A method for preparing an ultra-durable catalytic electrode for hydrogen evolution in water electrolysis
A porous, rough nickel sheet matrix was prepared by powder metallurgy and hydrothermal synthesis, and an in-situ self-generated catalytic phase was formed. This solved the problem of balancing durability and catalytic activity in the water electrolysis hydrogen production electrode, and achieved efficient and stable electrocatalytic performance.
Patent Information
- Application Number
- CN202311610949.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-28
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-11-28
AI Technical Summary
Existing catalytic electrodes for hydrogen production by water electrolysis struggle to balance durability and catalytic activity. Traditional preparation processes are cumbersome and inefficient, leading to the electrodes being prone to cracking or peeling during prolonged use, thus failing to meet the needs of industrial applications.
An ultra-durable catalytic electrode for hydrogen evolution in water electrolysis was prepared by using a combination of powder metallurgy, machining and hydrothermal synthesis. The nickel powder was pressed to form a porous structure, and then processed into a rough nickel sheet by wire electrical discharge machining. An in-situ self-generated catalytic phase was then formed on the sheet.
It improves the catalyst loading and binding strength, enhances catalytic activity and durability, simplifies the preparation process, improves production efficiency, and is suitable for existing electrolytic cell equipment.
Smart Images

Figure CN117626324B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of catalytic material preparation technology, specifically to a method for preparing an ultra-durable catalytic electrode for hydrogen evolution in water electrolysis. Background Technology
[0002] Hydrogen energy is considered one of the most promising clean energy sources. Electrolysis of water is a commonly used green hydrogen production method, offering advantages such as simple process, high-purity products, and environmental friendliness, and is gradually becoming an important route for large-scale hydrogen production. However, the activation energy barrier exists during the reaction, and various resistances throughout the process also consume some potential, leading to increased energy consumption and reduced efficiency in hydrogen production. Therefore, highly efficient electrocatalysts are needed to reduce the overpotential in the reaction kinetics and improve hydrogen production efficiency. Noble metal materials (such as Pt and Ru) can effectively reduce the overpotential, but they are expensive. In recent years, relatively inexpensive and high-performance transition metals and their alloys or compounds have received widespread attention, among which in-situ self-generated homologous transition metal sulfides (TMSs) or selenides (TMSes) are particularly prominent due to their good catalytic activity.
[0003] Previous research has made great progress in the in-situ loading of various compound catalytic phases onto nickel foam (NF) or nickel mesh as a matrix. However, due to the smooth surface and fine framework of NF or nickel mesh, the catalytic phase lacks sufficient self-generated reaction sites, resulting in low catalytic phase loading and internal stress during growth. Ultimately, this leads to cracking or peeling failure of the catalytic phase during the hydrogen evolution reaction. Therefore, the hydrogen evolution durability of such electrodes is generally poor and cannot meet the requirements of long-term stable hydrogen evolution in industrial applications. Their application prospects are not optimistic. Therefore, it is urgent to develop an electrolytic hydrogen production catalytic electrode that combines high activity and durability. Summary of the Invention
[0004] The purpose of this invention is to provide a method for preparing an ultra-durable catalytic electrode for hydrogen evolution in water electrolysis. Nickel powder is pressed into shape and then sintered to form a porous structure on a nickel substrate. Subsequent wire electrical discharge machining (EDM) is used to process the nickel powder into multiple rough-surfaced nickel sheets. The rough surface of the nickel sheets is beneficial for catalyst loading and catalytic activity, laying the foundation for improved catalytic performance of the final product. The rough-surfaced nickel sheets undergo a hydrothermal selenization reaction with sodium selenite, generating a homologous catalytic phase in situ on the nickel substrate, further enhancing the electrode's catalytic effect. The catalytic electrode prepared by this invention features easy processing, high production efficiency, high catalytic hydrogen evolution activity, and long service life, solving the technical challenge of simultaneously achieving catalytic activity and durability in key materials for existing electrolyzers.
[0005] This invention is specifically achieved through the following technical solution: a method for preparing an ultra-durable electrolytic hydrogen evolution catalytic electrode for water electrolysis, according to this invention, includes the following steps:
[0006] (1) Weigh a certain amount of nickel powder and put it into a stainless steel mold. Press it on a hydraulic press at 15-800MPa for 5-300s. After demolding, you will get a pressed blank.
[0007] (2) The pressed billet is sintered at 500-1100℃ and then cooled to room temperature to obtain a nickel matrix.
[0008] (3) The obtained nickel substrate is cut by electrical discharge wire cutting to obtain a certain number of nickel sheet substrates with rough surfaces;
[0009] (4) Weigh a certain amount of selenium source material and dissolve it in distilled water. After stirring thoroughly, obtain solution A. Transfer solution A together with the nickel sheet substrate obtained in step (3) into the polytetrafluoroethylene liner of the hydrothermal reactor. Tighten the hydrothermal reactor and place it in a drying oven at 170-210°C for hydrothermal selenization reaction.
[0010] (5) Take out the nickel sheet after hydrothermal selenization reaction from the polytetrafluoroethylene liner, rinse it with distilled water 3-4 times, then rinse it with anhydrous ethanol 2-3 times, and then put it into a vacuum drying oven. After drying, the final product is obtained - ultra-durable electrolytic hydrogen evolution catalytic electrode.
[0011] In the aforementioned method for preparing the ultra-durable electrolytic hydrogen evolution catalytic electrode for water electrolysis, the particle size of the nickel powder selected in step (1) is 300 to 5000 mesh, and the particle size affects the size of the product pores.
[0012] In the aforementioned method for preparing the ultra-durable electrolytic hydrogen evolution catalytic electrode for water electrolysis, the heating rate during sintering in step (2) is 3–15 °C / min, and the sintering holding time is 60–180 min. The sintering temperature, heating rate, and sintering time need to be strictly controlled. If the temperature is too low, the sample is not easy to form; if the temperature is too high, the formed sample has high density, reduced porous structure, and small specific surface area, which is not conducive to the adhesion of the catalyst and the improvement of its performance. Similarly, the heating rate and holding time will also affect the size of the product pores, thereby affecting the catalytic performance.
[0013] In the aforementioned method for preparing the ultra-durable electrolytic hydrogen evolution catalytic electrode, the hydrothermal selenization reaction time in step (4) is 5–18 h. If the hydrothermal time is too short, the catalyst cannot fully adhere and grow on the substrate surface; if the hydrothermal time is too long, the catalyst morphology will be uneven, reducing the catalytic efficiency.
[0014] In the aforementioned method for preparing the ultra-durable electrolytic hydrogen evolution catalytic electrode for water electrolysis, sodium selenite is selected as the selenium source material in step (4), and the concentration of sodium selenite in solution A is 1–16 mmol / L. The amount and concentration of the raw material must be strictly controlled. If the concentration and amount are too small, the catalytic phase will not adhere to the substrate surface or will only adhere in small amounts; if the amount and concentration are too large, the catalytic phase will accumulate and agglomerate on the substrate surface, and a large number of cracks will be generated, which is not conducive to the improvement of catalytic activity and durability, or the performance improvement will not be obvious, and the cost will increase.
[0015] In the aforementioned method for preparing the ultra-durable electrolytic hydrogen evolution catalytic electrode for water electrolysis, step (5) involves drying at a temperature of 50–80°C in a vacuum drying oven for 8–24 hours. The drying temperature and time must be strictly controlled. If the temperature is too low or the time too short, it will be difficult to remove moisture between particles; if the temperature is too high or the time too long, surface oxidation will occur, damaging the morphology of the attached catalyst and hindering the effective performance of the catalytic activity.
[0016] This invention also provides an ultra-durable catalytic electrode for hydrogen evolution in water electrolysis prepared according to the above method and its application in the hydrogen evolution reaction in water electrolysis. The catalytic active phase of the obtained ultra-durable catalytic electrode for hydrogen evolution in water electrolysis is uniformly grown in situ on a nickel substrate in a lamellar form, exposing more edge active sites, which lays the foundation for improving catalytic performance.
[0017] The performance of the catalytic electrode prepared in this invention for electrocatalytic water splitting was characterized using a three-electrode electrochemical workstation. A 1 mol / L KOH solution was used as the electrolyte. The ultra-durable water electrolysis hydrogen evolution catalytic electrode prepared in this invention was used as the working electrode, a graphite rod as the counter electrode, and a calomel electrode as the reference electrode. The catalytic performance of the ultra-durable water electrolysis hydrogen evolution catalytic electrode was tested by linear sweep voltammetry (LSV). The results showed that the ultra-durable water electrolysis hydrogen evolution catalytic electrode exhibited good performance at a current density of 100 mA / cm². 2 The required overpotential is 215 mV, indicating that the prepared electrode has excellent electrocatalytic hydrogen evolution activity. The durability of the ultra-durable water electrolysis hydrogen evolution catalytic electrode was tested by chronoamperometry (CA). The results showed that the electrode prepared in this invention showed almost no degradation after 410 h of hydrogen evolution, indicating that the electrode has excellent electrocatalytic hydrogen evolution durability.
[0018] Compared with existing technologies, this invention has significant advantages and beneficial effects. Through the above technical solution, this invention achieves considerable technological advancement and practicality, and has broad application value, possessing at least the following advantages:
[0019] (1) Traditional catalyst preparation processes generally involve first preparing a matrix, and then generating a catalytic phase loaded onto the matrix through multiple steps using methods such as wet chemical methods and chemical vapor deposition. The preparation process is cumbersome and involves many variables. In contrast, this invention uses a combination of powder metallurgy, machining, and hydrothermal synthesis, which simplifies the process steps, saves a lot of manpower and resources, and can produce a large number of electrodes at once with extremely high efficiency.
[0020] (2) In this invention, nickel powder is pressed and sintered to form a porous structure on a nickel substrate. This structure is then processed into multiple rough-surfaced nickel sheets by electrical discharge wire cutting. The rough surface of the nickel sheets facilitates catalyst loading and catalytic activity, laying the foundation for improved catalytic performance of the final product. The rough-surfaced nickel sheets undergo a hydrothermal selenization reaction with sodium selenite, generating a homologous catalytic active phase in situ on the nickel substrate. Compared to existing traditional nickel substrates such as nickel foam and nickel mesh, the electrode of this invention has significant advantages, including superior mechanical properties and high bonding strength with the catalytic phase.
[0021] (3) The ultra-durable electrolytic hydrogen evolution catalytic electrode prepared by the present invention has the characteristics of simple preparation process, easy processing, high production efficiency, high catalytic hydrogen production activity, long service life and good stability. It can be directly used as electrode plate material in existing electrolytic cell equipment, solving the technical problem that the catalytic activity and durability of the key electrode materials of existing electrolytic cells are difficult to balance, and has broad application prospects. Attached Figure Description
[0022] Figure 1 This is an SEM image of the nickel sheet substrate after wire electrical discharge machining prepared in Example 1;
[0023] Figure 2 This is an SEM image of the ultra-durable hydrogen evolution catalytic electrode for water electrolysis prepared in Example 1;
[0024] Figure 3 This is a performance diagram of the ultra-durable hydrogen evolution catalytic electrode for water splitting prepared in Example 2;
[0025] Figure 4 This is a durability diagram of the ultra-durable hydrogen evolution catalytic electrode for water splitting prepared in Example 3. Detailed Implementation
[0026] To make the objectives, technical solutions, and advantages of the embodiments of the present invention clearer, the technical solutions of the present invention will be clearly and completely described below in conjunction with specific embodiments. Obviously, the described embodiments are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0027] The method for preparing the ultra-durable hydrogen evolution catalytic electrode for water electrolysis provided by this invention mainly includes the following steps:
[0028] (1) Weigh a certain amount of nickel powder and put it into a stainless steel mold of appropriate size. Press it on a hydraulic press at 15-800MPa for 5-300s. After demolding, a pressed blank is obtained. The particle size of the nickel powder will affect the size of the pores of the final product. The preferred particle size of the nickel powder selected in this step is 300-5000 mesh.
[0029] The amount of nickel powder used can be determined based on the size of the final product, such as the diameter and thickness of the final product, to select a suitable mold size, and the required mass of nickel powder can be estimated by multiplying the volume and density.
[0030] (2) The pressed billet is sintered at 500-1100℃ with a heating rate of 3-15℃ / min and a sintering holding time of 60-180min. After completion, it is cooled to room temperature to obtain a nickel matrix.
[0031] The sintering temperature here needs to be strictly controlled. If the temperature is too low, the sample will not be easy to form; if the temperature is too high, the formed sample will have high density, few porous structures, and small specific surface area, which is not conducive to improving the catalyst performance. Similarly, the heating rate and holding time will also affect the size of the product pores, and thus affect the catalytic performance.
[0032] (3) The nickel substrate obtained in step (2) is processed into a certain size by electrical discharge wire cutting. During cutting, the nickel substrate is cut along the cross-section to obtain a certain number of nickel sheet substrates with rough surfaces.
[0033] The wire electrical discharge machining process here can not only improve production efficiency and reduce costs, but also change the surface roughness of the substrate by controlling the wire feed speed, which is beneficial to the loading and catalytic effect of the catalyst, laying the foundation for improving the catalytic performance of the final product.
[0034] (4) Weigh a certain amount of selenium source material (sodium selenite (Na2SeO3)) and dissolve it in distilled water. After stirring thoroughly, obtain solution A. Transfer solution A together with the nickel sheet substrate obtained in step (3) into the polytetrafluoroethylene liner of the hydrothermal reactor, tighten the hydrothermal reactor, and put it into a drying oven for hydrothermal selenization reaction.
[0035] The amount of sodium selenite used here is 0.05–0.8 mmol, and the concentration of Na₂SeO₃ in solution A is preferably 1–16 mmol / L. The amount and concentration of sodium selenite must be strictly controlled. If the amount and concentration of sodium selenite are too small, the catalyst material will not adhere to the substrate surface or will only adhere in small amounts. If the amount and concentration of sodium selenite are too large, the catalyst material will easily accumulate and agglomerate on the nickel substrate surface, and generate a large number of cracks, which is not conducive to improving catalytic activity and durability, or the performance improvement will not be significant, and the cost will be increased.
[0036] The preferred temperature for the hydrothermal selenization reaction in this step is 170–210°C, and the preferred reaction time is 5–18 h. If the hydrothermal temperature is too low or the time is too short, the catalyst cannot fully adhere and grow on the substrate surface; if the hydrothermal temperature is too high or the time is too long, the catalyst morphology will be uneven, thereby reducing the catalytic efficiency.
[0037] (5) Take out the nickel sheet after hydrothermal selenization reaction from the polytetrafluoroethylene liner, rinse it 4 times with distilled water, rinse it 2 times with anhydrous ethanol, and then put it into a vacuum drying oven. After drying, the final product - ultra-durable electrolytic hydrogen evolution catalytic electrode is obtained.
[0038] Rinsing with distilled water is primarily to remove residual sodium ions from the sample surface, while rinsing with anhydrous ethanol removes any remaining water molecules from the previous water rinse. The preferred drying temperature in the vacuum drying oven is 50–80℃, and the preferred drying time is 8–24 hours. Strict control of the drying temperature and time is crucial. If the temperature is too low or the time too short, it will be difficult to remove moisture between particles; if the temperature is too high or the time too long, surface oxidation can occur, damaging the morphology of the attached catalyst and hindering its effective catalytic performance.
[0039] The present invention employs a moderate temperature, heating rate, and holding time during the sintering of the nickel powder pressed billet. This allows the pressed billet to easily form a porous structure after sintering. Furthermore, different machining processes can be used to alter the surface roughness of the nickel sheet substrate, thereby creating a nickel sheet substrate suitable for in-situ growth of the catalytic phase. During the selenization process, a one-step hydrothermal treatment using a selenium source is employed to precipitate a nano-catalytic phase in situ on the nickel sheet substrate. The catalytic phase exhibits a uniform morphology, appearing as a layered structure on the nickel sheet substrate, exposing more edge active sites and laying the foundation for improved catalytic performance.
[0040] This invention, through control of raw materials, sintering conditions, and wire electrical discharge machining processes, produces a porous nickel substrate with a rough surface. This provides more sites for catalyst adhesion and significantly increases the contact area between the material and the electrolyte, allowing for a more complete catalytic reaction. Furthermore, the water splitting products, hydrogen and oxygen, readily escape from the pores and surface of the material, further optimizing its catalytic efficiency.
[0041] The present invention also discloses an ultra-durable hydrogen evolution catalytic electrode for water electrolysis prepared by the above method, and the application of the ultra-durable hydrogen evolution catalytic electrode for water electrolysis in hydrogen evolution reaction and oxygen evolution reaction under alkaline environment.
[0042] The present invention will now be described in detail with reference to specific embodiments:
[0043] Example 1:
[0044] (1) Weigh 50g of 5000 mesh nickel powder, put it into a stainless steel mold with a diameter of 25mm, press it on a hydraulic press at 150MPa for 30s, and obtain the pressed blank after demolding.
[0045] (2) The pressed blank obtained in step (1) is sintered at a temperature of 500℃, a heating rate of 15℃ / min, and a sintering holding time of 180min. After sintering, it is cooled to room temperature to obtain a nickel matrix.
[0046] (3) The obtained nickel substrate is processed into multiple nickel sheet substrates with a size of Φ25mm, a thickness of 1mm and a rough surface by wire EDM.
[0047] (4) Weigh 0.1 mmol of Na2SeO3 and dissolve it in 50 mL of distilled water. After stirring thoroughly, obtain solution A. Then, transfer solution A together with the nickel substrate obtained in step (3) into the polytetrafluoroethylene liner of a stainless steel hydrothermal reactor. Tighten the hydrothermal reactor and place it in a drying oven for hydrothermal selenization reaction. The temperature of the hydrothermal selenization reaction is 210℃ and the reaction time is 5 h.
[0048] (5) Remove the reacted nickel sheet from the polytetrafluoroethylene liner, rinse it four times with distilled water, then rinse it twice with anhydrous ethanol, and then place it in a vacuum drying oven at 50°C for 24 hours. After drying, the final product is obtained - an ultra-durable electrolytic hydrogen evolution catalytic electrode for water electrolysis.
[0049] The nickel sheet substrate prepared by wire EDM in step (3) of this embodiment and the finally prepared ultra-durable water electrolysis hydrogen evolution catalytic electrode were characterized by SEM images, and the results are as follows: Figure 1 and Figure 2 As shown. From Figure 1 It is known that the nickel sheet substrate after wire electrical discharge machining is porous and has a rough surface, providing more sites for catalyst adhesion. From Figure 2 As can be seen, after the ultra-durable electrolytic hydrogen evolution catalytic electrode prepared in this embodiment is magnified 10,000 times, it can be seen that the catalytic electrode has a porous structure, and the catalytic active phase is uniformly grown in situ on the nickel substrate in a sheet-like manner, exposing more edge active sites, which lays the foundation for improving catalytic performance.
[0050] Example 2:
[0051] (1) Weigh 40g of 2000-mesh nickel powder and put it into a stainless steel mold with a diameter of 30mm. Press it on a hydraulic press at 15MPa for 300s. After demolding, the pressed blank is obtained.
[0052] (2) The pressed blank obtained in step (1) is sintered at a temperature of 600℃, a heating rate of 10℃ / min, and a holding time of 120min. After sintering, it is cooled to room temperature to obtain a nickel matrix.
[0053] (3) The obtained nickel substrate is processed into multiple nickel sheet substrates with a size of Φ30mm, a thickness of 1mm and a rough surface by electric discharge wire cutting.
[0054] (4) Weigh 0.8 mmol of Na2SeO3 and dissolve it in 50 mL of distilled water. After stirring thoroughly, obtain solution A. Then, transfer solution A together with the nickel substrate obtained in step (3) into the polytetrafluoroethylene liner of a stainless steel hydrothermal reactor. Tighten the hydrothermal reactor and place it in a drying oven for hydrothermal selenization reaction. The temperature of the hydrothermal selenization reaction is 180℃ and the reaction time is 12 h.
[0055] (5) Remove the reacted nickel sheet from the polytetrafluoroethylene liner, rinse it four times with distilled water, then rinse it twice with anhydrous ethanol, and then place it in a vacuum drying oven at 60°C for 12 hours. After drying, the final product is obtained - an ultra-durable electrolytic hydrogen evolution catalytic electrode for water electrolysis.
[0056] The electrocatalytic water splitting performance of the electrode prepared in this invention was characterized using a three-electrode electrochemical workstation. The electrolyte used in this experiment was a 1 mol / L KOH solution. The ultra-durable water electrolysis hydrogen evolution catalytic electrode prepared in this embodiment was used as the working electrode, a graphite rod as the counter electrode, and a calomel electrode as the reference electrode. The catalytic performance of the ultra-durable water electrolysis hydrogen evolution catalytic electrode was tested by linear sweep voltammetry (LSV), and the results are as follows: Figure 3 As shown in the figure, the ultra-durable electrolytic hydrogen evolution catalytic electrode for water electrolysis prepared in this embodiment can withstand a current density of 100 mA / cm². 2 The required overpotential is 215mV, indicating that the electrode has excellent electrocatalytic hydrogen evolution activity.
[0057] Example 3:
[0058] (1) Weigh 10g of 300-mesh nickel powder and put it into a stainless steel mold with a diameter of 20mm. Press it on a hydraulic press at 800MPa for 5s. After demolding, the pressed blank is obtained.
[0059] (2) The pressed blank obtained in step (1) is sintered at a temperature of 1100℃, a heating rate of 3℃ / min, and a holding time of 60min. After sintering, it is cooled to room temperature to obtain a nickel matrix.
[0060] (3) The obtained nickel substrate is processed into multiple nickel sheet substrates with a size of Φ20mm, a thickness of 1mm and a rough surface by wire electrical discharge machining.
[0061] (4) Weigh 0.05 mmol of Na2SeO3 and dissolve it in 50 mL of distilled water. After stirring thoroughly, obtain solution A. Then, transfer solution A together with the nickel substrate obtained in step (3) into the polytetrafluoroethylene liner of a stainless steel hydrothermal reactor. Tighten the hydrothermal reactor and place it in a drying oven for hydrothermal selenization reaction. The temperature of the hydrothermal selenization reaction is 170℃ and the reaction time is 18 h.
[0062] (5) Remove the reacted nickel sheet from the polytetrafluoroethylene liner, rinse it four times with distilled water, then rinse it twice with anhydrous ethanol, and then place it in a vacuum drying oven at 80°C for 8 hours. After drying, the final product is obtained - an ultra-durable electrolytic hydrogen evolution catalytic electrode for water electrolysis.
[0063] To test the durability of the ultra-durable water electrolysis hydrogen evolution catalytic electrode prepared in this invention, a three-electrode test experiment was conducted using an electrochemical workstation. The electrolyte used in this experiment was a 1 mol / L KOH solution. The obtained ultra-durable water electrolysis hydrogen evolution catalytic electrode was directly used as the working electrode, a graphite rod was used as the counter electrode, and a calomel electrode was used as the reference electrode. The durability of the ultra-durable water electrolysis hydrogen evolution catalytic electrode was tested by chronoamperometry (CA), and the results showed a durability at 200 mA cm⁻¹. -2 The CA curves under current density are shown in the figure. Figure 4 As shown, the ultra-durable electrolytic hydrogen evolution catalytic electrode prepared in this embodiment shows virtually no degradation after 410 hours of hydrogen evolution, indicating that the electrode has excellent electrocatalytic hydrogen evolution durability.
[0064] This invention involves pressing nickel powder into a compact, sintering it, and then machining it using wire electrical discharge machining (EDM) to obtain multiple nickel sheets with rough surfaces. The rough surfaces are beneficial for catalyst loading and catalytic activity, laying the foundation for improved catalytic performance of the final product. Furthermore, EDM can produce multiple nickel sheets at once, allowing for simultaneous hydrothermal selenization with a sodium selenite solution, resulting in high electrode preparation efficiency. The final electrode exhibits a uniform, in-situ, lamellar growth of the catalytic active phase on the nickel sheet substrate, exposing more edge active sites and demonstrating excellent electrocatalytic hydrogen evolution performance and long-term durability.
[0065] The above description is merely an embodiment of the present invention and is not intended to limit the present invention in any way. The present invention can also have other embodiments based on the above structure and function, which will not be listed hereafter. Therefore, any simple modifications, equivalent changes, and alterations made by those skilled in the art to the above embodiments based on the technical essence of the present invention without departing from the scope of the present invention shall still fall within the scope of the present invention.
Claims
1. A method for preparing a catalytic electrode for hydrogen evolution in water electrolysis, characterized in that... Includes the following steps: (1) Weigh a certain amount of nickel powder and put it into a stainless steel mold. Press it on a hydraulic press at 15-800 MPa for 5-300 s. After demolding, the pressed blank is obtained. (2) The pressed billet is sintered at 500~1100 ℃. The heating rate during sintering is 3~15 ℃ / min, and the sintering holding time is 60-180 min. After completion, it is cooled to room temperature to obtain nickel matrix. (3) The obtained nickel substrate is cut by electrical discharge wire cutting to obtain a certain number of nickel sheet substrates with rough surfaces; (4) Weigh a certain amount of sodium selenite and dissolve it in distilled water. After stirring thoroughly, solution A is obtained. The concentration of sodium selenite in solution A is 1~16 mmol / L. Transfer solution A and the nickel substrate obtained in step (3) together to the polytetrafluoroethylene liner of the hydrothermal reactor. Tighten the hydrothermal reactor and place it in a drying oven at 170~210 ℃ for hydrothermal selenization reaction. The reaction time is 5~18 h. (5) Take out the nickel sheet after hydrothermal selenization reaction from the polytetrafluoroethylene liner, rinse it with distilled water 3-4 times, then rinse it with anhydrous ethanol 2-3 times, and then put it into a vacuum drying oven. After drying, the final product - electrolytic hydrogen evolution catalytic electrode is obtained.
2. The method for preparing the electrolytic hydrogen evolution electrode for water electrolysis as described in claim 1, characterized in that... The particle size of the nickel powder selected in step (1) is 300~5000 mesh.
3. The method for preparing the catalytic electrode for hydrogen evolution in water electrolysis as described in claim 1, characterized in that... Step (5) The drying temperature of the vacuum drying oven is 50~80 ℃ and the drying time is 8~24 h.
4. The hydrogen evolution catalytic electrode for water electrolysis obtained by any one of the preparation methods of claims 1-3.
5. The application of the catalytic electrode for hydrogen evolution in water electrolysis obtained by any one of the preparation methods of claims 1-3 in the hydrogen evolution reaction in water electrolysis.