A perovskite quantum dot photoresist and its preparation and application methods
By preparing a mixture of CsPbBr3 perovskite quantum dot solution, photosensitizer solution, oleic acid and oleylamine, perovskite quantum dot photoresist was directly prepared, solving the problem of quenching of perovskite quantum dots in the finished photoresist and achieving high light conversion efficiency and photolithography precision.
Patent Information
- Application Number
- CN202311670717.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-07
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-12-07
AI Technical Summary
Perovskite quantum dots are prone to quenching during mixing with and storage of finished photoresist, resulting in low light conversion efficiency. Existing technologies are unable to effectively solve the problems of structural stability and sensitivity to optical/electrical properties.
Perovskite quantum dot photoresist was directly prepared by mixing CsPbBr3 perovskite quantum dot solution, photosensitizer solution, oleic acid and oleylamine. The photosensitizer was cleaved during exposure and covalently crosslinked with alkyl ligands on the surface of the perovskite quantum dots to achieve patterning, thus avoiding mixing with the finished photoresist.
It effectively improves the light conversion efficiency, avoids the fluorescence quenching problem caused by highly polar solvents, and improves the lithography accuracy and light conversion efficiency.
Smart Images

Figure CN117631449B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of photoresist technology, specifically to a perovskite quantum dot photoresist and its preparation and application methods. Background Technology
[0002] Perovskite quantum dots have attracted widespread attention in the field of display materials due to their narrow half-slit width, tunable luminescence properties, and high quantum yield, and are highly anticipated in photoluminescence and electroluminescence applications. Currently, using ultraviolet / blue Micro LEDs combined with quantum dot color conversion arrays to achieve full-color displays is a popular technology, avoiding the problems of high circuit design difficulty and varying material aging rates associated with traditional three-color RGB methods. A common method for fabricating quantum dot color conversion arrays involves mixing perovskite quantum dots with pre-made photoresist, spin-coating to create a perovskite quantum dot-containing film, and then patterning it using traditional exposure and development techniques to obtain the quantum dot color conversion array.
[0003] However, perovskite quantum dots have unique ionic properties. Their surface chemistry is unstable, their structural stability in highly polar solvents is poor, their structural integrity is fragile, and their optical / electrical properties are sensitive. This makes perovskite quantum dots prone to quenching during mixing with finished photoresist and during storage after mixing, resulting in low light conversion efficiency. Summary of the Invention
[0004] The purpose of this invention is to overcome the shortcomings of the prior art. This invention provides a perovskite quantum dot photoresist and its preparation and application methods. By mixing CsPbBr3 perovskite quantum dot solution, photosensitizer solution, oleic acid and oleylamine, perovskite quantum dot photoresist is directly prepared. There is no need to mix perovskite quantum dots into the finished photoresist, which can effectively avoid the problem of fluorescence quenching of perovskite quantum dots caused by the finished photoresist, thereby effectively improving the light conversion efficiency.
[0005] This invention provides a method for preparing perovskite quantum dot photoresist, comprising the following steps:
[0006] S11. Prepare a CsPbBr3 perovskite quantum dot solution, wherein the concentration of the CsPbBr3 perovskite quantum dot solution is 100-150 mg / mL;
[0007] S12. Prepare a photosensitizer solution by dissolving the photosensitizer in an organic solvent to obtain a photosensitizer solution, wherein the ratio of the organic solvent to the photosensitizer is in the range of 1 mL: 30–50 mg;
[0008] The photosensitizer is one of 2,3,4,4'-tetrahydroxybenzophenone 1,2-naphthoquinone diazido-5-sulfonate, 6-diaza-5,6-dihydro-5-oxo-1-naphthalenesulfonate, 1,2-naphthoquinone-2-diazido-5-sulfonyl chloride, and 6-diaza-5,6-dihydro-5-oxo-1-naphthalenesulfonic acid;
[0009] S13. Prepare perovskite quantum dot photoresist: By volume, take 10-20 parts of the photosensitizer solution, 1500-3000 parts of the CsPbBr3 perovskite quantum dot solution, 0.5-1 parts of oleic acid and 1-1.5 parts of oleylamine and put them into a container. Stir for 20-40 hours under 580-590nm yellow light, nitrogen atmosphere and 10-20℃ to form perovskite quantum dot photoresist.
[0010] Specifically, the preparation of the CsPbBr3 perovskite quantum dot solution includes:
[0011] S111. Preparation of cesium oleate precursor: Cs2CO3, oleic acid and octadecene are mixed and heated at 100-120℃ for 1-2 hours, then heated to 150-180℃ until Cs2CO3 is completely dissolved to obtain cesium oleate precursor; the ratio of oleic acid to Cs2CO3 is 1mL:0.08-0.15g, and the ratio of oleic acid to octadecene is 1mL:6.66-15.00mL;
[0012] S112. To prepare the lead bromide precursor, PbBr2 and octadecene are mixed and stirred at 100-120°C under vacuum for 1-2 hours to obtain a first mixed solution. The ratio of octadecene to PbBr2 is 1 mL: 0.008-0.0125 g. Under nitrogen protection, oleic acid and oleylamine are injected into the first mixed solution to obtain the lead bromide precursor. The ratio of oleic acid, oleylamine and octadecene is 1 mL: 1 mL: 8-10 mL.
[0013] S113. To prepare a crude CsPbBr3 solution, the lead bromide precursor is heated to 140–190°C, and the cesium oleate precursor is rapidly injected into the heated lead bromide precursor. After reacting for 5–10 seconds, the solution is immersed in a cold water bath to cool to room temperature to obtain a crude CsPbBr3 solution. The ratio of cesium oleate precursor to lead bromide precursor is 1 mL: 9.09–10.91 mL.
[0014] S114. Purification: Add 2-3 times the volume of ethyl acetate solution to the crude CsPbBr3 solution, mix well, and centrifuge at 6000-10000 rpm for at least 15 min to obtain a first precipitate; redisperse the first precipitate in toluene, add 2-3 times the volume of ethyl acetate solution, mix well, and centrifuge at 6000-10000 rpm for at least 15 min to obtain a second precipitate; repeat the dispersion and precipitation of the second precipitate 2-6 times, and then disperse it again in toluene to obtain a CsPbBr3 perovskite quantum dot solution.
[0015] Specifically, in the preparation of the photosensitizer solution, the organic solvent is one or a mixture of n-hexane, n-octane, chlorobenzene, and toluene.
[0016] The present invention also provides a perovskite quantum dot photoresist, wherein the perovskite quantum dot photoresist is prepared by the preparation method described above.
[0017] This invention also provides a method for applying perovskite quantum dot photoresist, wherein the perovskite quantum dot photoresist prepared by the aforementioned method is applied to Micro LED full-color displays, and the application method includes the following steps:
[0018] S21. Spin coating: Spin coat the perovskite quantum dot photoresist onto a glass substrate or Micro LED array wafer, and heat treat it at 80-100°C for 2-4 minutes to obtain a first quantum dot photoresist film.
[0019] S22, Exposure: Based on the photomask, expose the first quantum dot photoresist film under light of 300-430nm for 10-30s to obtain the exposed film;
[0020] S23. First baking: The exposed film is baked at 50-80°C for 30-90 seconds to obtain a baked film.
[0021] S24. Prepare the developer by dissolving the passivating ligand in the developer solution to obtain the developer. The ratio of developer solution to passivating ligand is in the range of 1 mL: 0.01–0.02 mg.
[0022] S25. Development: Immerse the baked film in the developer for 10-30 seconds to obtain a developed film.
[0023] S26. Second baking: The developing film is baked at 50-80°C for 30-90 seconds to obtain the first quantum dot color conversion film.
[0024] S27. Deposit a passivation layer, depositing a first passivation layer on the first quantum dot color conversion film;
[0025] S28. Prepare a second quantum dot color conversion film by spin-coating the perovskite quantum dot photoresist onto the first passivation layer and heat-treating it at 80-100°C for 2-4 minutes to obtain a second quantum dot photoresist film; then repeat the operations from S22 to S26 to form a second quantum dot color conversion film, and deposit a second passivation layer on the second quantum dot color conversion film.
[0026] The first quantum dot color conversion film and the second quantum dot color conversion film form a perovskite quantum dot color conversion array, and the perovskite quantum dot color conversion array is combined with blue Micro LED or ultraviolet Micro LED to form a full-color display module.
[0027] Specifically, the spin coating speed of the perovskite quantum dot photoresist is in the range of 1000 to 3000 rpm, the spin coating acceleration range of the perovskite quantum dot photoresist is in the range of 1000 to 2000 rpm / s, and the spin coating time of the perovskite quantum dot photoresist is 45 to 55 s.
[0028] Specifically, in step S22, the power density of the light is in the range of 20–30 mW / cm². 2 .
[0029] Specifically, when preparing the first quantum dot color conversion film, the passivation ligand is one of oleylamine iodine, octylamine iodine, 2-phenylethylamine hydroiodate, and 3-fluorophenylethylamine iodide; when preparing the second quantum dot color conversion film, the passivation ligand is one of oleylamine bromide, octylamine bromide, 2-phenylethylamine hydrobromide, and 3-fluorophenylethylamine bromide.
[0030] Specifically, when preparing the first quantum dot color conversion film, the passivation ligand is one of oleylamine bromide, octylamine bromide, 2-phenylethylamine hydrobromide, and 3-fluorophenylethylamine bromide; when preparing the second quantum dot color conversion film, the passivation ligand is one of oleylamine iodide, octylamine iodide, 2-phenylethylamine hydroiodide, and 3-fluorophenylethylamine iodide.
[0031] Specifically, the developing solution is one or a mixture of n-hexane, n-octane, toluene, chlorobenzene, ethyl acetate, and methyl acetate;
[0032] The thickness of the first passivation layer ranges from 5 to 20 nm, and the material of the first passivation layer is SiO2 or SiN. x h-BN, AlO x One of them;
[0033] The thickness of the second passivation layer ranges from 5 to 20 nm, and the material of the second passivation layer is SiO2 or SiN. x h-BN, AlO x One of them.
[0034] Compared with the prior art, the beneficial effects of the present invention are:
[0035] The perovskite quantum dot photoresist of the present invention is directly prepared by mixing a CsPbBr3 perovskite quantum dot solution, a photosensitizer solution, oleic acid, and oleylamine. During exposure, the photosensitizer in the photoresist film breaks down and covalently crosslinks adjacent CsPbBr3 perovskite quantum dots with alkyl ligands on the surface of the CsPbBr3 perovskite quantum dots, thereby directly patterning the CsPbBr3 perovskite quantum dots. This eliminates the need to mix the CsPbBr3 perovskite quantum dots into the finished photoresist, effectively avoiding the fluorescence quenching problem caused by the finished photoresist and thus significantly improving the light conversion efficiency.
[0036] The exposed film has low polarity requirements for the developer and does not require the use of highly polar solvents for development. Low polar solvents can be used to develop the exposed film, which avoids the fluorescence quenching problem of perovskite quantum dots caused by highly polar solvents and is also beneficial to improving the light conversion efficiency. Attached Figure Description
[0037] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.
[0038] Figure 1 This is a flowchart of the preparation method of perovskite quantum dot photoresist in this embodiment of the invention;
[0039] Figure 2 This is a flowchart of the preparation method of CsPbBr3 perovskite quantum dot solution in an embodiment of the present invention;
[0040] Figure 3 This is a flowchart illustrating the application method of perovskite quantum dot photoresist in this invention embodiment;
[0041] Figure 4 This is a scanning electron microscope image of the quantum dot photoresist film after exposure in Example 1;
[0042] Figure 5 This is the XRD pattern of the quantum dot photoresist film in Example 1;
[0043] Figure 6 This is the photoluminescence (PL) spectrum of the quantum dot photoresist film in Example 1;
[0044] Figure 7This is a scanning electron microscope image of the quantum dot photoresist film after exposure in Example 2;
[0045] Figure 8 This is the XRD pattern of the quantum dot photoresist film in Example 2;
[0046] Figure 9 This is the photoluminescence (PL) spectrum of the quantum dot photoresist film in Example 2;
[0047] Figure 10 This is a microscope image of the perovskite quantum dot photoresist pattern of Example 3;
[0048] Figure 11 This is the photoluminescence (PL) spectrum of the quantum dot color conversion film in Example 3;
[0049] Figure 12 This is the photoluminescence (PL) spectrum of the quantum dot color conversion film in Example 4;
[0050] Figure 13 This is a schematic diagram of the full-color display module in Example 5;
[0051] Figure 14 This is the photoluminescence (PL) spectrum of the full-color display module in Example 5. Detailed Implementation
[0052] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.
[0053] This invention provides a method for preparing perovskite quantum dot photoresist. Figure 1 A flowchart illustrating the preparation method of perovskite quantum dot photoresist in an embodiment of the present invention is shown, including the following steps:
[0054] S11. Preparation of CsPbBr3 perovskite quantum dot solution;
[0055] The concentration of the CsPbBr3 perovskite quantum dot solution is 100-150 mg / mL. If the concentration is too low, the quantum dot content in the final perovskite quantum dot photoresist will be too low, and the light conversion efficiency will not meet the requirements. If the concentration is too high, the CsPbBr3 perovskite quantum dot solution is prone to agglomeration and precipitation, and it will also lead to a higher viscosity of the final perovskite quantum dot photoresist.
[0056] Figure 2A flowchart illustrating the preparation method of CsPbBr3 perovskite quantum dot solution in an embodiment of the present invention is shown. The preparation of CsPbBr3 perovskite quantum dot solution includes:
[0057] S111, Preparation of cesium oleate precursor;
[0058] Cs₂CO₃, oleic acid, and octadecene are mixed and heated at 100–120 °C for 1–2 h to remove water and oxygen from the solution. The temperature is then increased to 150–180 °C to promote the reaction. The reaction continues until Cs₂CO₃ is completely dissolved to obtain the cesium oleate precursor. The ratio of oleic acid to Cs₂CO₃ is 1 mL: 0.08–0.15 g, and the ratio of oleic acid to octadecene is 1 mL: 6.66–15.00 mL.
[0059] Preferably, Cs2CO3, oleic acid, and octadecene are mixed and heated at 110°C for 1–2 hours. Choosing 110°C offers high cost-effectiveness and helps save energy while ensuring thorough dehydration and deoxygenation. The temperature is then raised to 160°C, and the Cs2CO3 is completely dissolved to obtain the cesium oleate precursor. Choosing 160°C not only allows for the complete and rapid dissolution of Cs2CO3 but also reduces solvent evaporation. The ratio of oleic acid to Cs2CO3 is 1 mL: 0.108 g, and the ratio of oleic acid to octadecene is 1 mL: 12.00 mL.
[0060] S112, Preparation of lead bromide precursor;
[0061] PbBr2 and octadecene were mixed and stirred at 100–120°C under vacuum for 1–2 hours to remove water from the solution, obtaining a first mixed solution. The ratio of octadecene to PbBr2 was 1 mL: 0.008–0.0125 g. Then, under nitrogen protection, oleic acid and oleylamine were injected into the first mixed solution to obtain the lead bromide precursor. The ratio of oleic acid, oleylamine, and octadecene was 1 mL: 1 mL: 8–10 mL.
[0062] Preferably, PbBr2 and octadecene are mixed and stirred at 120°C and under vacuum for 1 hour to obtain a first mixed solution, wherein the ratio of octadecene to PbBr2 is 1 mL: 0.0091 g; then, under nitrogen protection, oleic acid and oleylamine are injected into the first mixed solution to obtain the lead bromide precursor, wherein the ratio of oleic acid, oleylamine and octadecene is 1 mL: 1 mL: 10 mL.
[0063] S113. Prepare a crude CsPbBr3 solution;
[0064] The lead bromide precursor was heated to 140–190°C, and the cesium oleate precursor was rapidly injected into the heated lead bromide precursor. After reacting for 5–10 seconds, the mixture was immersed in a cold water bath to cool to room temperature, yielding a crude CsPbBr3 solution. The ratio of cesium oleate precursor to lead bromide precursor was 1 mL: 9.09–10.91 mL. CsPbBr3 crystals could be effectively produced under the conditions of 140–190°C. In addition, the reaction should be stopped by cooling in time, otherwise precipitation is likely to occur, resulting in the inability to disperse the CsPbBr3 crystals.
[0065] Preferably, the lead bromide precursor is heated to 180°C, and the cesium oleate precursor is rapidly injected into the heated lead bromide precursor. After reacting for 8 seconds, the mixture is immersed in a cold water bath to cool to room temperature to obtain a crude CsPbBr3 solution. The ratio of the cesium oleate precursor to the lead bromide precursor is 1 mL: 10.91 mL.
[0066] S114, purification;
[0067] Add 2-3 times the volume of ethyl acetate solution to the crude CsPbBr3 solution to remove excess oleic acid and oleylamine, facilitating the binding of perovskite quantum dots with photosensitizers during subsequent film formation photolithography. After mixing, centrifuge at 6000-10000 rpm for at least 15 min to obtain a first precipitate. Redisperse the first precipitate in toluene and add 2-3 times the volume of ethyl acetate solution, mix well, and centrifuge at 6000-10000 rpm for at least 15 min to obtain a second precipitate. Repeat the dispersion and precipitation of the second precipitate 2-6 times, and then disperse it again in toluene to obtain a CsPbBr3 perovskite quantum dot solution.
[0068] Preferably, three volumes of ethyl acetate solution are added to the crude CsPbBr3 solution, mixed, and centrifuged at 6000–10000 rpm for 15 min to obtain a first precipitate; the first precipitate is redispersed in toluene, and three volumes of ethyl acetate solution are added, mixed, and centrifuged at 6000–10000 rpm for 15 min to obtain a second precipitate; the second precipitate is repeatedly dispersed and precipitated four times, and then dispersed again in toluene to obtain a CsPbBr3 perovskite quantum dot solution.
[0069] S12. Prepare photosensitizer solution;
[0070] A photosensitizer solution is obtained by dissolving a photosensitizer in an organic solvent, wherein the ratio of the organic solvent to the photosensitizer is in the range of 1 mL: 30–50 mg.
[0071] The photosensitizer is one of 2,3,4,4'-tetrahydroxybenzophenone-1,2-naphthoquinone diazido-5-sulfonate, 6-diaza-5,6-dihydro-5-oxo-1-naphthalenesulfonate, 1,2-naphthoquinone-2-diazido-5-sulfonyl chloride, and 6-diaza-5,6-dihydro-5-oxo-1-naphthalenesulfonic acid. Sulfonic acid groups and sulfonyl groups can be adsorbed onto the surface of perovskite quantum dots; therefore, photosensitizers with sulfonic acid groups or sulfonyl groups can also be effectively adsorbed onto the surface. The surface of perovskite quantum dots; when these photosensitizers are irradiated with light of a specific wavelength, their ligands will cleave, leaving behind bound sulfonic acid groups (or sulfonyl groups) and active nitrogen free radicals at the other end. The active nitrogen free radicals can easily insert into the long alkyl chains of the natural ligands (such as oleylamine, oleic acid) through CH bonds to form covalent CN bonds; when these photochemical reactions occur between adjacent perovskite quantum dots, the perovskite quantum dots can easily crosslink to form an insoluble network structure, thereby achieving patterning.
[0072] Specifically, the organic solvent is one or a mixture of n-hexane, n-octane, chlorobenzene, and toluene.
[0073] Preferably, the photosensitizer is 2,3,4,4'-tetrahydroxybenzophenone 1,2-naphthoquinone diazido-5-sulfonate or 1,2-naphthoquinone-2-diazido-5-sulfonyl chloride, and the organic solvent is chlorobenzene.
[0074] S13, Preparation of perovskite quantum dot photoresist;
[0075] By volume, 10-20 parts of the photosensitizer solution, 1500-3000 parts of the CsPbBr3 perovskite quantum dot solution, 0.5-1 parts of oleic acid and 1-1.5 parts of oleylamine are added to a container and stirred for 20-40 hours under yellow light at 580-590 nm, nitrogen atmosphere and 10-20 °C to form perovskite quantum dot photoresist.
[0076] Adding oleic acid and oleylamine facilitates ligand exchange between CsPbBr3 perovskite quantum dots and the photosensitizer; the use of yellow light at 580–590 nm prevents photosensitizer degradation and avoids cross-linking of CsPbBr3 perovskite quantum dots; a nitrogen atmosphere prevents the oxidation of incompletely coordinated oleic acid and oleylamine; a temperature of 10–20 °C prevents the aggregation and precipitation of CsPbBr3 perovskite quantum dots; stirring for 20–40 h ensures thorough mixing of the photosensitizer, CsPbBr3 perovskite quantum dots, oleic acid, and oleylamine, resulting in a perovskite quantum dot photoresist with excellent photolithographic properties.
[0077] Preferably, by volume, 15 parts of the photosensitizer solution, 1500 parts of the CsPbBr3 perovskite quantum dot solution, 1 part of oleic acid and 1.5 parts of oleylamine are added to a container and stirred for 30 hours under 580-590 nm yellow light, nitrogen atmosphere and 10°C to form a perovskite quantum dot photoresist. The perovskite quantum dot photoresist prepared has good photolithographic patterning effect.
[0078] This invention also provides a perovskite quantum dot photoresist, which is prepared by the aforementioned method. The perovskite quantum dot photoresist is directly prepared by mixing a CsPbBr3 perovskite quantum dot solution, a photosensitizer solution, oleic acid, and oleylamine. When the film made from this perovskite quantum dot photoresist is exposed, the photosensitizer will cleave and covalently crosslink adjacent CsPbBr3 perovskite quantum dots with alkyl ligands on the surface of the CsPbBr3 perovskite quantum dots, thereby directly patterning the CsPbBr3 perovskite quantum dots. This eliminates the need to mix the CsPbBr3 perovskite quantum dots into the finished photoresist, effectively avoiding the fluorescence quenching problem caused by the finished photoresist and thus effectively improving the light conversion efficiency.
[0079] The exposed film has low polarity requirements for the developer and does not require the use of highly polar solvents for development. Low polar solvents can be used to develop the exposed film, which avoids the fluorescence quenching problem of perovskite quantum dots caused by highly polar solvents and is also beneficial to improving the light conversion efficiency.
[0080] This invention also provides a method for applying perovskite quantum dot photoresist, wherein the perovskite quantum dot photoresist prepared by the aforementioned method is applied to Micro LED full-color displays. Figure 3 A flowchart illustrating the application method of perovskite quantum dot photoresist in an embodiment of the present invention is shown. The application method includes the following steps:
[0081] S21, Spin coating;
[0082] The perovskite quantum dot photoresist is spin-coated onto a glass substrate or a Micro LED array wafer, and then heat-treated at 80–100°C for 2–4 minutes to obtain a first quantum dot photoresist film.
[0083] Specifically, in air, a glass substrate or Micro LED array wafer with the perovskite quantum dot photoresist spin-coated is placed on a heating stage for heat treatment, which is beneficial for the full evaporation of the solvent; preferably, the first quantum dot photoresist film is obtained by heat treatment at 90°C for 3 minutes to ensure that the solvent evaporates completely.
[0084] Furthermore, the spin coating speed of the perovskite quantum dot photoresist is in the range of 1000 to 3000 rpm, the spin coating acceleration range is in the range of 1000 to 2000 rpm / s, and the spin coating time is in the range of 45 to 55 s, which is beneficial for generating a uniform quantum dot photoresist film.
[0085] Preferably, the spin coating speed of the perovskite quantum dot photoresist is 1500 rpm, the spin coating acceleration of the perovskite quantum dot photoresist is 2000 rpm / s, and the spin coating time of the perovskite quantum dot photoresist is 50s. Matching the viscosity of the perovskite quantum dot photoresist, it can effectively and uniformly spin coat the perovskite quantum dot photoresist to form a quantum dot photoresist film with a thickness of about 1μm.
[0086] S22, Exposure;
[0087] Based on the photomask, the first quantum dot photoresist film is exposed to light at 300-430nm for 10-30s to obtain the exposed film.
[0088] The exposed area of the first quantum dot photoresist film undergoes photosensitive cross-linking. Light in the 300-430nm range passes through the photomask, and the area of the first quantum dot photoresist film irradiated by this wavelength of light undergoes a photochemical reaction. The photosensitizer is decomposed and covalently cross-links with the alkyl ligands on the surface of the CsPbBr3 perovskite quantum dots, thereby directly patterning the CsPbBr3 perovskite quantum dots.
[0089] The exposed film has low polarity requirements for the developer and does not require the use of highly polar solvents for development. Low polar solvents can be used for development, which avoids the fluorescence quenching problem of perovskite quantum dots caused by highly polar solvents and is also beneficial to improving the light conversion efficiency.
[0090] If the exposure time is less than 10 seconds, the lithographic pattern will not be well formed; if the exposure time is greater than 30 seconds, the edges of the lithographic pattern will be blurred.
[0091] Specifically, the power density of the light ranges from 20 to 30 mW / cm². 2 This ensures that the area of the first quantum dot photoresist film exposed to 300–430 nm light undergoes a full photochemical reaction.
[0092] Preferably, the first quantum dot photoresist film is exposed to 405nm light for 15s using a photomask to obtain an exposed film, wherein the power density of the light is in the range of 30mW / cm². 2 The photolithographic patterning effect is excellent.
[0093] S23, First baking;
[0094] The exposed film is baked at 50-80°C for 30-90 seconds to obtain a baked film;
[0095] This enhances the adhesion of the film and improves the pattern development effect; preferably, baking the exposed film on a hot stage at 70°C for 60 seconds to obtain a baked film can reduce the flow of the exposed film and effectively maintain the shape and structure of the exposed film.
[0096] S24. Prepare the developer;
[0097] The passivating ligand is dissolved in the developing solution to obtain the developing agent, and the ratio of developing solution to passivating ligand is in the range of 1 mL: 0.01–0.02 mg;
[0098] Specifically, the passivating ligand can be ammonium halide salts such as oleylamine iodide, oleylamine bromide, octylamine iodide, octylamine bromide, 2-phenylethylamine hydroiodate, 2-phenylethylamine hydrobromide, 3-fluorophenylethylamine iodide, and 3-fluorophenylethylamine bromide. Among them, ammonium iodide salts are mainly used to exchange ions with Br halogens in CsPbBr3 perovskite quantum dots to form red light quantum dots CsPbBrI2, realizing the red light emitting layer of the full-color display module. CsPbBr3 perovskite quantum dots are themselves green light quantum dots, and the role of ammonium bromide salts is to supplement Br halogens and passivate CsPbBr3 perovskite quantum dots, which can effectively improve the luminescence effect of CsPbBr3 perovskite quantum dots.
[0099] Furthermore, the developing solution is one or more of hexane, n-octane, toluene, chlorobenzene, ethyl acetate, and methyl acetate, which has low polarity. This avoids the fluorescence quenching problem of perovskite quantum dots caused by excessively high solvent polarity and is also beneficial to improving light conversion efficiency. Preferably, the developing solution is composed of methyl acetate and toluene, with a volume ratio of methyl acetate to toluene of 1:50, resulting in good developing effect and clean development.
[0100] Adding ammonium halide salts to the developer can not only effectively reduce surface defects of perovskite quantum dot materials and improve their luminescence brightness, but also enable the exchange of anions in perovskite quantum dots, thereby achieving spectral modulation. This eliminates the need to mix quantum dots of different colors with different photoresists for photolithography, thus reducing the complexity and cost of the process.
[0101] S25, Development;
[0102] The baked film is immersed in the developer and developed for 10-30 seconds to obtain a developed film.
[0103] The developer dissolves the areas of the baked film that have not undergone photocrosslinking, leaving behind the photocrosslinked film pattern, thus achieving film patterning. If the development time is less than 10 seconds, the development is incomplete and the uncrosslinked film cannot be completely dissolved; if the development time is greater than 30 seconds, the development is over-developed, which can easily lead to poor pattern edges. Preferably, immersing the baked film in the developer for 25 seconds yields a developed film with excellent patterning effect.
[0104] S26, Second baking;
[0105] The developing film is baked at 50-80°C for 30-90 seconds to obtain the first quantum dot color conversion film;
[0106] Specifically, the developing film is placed on a hot plate at 50-80°C and baked for 30-90 seconds to obtain a first quantum dot color conversion film, which is used to dry the developing solution remaining on the developing film; preferably, the temperature is 80°C and the baking time is 60 seconds to ensure that there is no developing solution residue.
[0107] S27, Deposited passivation layer;
[0108] A first passivation layer is deposited on the first quantum dot color conversion film;
[0109] The first passivation layer can prevent the quantum dots in the first quantum dot color conversion film from coming into contact with the outside air, thus avoiding the quantum dots in the first quantum dot color conversion film from being induced to quench.
[0110] Specifically, the thickness of the first passivation layer ranges from 5 to 20 nm. If the thickness is less than 5 nm, the first passivation layer cannot completely cover the first quantum dot color conversion film; if the thickness is greater than 20 nm, the cost is increased. The material of the first passivation layer is SiO2 or SiN. x h-BN, AlO x One of them; preferably, the thickness of the first passivation layer is 10 nm, and the material of the first passivation layer is SiO2.
[0111] Furthermore, an atomic deposition (ALD) method is used to deposit a first passivation layer on the first quantum dot color conversion film.
[0112] S28. Prepare the second quantum dot color conversion film;
[0113] The perovskite quantum dot photoresist is spin-coated onto the first passivation layer and heat-treated at 80-100°C for 2-4 minutes to obtain a second quantum dot photoresist film; then, the operations from S22 to S26 are repeated to form a second quantum dot color conversion film, and a second passivation layer is deposited on the second quantum dot color conversion film.
[0114] The thickness of the second passivation layer ranges from 5 to 20 nm, and the material of the second passivation layer is SiO2 or SiN. x h-BN, AlO x In one of the methods, the function of the second passivation layer is similar to that of the first passivation layer, which will not be elaborated here; preferably, the thickness of the second passivation layer is 10 nm, and the material of the second passivation layer is SiO2.
[0115] Specifically, when preparing the first quantum dot color conversion film, if the passivating ligand is one of oleylamine iodide, octylamine iodide, 2-phenylethylamine hydroiodate, or 3-fluorophenylethylamine iodide, then the first quantum dot color conversion film is a red light emitting layer; preferably, the passivating ligand is oleylamine iodide. When preparing the second quantum dot color conversion film, if the passivating ligand is one of oleylamine bromide, octylamine bromide, 2-phenylethylamine hydrobromide, or 3-fluorophenylethylamine bromide, then the second quantum dot color conversion film is a green light emitting layer; preferably, the passivating ligand is oleylamine bromide.
[0116] Alternatively, when preparing the first quantum dot color conversion film, if the passivating ligand is one of oleylamine bromide, octylamine bromide, 2-phenylethylamine hydrobromide, or 3-fluorophenylethylamine bromide, then the first quantum dot color conversion film is a green light emitting layer; preferably, the passivating ligand is oleylamine bromide. When preparing the second quantum dot color conversion film, if the passivating ligand is one of oleylamine iodide, octylamine iodide, 2-phenylethylamine hydroiodide, or 3-fluorophenylethylamine iodide, then the second quantum dot color conversion film is a red light emitting layer; preferably, the passivating ligand is oleylamine iodide.
[0117] The first quantum dot color conversion film and the second quantum dot color conversion film are formed by photolithography based on different photomasks, and the light emitted by the two is different; thus, the first quantum dot color conversion film and the second quantum dot color conversion film form a perovskite quantum dot color conversion array, and the perovskite quantum dot color conversion array is combined with blue Micro LED or ultraviolet Micro LED to form a full-color display module.
[0118] In this invention, a perovskite quantum dot photoresist is directly prepared by mixing a CsPbBr3 perovskite quantum dot solution, a photosensitizer solution, oleic acid, and oleylamine. During exposure, the photosensitizer in the quantum dot photoresist film breaks down and covalently crosslinks adjacent CsPbBr3 perovskite quantum dots with alkyl ligands on the surface of the CsPbBr3 perovskite quantum dots, thereby directly patterning the CsPbBr3 perovskite quantum dots. This eliminates the need to mix the CsPbBr3 perovskite quantum dots into the finished photoresist, effectively avoiding the fluorescence quenching problem caused by the finished photoresist and thus significantly improving the light conversion efficiency.
[0119] Subsequently, the polarity requirement of the developer for the exposed film is lower. It is not necessary to use high-polarity solvents for development. Low-polarity solvents can be used for development. This avoids the fluorescence quenching problem of perovskite quantum dots caused by high-polarity solvents and is also beneficial to improving the light conversion efficiency.
[0120] Moreover, the developer used for developing contains ammonium halide salts, which can not only effectively reduce defects on the surface of perovskite quantum dot materials and improve their luminescence brightness, but also realize the exchange of perovskite quantum dot anions, thereby achieving spectral modulation.
[0121] This invention can significantly improve the photolithographic precision of perovskite quantum dots, realize the micron-level patterned manufacturing of quantum dots, and can be applied to wide color gamut and high color accuracy Micro LED full-color displays.
[0122] Example 1
[0123] This embodiment provides a method for preparing perovskite quantum dot photoresist, including the following steps:
[0124] (1) Add 0.27g Cs2CO3 and 2.5mL oleic acid to 30mL octadecene and heat continuously at 110℃ for 1-2h. Then raise the temperature to 160℃ and react until Cs2CO3 is completely dissolved to obtain cesium oleate precursor.
[0125] (2) Mix 0.0453 g PbBr2 and 5 mL octadecene, and stir at 120 °C and vacuum for 1 h to obtain a first mixed solution; then, inject 0.5 mL oleic acid and 0.5 mL oleylamine into the first mixed solution under nitrogen protection to obtain the lead bromide precursor;
[0126] (3) Heat the lead bromide precursor to 180℃ and quickly inject 0.55 mL of cesium oleate precursor into the heated lead bromide precursor. After reacting for 8 seconds, immerse it in a cold water bath to cool to room temperature to obtain a crude CsPbBr3 solution.
[0127] (4) Add 3 times the volume of ethyl acetate solution to the crude CsPbBr3 solution, mix well, and centrifuge at 6000-10000 rpm for 15 min to obtain the first precipitate; then, redisperse the first precipitate in 1.5 mL of toluene, add 3 times the volume of ethyl acetate solution, mix well, and centrifuge at 6000-10000 rpm for 15 min to obtain the second precipitate; repeat the dispersion and precipitation of the second precipitate 4 times, and then disperse it again in toluene to obtain the CsPbBr3 perovskite quantum dot solution, and adjust the concentration of the CsPbBr3 perovskite quantum dot solution to 140 mg / mL;
[0128] (5) Dissolve 30 mg of 2,3,4,4'-tetrahydroxybenzophenone-1,2-naphthoquinone diazido-5-sulfonate in 1 mL of chlorobenzene to obtain a photosensitizer solution;
[0129] (6) Take 15 μL of photosensitizer solution and add 1.5 mL of CsPbBr3 perovskite quantum dot solution, then add 1 μL of oleic acid and 1.5 μL of oleylamine. Stir for 30 h under 580-590 nm yellow light, nitrogen atmosphere and 10 °C to form perovskite quantum dot photoresist.
[0130] The perovskite quantum dot photoresist of this embodiment was spin-coated onto a glass substrate to form a quantum dot photoresist film. The film was then irradiated with 405nm light through a mask, and analyzed by SEM, XRD, and fluorescence spectroscopy. The results are as follows: Figure 4 , Figure 5 and Figure 6 As shown.
[0131] Figure 4 The image shows a scanning electron microscope image of the quantum dot photoresist film after exposure in Example 1. It shows a relatively uniform film with sufficient cross-linking between quantum dots, but some individual pores are present. Figure 5 The XRD pattern of the quantum dot photoresist film of Example 1 is shown. The diffraction peaks all show the (100), (110) and (200) crystal planes of the cubic CsPbBr3, indicating that the CsPbBr3 perovskite quantum dots are cubic phase and the crystal planes are randomly oriented. Figure 6 The photoluminescence (PL) spectrum of the quantum dot photoresist film of Example 1 is shown, and it can be seen that the absorption peak is located at 525 nm.
[0132] Example 2
[0133] This embodiment provides a method for preparing perovskite quantum dot photoresist, which differs from Example 1 in that the photosensitizer used in this embodiment is 1,2-naphthoquinone-2-azido-5-sulfonyl chloride.
[0134] The perovskite quantum dot photoresist of this embodiment was spin-coated onto a glass substrate to form a quantum dot photoresist film. The film was then irradiated with 405nm light through a mask, and analyzed by SEM, XRD, and fluorescence spectroscopy. The results are as follows: Figure 7 , Figure 8 and Figure 9 As shown.
[0135] Figure 7 The image shows a scanning electron microscope image of the quantum dot photoresist film after exposure in Example 2. It shows a relatively uniform film with sufficient cross-linking between quantum dots and no pores. Figure 8The XRD pattern of the quantum dot photoresist film of Example 2 is shown. The diffraction peaks all show the (100), (110) and (200) crystal planes of the CsPbBr3 cubic crystal, indicating that the CsPbBr3 perovskite quantum dots are cubic phase and the crystal planes are randomly oriented. Figure 9 The photoluminescence (PL) spectrum of the quantum dot photoresist film of Example 2 is shown. It can be seen that the absorption peak is located at 520 nm, which shows a slight blue shift compared to Example 1. This is mainly due to the exchange of Cl halogen and Br halogen.
[0136] Example 3
[0137] This embodiment provides a method for applying perovskite quantum dot photoresist, including the following steps:
[0138] (1) Spin-coat the perovskite quantum dot photoresist of Example 1 onto a glass substrate or a Micro LED array wafer; specifically, the spin-coating speed of the perovskite quantum dot photoresist is 1500 rpm, the spin-coating acceleration is 2000 rpm / s, and the spin-coating time is 50 s; then, in air, place the glass substrate or Micro LED array wafer with the perovskite quantum dot photoresist spin-coated on a heating stage at 90°C for 3 min to heat-treat and obtain a quantum dot photoresist film.
[0139] (2) Placing the quantum dot photoresist film under 405nm light (power density of 30mW / cm²) based on a photomask. 2 Exposure for 15 seconds under the specified conditions to obtain the exposed film;
[0140] (3) Place the exposed film on a hot plate at 70°C and bake for 60 seconds to obtain a baked film.
[0141] (4) Dissolve 10 mg of oleamide bromide in 500 mL of developing solution to obtain developing agent; wherein, the developing solution is composed of methyl acetate and toluene, and the volume ratio of methyl acetate to toluene is 1:50;
[0142] (5) Immerse the baked film in the developer for 25 seconds to obtain the developed film;
[0143] (6) The developing film was baked on a hot plate at 80°C for 60 seconds to obtain a quantum dot color conversion film;
[0144] (7) A 10 nm thick passivation layer was deposited on the quantum dot color conversion film by atomic deposition (ALD), and the material of the passivation layer was SiO2.
[0145] The perovskite quantum dot photoresist lithography pattern of this embodiment was observed under a microscope and analyzed by fluorescence spectroscopy. The results are as follows: Figure 10 and Figure 11 As shown.
[0146] Figure 10 A microscope image of the perovskite quantum dot photoresist lithography pattern of Example 3 is shown. The size of the lithography pattern is 4 μm, which can achieve micron-level lithography. Figure 11 The photoluminescence (PL) spectrum of the quantum dot color conversion film of Example 3 is shown. It can be seen that the absorption peak is located at 525 nm, realizing green light emission.
[0147] Example 4
[0148] This embodiment provides a method for applying perovskite quantum dot photoresist, which differs from Embodiment 3 in that the passivation ligand used in this embodiment is oleylamine iodine.
[0149] Fluorescence spectroscopy analysis was performed on the perovskite quantum dot photoresist pattern of this embodiment, and the results are as follows: Figure 12 As shown.
[0150] Figure 12 The photoluminescence (PL) spectrum of the quantum dot color conversion film of Example 4 is shown. It can be seen that the absorption peak is located at 625 nm, realizing red light emission.
[0151] Example 5
[0152] This invention also provides a method for applying perovskite quantum dot photoresist, which applies the prepared perovskite quantum dot photoresist to Micro LED full-color displays, including the following steps:
[0153] (1) Spin-coat the perovskite quantum dot photoresist of Example 2 onto a glass substrate or a Micro LED array wafer; specifically, the spin-coating speed of the perovskite quantum dot photoresist is 1500 rpm, the spin-coating acceleration is 2000 rpm / s, and the spin-coating time is 50 s; then, in air, place the glass substrate or Micro LED array wafer with the perovskite quantum dot photoresist spin-coated on a heating stage at 90°C for 3 min to heat-treat and obtain the first quantum dot photoresist film;
[0154] (2) The first quantum dot photoresist film is placed under 405nm light (power density of 30mW / cm²) based on the first mask. 2 The first exposure film is obtained by exposing the substrate for 15 seconds; the first mask is used to expose a single pixel on the glass substrate or Micro LED array wafer.
[0155] (3) The first exposed film is placed on a hot plate at 70°C and baked for 60 seconds to obtain the first baked film;
[0156] (4) Dissolve 10 mg of oleamide bromide in 500 mL of developer to obtain the first developer; wherein the developer is composed of methyl acetate and toluene, and the volume ratio of methyl acetate to toluene is 1:50;
[0157] (5) Immerse the first baked film in the first developer for 25 seconds to obtain the first developed film;
[0158] (6) The first developing film is baked on a hot table at 80°C for 60s to obtain the first quantum dot color conversion film, which is a green light emitting layer.
[0159] (7) A 10 nm thick first passivation layer is deposited on the first quantum dot color conversion film by atomic deposition (ALD), and the material of the first passivation layer is SiO2;
[0160] (8) Spin-coat the perovskite quantum dot photoresist of Example 2 onto the first passivation layer; specifically, the spin-coating speed of the perovskite quantum dot photoresist is 1500 rpm, the spin-coating acceleration is 2000 rpm / s, and the spin-coating time is 50s; then heat-treat it in air on a heating stage at 90°C for 3 minutes to obtain the second quantum dot photoresist film.
[0161] (9) Place the second quantum dot photoresist film under 405nm light (power density of 30mW / cm²) based on the second mask. 2 The second exposure film is obtained by exposing for 15 seconds.
[0162] (10) Place the second exposed film on a hot plate at 70°C and bake for 60 seconds to obtain the second baked film.
[0163] (11) Dissolve 10 mg of oleamide iodine in 500 mL of developing solution to obtain a second developing agent; wherein the developing solution is composed of methyl acetate and toluene, and the volume ratio of methyl acetate to toluene is 1:50;
[0164] (12) Immerse the second baked film in the second developer for 25 seconds to obtain the second developed film;
[0165] (13) The second developing film is baked on a hot table at 80°C for 60s to obtain the second quantum dot color conversion film, which is a red light emitting layer.
[0166] (14) A 10 nm thick second passivation layer is deposited on the second quantum dot color conversion film by atomic deposition (ALD), and the material of the second passivation layer is SiO2.
[0167] The first and second quantum dot color conversion films are formed by photolithography using different photomasks, and they emit different colors. Ultimately, the first and second quantum dot color conversion films form a perovskite quantum dot color conversion array, which, combined with a blue Micro LED, forms a red-green-blue (RGB) array—a full-color display module. Figure 13 A schematic diagram of the full-color display module of Embodiment 5 is shown.
[0168] Fluorescence spectroscopy analysis was performed on the full-color display module of this embodiment, and the results are as follows: Figure 14 As shown.
[0169] Figure 14 The photoluminescence (PL) spectrum of the full-color display module of Example 5 is shown, which realizes red, green and blue (RGB) emission.
[0170] The above provides a detailed description of a perovskite quantum dot photoresist and its preparation and application methods provided by embodiments of the present invention. Specific examples have been used to illustrate the principles and implementation methods of the present invention. The descriptions of the above embodiments are only for the purpose of helping to understand the methods and core ideas of the present invention. At the same time, for those skilled in the art, there will be changes in the specific implementation methods and application scope based on the ideas of the present invention. Therefore, the content of this specification should not be construed as a limitation of the present invention.
Claims
1. A method for preparing a perovskite quantum dot photoresist, characterized in that, Includes the following steps: S11. Prepare a CsPbBr3 perovskite quantum dot solution, wherein the concentration of the CsPbBr3 perovskite quantum dot solution is 100-150 mg / mL; S12. Prepare a photosensitizer solution by dissolving the photosensitizer in an organic solvent to obtain a photosensitizer solution, wherein the ratio of the organic solvent to the photosensitizer is in the range of 1 mL: 30–50 mg; The photosensitizer is one of 2,3,4,4'-tetrahydroxybenzophenone 1,2-naphthoquinone diazido-5-sulfonate, 6-diaza-5,6-dihydro-5-oxo-1-naphthalenesulfonate, 1,2-naphthoquinone-2-diazido-5-sulfonyl chloride, and 6-diaza-5,6-dihydro-5-oxo-1-naphthalenesulfonic acid; S13. Prepare perovskite quantum dot photoresist: By volume, take 10-20 parts of the photosensitizer solution, 1500-3000 parts of the CsPbBr3 perovskite quantum dot solution, 0.5-1 parts of oleic acid and 1-1.5 parts of oleylamine and put them into a container. Stir for 20-40 hours under 580-590nm yellow light, nitrogen atmosphere and 10-20℃ to form perovskite quantum dot photoresist.
2. The preparation method according to claim 1, characterized in that, The preparation of the CsPbBr3 perovskite quantum dot solution includes: S111. Preparation of cesium oleate precursor: Cs2CO3, oleic acid and octadecene are mixed and heated at 100-120℃ for 1-2 hours, then heated to 150-180℃ until Cs2CO3 is completely dissolved to obtain cesium oleate precursor; the ratio of oleic acid to Cs2CO3 is 1mL:0.08-0.15g, and the ratio of oleic acid to octadecene is 1mL:6.66-15.00mL; S112. To prepare the lead bromide precursor, PbBr2 and octadecene are mixed and stirred at 100-120°C under vacuum for 1-2 hours to obtain a first mixed solution. The ratio of octadecene to PbBr2 is 1 mL: 0.008-0.0125 g. Under nitrogen protection, oleic acid and oleylamine are injected into the first mixed solution to obtain the lead bromide precursor. The ratio of oleic acid, oleylamine and octadecene is 1 mL: 1 mL: 8-10 mL. S113. To prepare a crude CsPbBr3 solution, the lead bromide precursor is heated to 140–190°C, and the cesium oleate precursor is rapidly injected into the heated lead bromide precursor. After reacting for 5–10 seconds, the solution is immersed in a cold water bath to cool to room temperature to obtain a crude CsPbBr3 solution. The ratio of cesium oleate precursor to lead bromide precursor is 1 mL: 9.09–10.91 mL. S114. Purification: Add 2-3 times the volume of ethyl acetate solution to the crude CsPbBr3 solution, mix well, and centrifuge at 6000-10000 rpm for at least 15 min to obtain a first precipitate; redisperse the first precipitate in toluene, add 2-3 times the volume of ethyl acetate solution, mix well, and centrifuge at 6000-10000 rpm for at least 15 min to obtain a second precipitate; repeat the dispersion and precipitation of the second precipitate 2-6 times, and then disperse it again in toluene to obtain a CsPbBr3 perovskite quantum dot solution.
3. The preparation method according to claim 1, characterized in that, In the preparation of the photosensitizer solution, the organic solvent is one or a mixture of n-hexane, n-octane, chlorobenzene, and toluene.
4. A perovskite quantum dot photoresist, characterized in that, The perovskite quantum dot photoresist is prepared by the preparation method according to any one of claims 1 to 3.
5. A method for applying perovskite quantum dot photoresist, characterized in that, The perovskite quantum dot photoresist prepared by the preparation method according to any one of claims 1 to 3 is applied to a Micro LED full-color display, the application method comprising the following steps: S21. Spin coating: Spin coat the perovskite quantum dot photoresist onto a glass substrate or Micro LED array wafer, and heat treat it at 80-100°C for 2-4 minutes to obtain a first quantum dot photoresist film. S22, Exposure: Based on the photomask, expose the first quantum dot photoresist film under light of 300-430nm for 10-30s to obtain the exposed film; S23. First baking: The exposed film is baked at 50-80°C for 30-90 seconds to obtain a baked film. S24. Prepare the developer by dissolving the passivating ligand in the developer solution to obtain the developer. The ratio of developer solution to passivating ligand is in the range of 1 mL: 0.01–0.02 mg. S25. Development: Immerse the baked film in the developer for 10-30 seconds to obtain a developed film. S26. Second baking: The developing film is baked at 50-80°C for 30-90 seconds to obtain the first quantum dot color conversion film. S27. Deposit a passivation layer, depositing a first passivation layer on the first quantum dot color conversion film; S28. Prepare a second quantum dot color conversion film by spin-coating the perovskite quantum dot photoresist onto the first passivation layer and heat-treating it at 80-100°C for 2-4 minutes to obtain a second quantum dot photoresist film; then repeat the operations from S22 to S26 to form a second quantum dot color conversion film, and deposit a second passivation layer on the second quantum dot color conversion film. The first quantum dot color conversion film and the second quantum dot color conversion film form a perovskite quantum dot color conversion array, and the perovskite quantum dot color conversion array is combined with blue Micro LED or ultraviolet Micro LED to form a full-color display module.
6. The application method as described in claim 5, characterized in that, The spin coating speed range of the perovskite quantum dot photoresist is 1000-3000 rpm, the spin coating acceleration range of the perovskite quantum dot photoresist is 1000-2000 rpm / s, and the spin coating time of the perovskite quantum dot photoresist is 45-55s.
7. The application method as described in claim 5, characterized in that, In step S22, the power density of the light is in the range of 20–30 mW / cm². 2 .
8. The application method as described in claim 5, characterized in that, When preparing the first quantum dot color conversion film, the passivation ligand is one of oleylamine iodine, octylamine iodine, 2-phenylethylamine hydroiodate, and 3-fluorophenylethylamine iodide; when preparing the second quantum dot color conversion film, the passivation ligand is one of oleylamine bromide, octylamine bromide, 2-phenylethylamine hydrobromide, and 3-fluorophenylethylamine bromide.
9. The application method as described in claim 5, characterized in that, When preparing the first quantum dot color conversion film, the passivating ligand is one of oleylamine bromide, octylamine bromide, 2-phenylethylamine hydrobromide, and 3-fluorophenylethylamine bromide; when preparing the second quantum dot color conversion film, the passivating ligand is one of oleylamine iodide, octylamine iodide, 2-phenylethylamine hydroiodide, and 3-fluorophenylethylamine iodide.
10. The application method as described in claim 5, characterized in that, The developing solution is one or a mixture of n-hexane, n-octane, toluene, chlorobenzene, ethyl acetate, and methyl acetate; The thickness of the first passivation layer ranges from 5 to 20 nm, and the material of the first passivation layer is SiO2 or SiN. x h-BN, AlO x One of them; The thickness of the second passivation layer ranges from 5 to 20 nm, and the material of the second passivation layer is SiO2 or SiN. x h-BN, AlO x One of them.
Citation Information
Patent Citations
Quantum dot light-emitting structure and photoinduced patterning method and application thereof
CN116096197A
Synthesis method of quantum dot photoresist and application of quantum dot photoresist in Mini LED / Micro LED
CN116400563A