlled according to the pH value of the slurry.
[0031] In a preferred embodiment of the present invention, the weight of sodium silicate solution in S4, calculated as SiO2, is 1.0-5.0% of the weight of titanium dioxide slurry.
[0032] The sodium silicate solution in S4 is added over a period of 30-45 minutes.
[0033] The pH in S4 is adjusted by adding dilute sulfuric acid, with a concentration of 10-30%.
[0034] The above parameters enable silicic acid to form a loose oxide film on the surface of a dense oxide film.
[0035] In a preferred embodiment of the present invention, the weight of sodium silicate solution in S5, calculated as SiO2, is 0.5-1.0% of the weight of titanium dioxide slurry.
[0036] The sodium silicate solution in S5 is added over a period of 30-45 minutes.
[0037] The above parameters enable silicic acid to form an even looser oxide film on the surface of the already loose oxide film.
[0038] In a preferred embodiment of the present invention, the titanium dioxide slurry in S1 has a weight percentage concentration of 20-30% based on TiO2.
[0039] In a preferred embodiment of the present invention, the method for preparing the titanium dioxide slurry in S1 is to add titanium dioxide to deionized water to form a slurry, add a dispersant, and then perform sand milling, sieving, and dilution with water.
[0040] The dispersant mentioned in S1 is sodium hexametaphosphate;
[0041] The weight percentage of the dispersant mentioned in S1 is 0.1-0.5%;
[0042] The slurry concentration described in S1 is 600-1000 g / L;
[0043] The mesh size of the sieve in S1 is 300-500 mesh.
[0044] S1 ensures that titanium dioxide particles exist as individual particles in the system, allowing the subsequent oxide film to uniformly coat the surface of each TiO2 particle. S2 filters the milled slurry through a sieve to further remove coarse titanium dioxide particles and other impurities.
[0045] In a preferred embodiment of the present invention, the alcoholysis organic treatment agent in S6 is an alcoholysis silane coupling agent;
[0046] The weight percentage of the added alcoholysis silane coupling agent is 0.2-1.0%;
[0047] The preparation method of the alcoholysis silane coupling agent is as follows: prepare 40-60 ml of acetic acid solution, add 2-3 ml of γ-aminopropyltriethoxysilane dropwise while stirring, and stir for 20-30 min after the addition is complete; or;
[0048] To prepare 150-250 ml of acetic acid solution, add 10-30 ml of anhydrous ethanol, and while stirring, add 5-15 ml dropwise.
[0049] Add r-aminopropyltriethoxysilane and stir for 20-30 minutes.
[0050] The present invention also discloses a titanium dioxide prepared according to the preparation method described above.
[0051] The present invention also discloses the application of the titanium dioxide, wherein the titanium dioxide is suitable for a pH of 5-9.
[0052] There are two types of SiO2 coatings. One is a dense, skin-like or glass-like film, which has excellent weather resistance and is mainly used in high-weather-resistant coatings and plastics. This film also protects titanium dioxide particles from chemical corrosion. The other type is a porous, high-volume, sponge-like film, mainly used in matte latex paints. After the paint film dries, the micropores that were previously occupied by water allow some air to enter, thereby generating dry hiding power and improving the dry hiding power of the latex paint.
[0053] Depend on Figure 1 It can be seen that the dispersion mechanism of sodium silicate is as follows: when the pH is above 10, the absolute value of the Zeta potential is greater than 40MV, and its dispersibility is good, and the polymerization of silicic acid is very slow. When the pH is below 9, the absolute value of the Zeta potential is greater than 30MV, and the dispersibility is relatively stable, but silicic acid has a tendency to polymerize. When the pH drops from 9 to 8, the potential is -20MV, and the polymerization rate of silicic acid accelerates. When the pH of sodium silicate reaches below 6, silicic acid gradually precipitates and becomes a sol.
[0054] Depend on Figure 2 It can be seen that the relationship between the logarithm of the gelation time of silicic acid solution and pH presents a complete large "N" curve. It can also be seen that the gelation speed of silicic acid is most sensitive to pH. Therefore, the gelation speed of silicic acid is slowest when pH ≤ 3 or pH ≥ 10, and fastest when pH is 6-8.
[0055] The precipitate obtained at the pH corresponding to the highest point of the large "N" curve is dense and uniform. In the lower pH range of the curve, due to the rapid polymerization of silicic acid, it is impossible for silicic acid to deposit on the surface of TiO2 particles to form a dense, skin-like film. Instead, many small spherical SiO2 particles are generated, resulting in homogeneous nucleation. Below pH 3, the TiO2 slurry itself undergoes severe agglomeration. Therefore, titanium dioxide coating is not chosen in the low pH range. Generally, coating is selected in the high pH range, i.e., pH ≥ 10, to form a dense and uniform film.
[0056] Sodium silicate solution is added to TiO2 slurry to neutralize the silicon and form "active silicon" in the form of Si(OH)4, which precipitates on the surface of TiO2 particles. The characteristics of this coating are: (1) the coating thickness is relatively uniform and continuous, and the structure is dense; (2) amorphous hydrated silicon oxide is firmly bonded to the TiO2 surface in the form of hydroxyl groups. In the process of silicon coating, there is a sol-gel chemical process. After the silicon compound forms a sol, it is adsorbed on the surface of TiO2 particles, then gels, and finally forms a film on the particle surface. Therefore, the process conditions must be strictly controlled from the preparation of slurry to the silicon sol-adsorption-gel-film formation process. This includes the amount of silicon compound added, the pH value of the slurry, the reaction temperature, the reaction time, and as uniform a reaction condition as possible, to ensure that SiO2 is uniformly coated on the surface of TiO2 particles.
[0057] In step S2, sodium silicate is added to the titanium dioxide slurry under high pH conditions, ensuring that the sodium silicate is uniformly dispersed in the slurry. The sodium silicate solution does not contain metasilicic acid ions (SiO3). 2- Only H3SiO4 - and H2SiO4 2- When sodium silicate solution is acidified with dilute acid, the initially precipitated Si(OH)4 form of orthosilicic acid is highly reactive and quickly undergoes a condensation reaction to form polymeric silicic acid with siloxane chains. To control the polymerization rate of silicic acid and ensure the formation of a dense film on the titanium dioxide surface, the concentration of sodium silicate solution is controlled at 2-5% (based on SiO2), and the concentration of sulfuric acid is controlled at 2-8%. Low concentrations ensure good dispersion of sodium silicate in the titanium dioxide slurry, avoiding localized high concentrations or high pH values that could affect the formation of a dense film. The acidification pH is controlled at 10-10.5 to ensure a slow polymerization rate of silicic acid under these conditions, resulting in the formation of a dense film.
[0058] The weight concentration of the S3 sodium silicate solution is controlled at 2-5% (based on SiO2), and the concentration of sulfuric acid is controlled at 2-8%. To ensure that silicon forms a dense oxide film on the titanium dioxide surface, the addition time of dilute sulfuric acid is controlled according to the pH value of the slurry. The total time is 3-4 hours, and the time distribution is shown in the table below.
[0059] Acidification pH 10-9.5 9.5-9.0 9.0-8.5 8.5-8.0 8.0-7.0 7.0-6.0 6.0-5.5 % of total time 45-50 30-35 10-15 3-5 2-3 1-2 0.5-1
[0060] The pH of the slurry was finally adjusted to 5.5-6.0. This was done to ensure that all silicic acid was deposited on the surface of titanium dioxide, thereby increasing the SiO2 coating rate.
[0061] S4 is formed by coating a dense silicon film (S3) with a loosely packed SiO2 film. The sodium silicate concentration is 10-20% by weight (based on SiO2), and the sulfuric acid concentration is 10-20%. The temperature is controlled at 60-70℃, and the pH value is 6.0-7.0, in order to form a loose oxide film of silicic acid on the TiO2 surface.
[0062] S5 is made by coating another layer of loose silicon film onto a loose silicon film on top of the titanium dioxide loose silicon film, so that the silicon films are stacked layer by layer, which further improves the weather resistance of titanium dioxide. Its sodium silicate concentration is 10-20% (calculated as SiO2), and the sulfuric acid concentration is 10-20%.
[0063] Compared with the prior art, the beneficial effects of the present invention are as follows:
[0064] This invention coats the surface of titanium dioxide with multiple layers of dense and porous silicon films, isolating the titanium dioxide particles from the medium, thus solving the problem caused by the photocatalytic activity of titanium dioxide and greatly increasing the weather resistance of titanium dioxide.
[0065] This invention involves a dense double-layer silicon coating on the surface of titanium dioxide single particles, followed by a loose silicon coating on the surface of the titanium dioxide single particles to ensure that the coated material is not affected by water washing. Finally, an organic coating treatment is applied to give the titanium dioxide good dispersibility and weather resistance.
[0066] In this invention, the interaction of two dense films, two loose silicon films, and an alcoholysis organic film provides weather resistance comparable to that of aluminum-coated films in the prior art. Since this invention uses silicon coating, the titanium dioxide produced can be used in a wider pH range and has broad application prospects. Attached Figure Description
[0067] Figure 1 The curve shows the relationship between pH value and Zeta potential in the sodium silicate system.
[0068] Figure 2 This is the theoretical curve showing the logarithmic relationship between pH and time in the polymerization of monosilicic acid.
[0069] Figure 3 The image shows an electron microscope image of the titanium dioxide obtained in step (5) of Example 1.
[0070] Figure 4 This is an electron microscope magnified image of the titanium dioxide obtained in step (5) of Example 1.
[0071] Figure 5 This is an electron microscope image of the titanium dioxide prepared in Example 1.
[0072] Figure 6 This is a magnified electron microscope image of the titanium dioxide prepared in Example 1. Detailed Implementation
[0073] Example 1
[0074] (1) Titanium dioxide was added to deionized water to make a slurry with a concentration of 800 g / L, and 0.3% sodium hexametaphosphate was added. The mixture was then sand-milled to improve the dispersion of the particles. This allowed the titanium dioxide particles to exist as single particles in the system, so that the oxide film that was subsequently coated could be uniformly coated on the surface of each particle.
[0075] (2) The slurry after sand milling is filtered through a 400-mesh sieve to further remove large particles of titanium dioxide and other impurities.
[0076] (3) Transfer the sand milling slurry from the second step to the coating tank, add water to dilute and prepare a titanium dioxide slurry with a TiO2 weight percentage concentration of 20%.
[0077] (4) Heat the slurry to be coated with steam to 85-90℃, add 10% NaOH solution to adjust the pH of the slurry to 10, add sodium silicate solution with a weight percentage concentration of 2% (as SiO2), the weight percentage of sodium silicate solution (as SiO2) to titanium dioxide slurry (as TiO2) is 2.0%, the addition time is 20 minutes, and dilute sulfuric acid is added at the same time to control the pH to 10.0. The maturation time is 3 hours.
[0078] (5) Continue adding a 2% (by weight, based on SiO2) sodium silicate solution. The weight percentage of the sodium silicate solution (based on SiO2) in the titanium dioxide slurry (based on TiO2) is 1.0%, and the addition time is 25 minutes. Allow to mature for 90 minutes. Acidify by adding a 2% (by weight, based on SiO2) dilute sulfuric acid for 237 minutes and 28 seconds. The addition time should be controlled stepwise according to the pH value. Finally, adjust the pH of the slurry to 6.0. The maturation time is 80 minutes.
[0079] Acidification pH 10-9.5 9.5-9.0 9.0-8.5 8.5-8.0 8.0-7.0 7.0-6.0 6.0-5.5 time 115′12″ 80′33″ 25′ 7′30″ 5′10″ 2′48″ 1′15″ % of total time 48.5 33.9 10.5 3.2 2.2 1.2 0.5
[0080] (6) Cool the coating slurry to 65°C, add sodium silicate solution with a sodium silicate (SiO2) weight percentage concentration of 10%, and the weight percentage of sodium silicate solution (SiO2) to titanium dioxide slurry (TiO2) is 5.0%. Add the solution over 30 minutes, and simultaneously add 20% dilute sulfuric acid to control the pH at 6.8. The maturation time is 60 minutes.
[0081] (7) Cool the S6 coating slurry to 55°C, add sodium silicate solution with a sodium silicate (as SiO2) weight percentage concentration of 20%, and the weight percentage of sodium silicate solution (as SiO2) to titanium dioxide slurry (as TiO2) is 1.0%. Add the solution over 45 minutes, add dilute sulfuric acid at the same time, control the pH to 6.5, and allow it to mature for 50 minutes.
[0082] (8) Wash the coating material with water, dry it, and add 0.2% of the alcoholysis silane coupling agent prepared by method 1 and gas powder.
[0083] Example 2
[0084] (1)-(7) are the same as in Example 1
[0085] (8) Wash the coating material with water, dry it, and add 1.0% of the alcoholysis silane coupling agent prepared by method 1.
[0086] Example 3
[0087] (1)-(7) Same as Example 1
[0088] (8) Wash the coating material with water, dry it, and add 0.2% of the alcoholysis silane coupling agent prepared by method 2.
[0089] Example 4
[0090] (1)-(4) are the same as in Example 1
[0091] (6) and (7) are the same as in Example 1
[0092] (5) Continue adding a 2% (by weight, based on SiO2) sodium silicate solution, the weight percentage of which is 1.0% of the titanium dioxide slurry (based on TiO2), over a period of 25 minutes. Then add a 2% (by weight, based on SiO2) dilute sulfuric acid over a period of 182 minutes. The addition time should be controlled stepwise according to the pH value. The final pH of the slurry should be adjusted to 6.0. The maturation time is 80 minutes.
[0093]
[0094]
[0095] (8) Wash the coating material with water, dry it, and add 1.0% of the alcoholysis silane coupling agent prepared by method 2.
[0096] Example 5
[0097] (1)-(7) Same as Example 4
[0098] (8) Wash the coating material with water, dry it, and add 1.0% of the alcoholysis silane coupling agent prepared by method 2.
[0099] Example 6
[0100] (1)-(7) Same as Example 4
[0101] (8) Wash the coating material with water, dry it, and add 0.6% of the alcoholysis silane coupling agent prepared by method 2.
[0102] The preparation methods of the alcoholysis silane coupling agents in Examples 1-6 are as follows:
[0103] (1) Prepare a 1% acetic acid solution.
[0104] (2) Take 50 ml of the prepared HAC solution and add 2.5 ml of R-aminopropyltriethoxysilane dropwise while stirring. After adding the solution, stir for 20-30 min.
[0105] The titanium dioxide prepared in Examples 1-6, after being washed with water, all had a resistivity greater than 100 Ωm, which met the requirements.
[0106] Weathering test methods
[0107] (1) Test instrument: Ultraviolet aging instrument (Q-Panel Lab Products, USA)
[0108] (2) Test conditions: Alkyd resin system, paint spraying board under the premise of equal addition (mass), and natural drying for 48 hours.
[0109] (3) Parameters and time of UV aging instrument:
[0110] UV lamp: UVA-340nm, light intensity 1.55w / m 2 / nm
[0111] Cyclic conditions: UV (60℃ 8hrs) ----- Cond (50℃ 4hrs)
[0112] (4) Two samples were painted for each sample, and the samples were subjected to parallel aging. The following data are the average of the two samples.
[0113] Table 1. Color change of titanium dioxide prepared in Examples 1-6 at different aging times.
[0114]
[0115]
[0116]
[0117] △L * , △a * , △b * , where L is the lightness difference between the reference sample and the tested sample. * and chromaticity index a * b * The color difference is represented by ΔE, which is the total color difference. Colorimeters typically provide the corresponding results. Specifically, ΔL+ indicates a whiter tint, ΔL- indicates a darker tint; Δa+ indicates a reddish tint, Δa- indicates a greenish tint; Δb+ indicates a yellowish tint, Δb- indicates a bluish tint.
[0118] Specific calculation method and brightness difference ΔL * Red-green difference △a * Yellow-blue difference △b * Both are related.
[0119] The computer formula is: △E * =[(△L * )2+(△a * )2+(△b * )2]ˇ1 / 2.
[0120] The titanium dioxide prepared in Examples 1-6 has a measured ΔE between 0 and 1, and the color difference is indistinguishable to the naked eye.
Claims
1. A method for preparing high weather-resistant titanium dioxide, characterized in that... It consists of the following steps: S1. Prepare titanium dioxide slurry; S2. Heat the titanium dioxide slurry in S1 to 85-90℃, control the pH to 10-10.5, add sodium silicate solution to react, and let it mature for 2-3 hours. S3. Add sodium silicate solution to the titanium dioxide slurry obtained in S2, and then add dilute acid dropwise to make the pH of the slurry finally 5.0-6.0, and the maturation time is 60-90 minutes. S4. Cool the titanium dioxide slurry obtained in S3 to 60-70℃, then add sodium silicate solution to adjust the pH to 6.0-7.0, and let it mature for 30-60 minutes. S5. Cool the titanium dioxide slurry obtained in S4 to 50-60℃, then add sodium silicate solution, adjust the pH to 5.5-6.5, and let it mature for 30-60 minutes. S6. Wash the titanium dioxide slurry obtained in S5 with water, filter it to obtain a filter cake, dry the filter cake, and then add the alcoholysis organic treatment agent and stir to obtain the final product. Based on SiO2, the weight of sodium silicate solution in S3 is 0.5-1.0% of the weight of titanium dioxide slurry; The sodium silicate solution in S3 is added over a period of 20-35 minutes. The dilute acid mentioned in S3 is dilute sulfuric acid; The weight concentration of the dilute acid in S3 is 2-8%; The dilute acid mentioned in S3 is added over a period of 3-4 hours; The pH control process in S3 is as follows: ; The alcoholysis organic treatment agent in S6 is an alcoholysis silane coupling agent; The weight percentage of the added alcoholysis silane coupling agent is 0.2-1.0%.
2. The preparation method according to claim 1, characterized in that, Based on SiO2, the weight of sodium silicate solution in S2 is 2.0-3.0% of the weight of titanium dioxide slurry; The sodium silicate solution in S2 is added over a period of 20-30 minutes. Add dilute acid to S2 to adjust the pH, wherein the weight concentration of the dilute acid is 2-8%.
3. The preparation method according to claim 1, characterized in that, Based on SiO2, the weight of sodium silicate solution in S4 is 1.0-5.0% of the weight of titanium dioxide slurry; The sodium silicate solution in S4 is added over a period of 30-45 minutes. The pH in S4 is adjusted by adding dilute sulfuric acid, with a concentration of 10-30%.
4. The preparation method according to claim 1, characterized in that, Based on SiO2, the weight of sodium silicate solution in S5 is 0.5-1.0% of the titanium dioxide slurry; The sodium silicate solution in S5 is added over a period of 30-45 minutes.
5. The preparation method according to claim 1, characterized in that, The titanium dioxide slurry described in S1 has a TiO2 weight percentage concentration of 20-30%.
6. The preparation method according to claim 1, characterized in that, The method for preparing the titanium dioxide slurry described in S1 is to add titanium dioxide to deionized water to form a slurry, add a dispersant, and then perform sand milling, sieving, and dilution with water. The dispersant mentioned in S1 is sodium hexametaphosphate; The weight percentage of the dispersant mentioned in S1 is 0.1-0.5%; The slurry described in S1 has a weight concentration of 600-1000 g / L; The mesh size of the sieve in S1 is 300-500 mesh.
7. The preparation method according to claim 1, characterized in that, The preparation method of the alcoholysis silane coupling agent is as follows: prepare 40-60 ml of acetic acid solution, add 2-3 ml of R-aminopropyltriethoxysilane dropwise while stirring, and stir for 20-30 min after the addition is complete; or; Prepare 150-250 ml of acetic acid solution, add 10-30 ml of anhydrous ethanol, and while stirring, add 5-15 ml of R-aminopropyltriethoxysilane dropwise. After the addition is complete, stir for 20-30 minutes.
8. A titanium dioxide prepared by the preparation method according to any one of claims 1-7.
9. An application of the titanium dioxide according to claim 8, characterized in that, The suitable pH for the titanium dioxide is 5-9.
Citation Information
Patent Citations
Method for coating surface of titanium dioxide with compact alumina
CN111100481A
Method for producing high covering power titanium dioxide pigment
CN1850914A