A method for preparing an ablation-resistant resin-based composite material
By combining modified phenolic resin and quartz fiber with a low-pressure, long-term heat-insulating molding process, the micro-crack and porosity problems of phenolic resin-based composite materials under high-temperature environments have been solved, improving product appearance and yield.
Patent Information
- Application Number
- CN202311683668.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-10
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2043-12-10
AI Technical Summary
Existing phenolic resin-based composite materials are prone to microcracks and crack propagation under high-temperature environments, and solvents and low-molecular-weight substances form pores and weak cross-linking defects, affecting the product's appearance quality and pass rate.
Using modified phenolic resin as the matrix and quartz fiber as the reinforcement, a molding and curing process with low pressure and long-term heat preservation parameters is adopted. This process combines physical and chemical methods to reduce the volatilization of solvents and small molecule products, increase the internal bonding force of the material, prevent crack propagation, and improve the curing process.
It improves the appearance quality and pass rate of materials, reduces microcracks and porosity defects, and enhances the overall strength and uniformity of materials.
Smart Images

Figure CN117656528B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of composite material preparation technology, and in particular to a method for preparing an ablation-resistant resin-based composite material. Background Technology
[0002] Aviation materials are a general term for all kinds of materials used in the manufacture of aircraft, aero-engines, and airborne equipment. Aviation materials are the material guarantee for the research and production of aviation products, and also the technical foundation for enabling aviation products to achieve the expected performance, service life, and reliability.
[0003] Based on their composition and structural characteristics, aerospace materials are categorized into four main types: metallic materials, organic polymer materials, inorganic non-metallic materials, and composite materials. Composite materials are multiphase materials composed of two or more materials. They generally refer to structural materials with high strength, made by combining one or more reinforcing materials (reinforcing bodies) with a binding material (matrix). The reinforcing body is the component in a composite material that, through bonding with the matrix, has a strength and modulus far exceeding that of the matrix. Reinforcing bodies are classified into four types according to their morphology: granular, fibrous, sheet-like, and three-dimensional. Continuous fiber reinforcements used in industry, such as glass fiber, carbon fiber, graphite fiber, silicon carbide fiber, boron fiber, and high-modulus organic fibers, are primarily used as reinforcing materials in composite materials.
[0004] The matrix refers to the component that binds and reinforces in a composite material. It is generally classified into three main categories: metallic matrices, polymer matrices, and inorganic non-metallic matrices. Polymer matrices include resins and rubbers. The matrix should exhibit good adhesion and compatibility with the reinforcement. The contact surface between the matrix and the reinforcement is called the "interface." Due to the adhesive effect of the matrix on the reinforcement, the interface exhibits effects such as force propagation, crack blocking, energy absorption, and scattering, thus enabling the composite material to possess certain superior properties not found in single materials.
[0005] As the flight speeds of various aircraft continue to increase, the thermal environments they operate in are becoming increasingly harsh, leading to higher requirements for heat-resistant products. Heat-resistant materials have primarily evolved through four main types: heat sink, evaporative, radiation-based, and ablation-based. Currently, ablation-based heat-resistant materials are the most mature and widely used. Phenolic resin-based composites have become the mainstream heat-resistant material due to their excellent ablation resistance. The heat-resistant performance of phenolic resin-based composites can be further improved through high-temperature fiber reinforcement and inorganic particle modification. However, the addition of inorganic particles weakens the strength of the resin matrix, making the product more prone to defects such as microcracks. Summary of the Invention
[0006] The purpose of this invention is to provide a method for preparing ablation-resistant resin-based composite materials. This method uses physical means to increase the internal bonding force of the material matrix, making it less prone to microcracks and preventing crack propagation. At the same time, it uses chemical methods to improve the curing process, reducing defects such as pores and weak cross-linking formed by solvents and low-molecular-weight substances inside the material, effectively improving the appearance quality of the product and increasing the product qualification rate.
[0007] To solve the above-mentioned technical problems, the technical solution adopted by the present invention is as follows:
[0008] A method for preparing an ablation-resistant resin-based composite material, using modified phenolic resin as the matrix and quartz fiber as the reinforcement, includes the following:
[0009] (1) Fill the short fiber prepreg into the cavity of the pre-compression mold and pre-compact the short fiber prepreg with a mold temperature of 38-42℃;
[0010] (2) Use a cutting machine to cut the mesh prepreg into the specified size and shape;
[0011] (3) Set a release cloth in the molding mold, lay a layer of mesh prepreg flat on the release cloth, put in the short fiber prepreg blank pre-compacted in step (1), lay a layer of mesh prepreg flat on the upper surface of the blank, and close the mold.
[0012] (4) The press is subjected to low pressure and long-term heat preservation parameters at a specific temperature point for molding and curing, and then demolded to obtain the product;
[0013] The long-term heat preservation parameters include: 10-70 min, 60-60℃; 80-220 min, 100-100℃.
[0014] This invention uses modified phenolic resin as the matrix and quartz fiber as the reinforcement. First, short-fiber prepreg and mesh prepreg are prepared, and then an ablation-resistant resin-based composite material is prepared using these materials. During molding, a layer of mesh prepreg is laid on the outermost surface of the product. This mesh prepreg can embed itself into the short-fiber prepreg matrix during molding and curing, forming a continuous fiber layer on the product surface. This results in a more uniform material composition and reduces the likelihood of internal stress. By using physical means to increase the internal bonding force of the material, it effectively prevents crack propagation when cracks occur in the resin matrix.
[0015] Meanwhile, during the molding process, this invention employs low pressure and long-term heat preservation parameters at the solvent evaporation temperature points of the resin system to ensure complete solvent evaporation; and at the evaporation temperature points of the small molecule products from the phenolic polycondensation reaction, low pressure and long-term heat preservation parameters are used: 10-70 min, 60-60℃, 80-220 min, 100-100℃, to ensure the complete evaporation of small molecules generated during the reaction. Through these process optimization measures, the curing process is improved, reducing defects such as pores and weak cross-linking formed by solvents and low-molecular-weight substances within the material, lowering internal stress, and further increasing the material's overall strength.
[0016] The appearance quality of the products made by this invention is greatly improved, and the pass rate is doubled.
[0017] Furthermore, the low pressure in step (4) is: 0-260 min, 0.5 MPa; 260-400 min, 0.5-5 MPa; 400-760 min, 5 MPa.
[0018] This invention employs a pressure of 0.5 MPa for 0-300 minutes, combined with long-term heat preservation at 60-60℃ for 10-70 minutes, 80-220 minutes, and 100-100℃, to allow the solvent and small molecule products in the phenolic polycondensation reaction within the resin system to fully volatilize, thereby reducing defects such as pores and weak crosslinking formed by solvents and low-molecular-weight substances inside the material.
[0019] Further, the low pressure in step (4) is: 260-280 min, 0.5 MPa; 280-300 min, 0.5-5 MPa; 300-400 min, 5 MPa.
[0020] Furthermore, the long-term heat preservation parameters also include 0-10 min, 40-60℃; 70-80 min, 60-100℃; 220-260 min, 100-125℃; 260-400 min, 125-125℃; 400-440 min, 125-160℃; 440-580 min, 160-160℃; 580-600 min, 160-180℃; 600-760 min, 180-180℃.
[0021] Furthermore, the modified phenolic resin is an inorganic particulate modified phenolic resin.
[0022] Furthermore, the inorganic particles are ceramic powder.
[0023] Furthermore, the short fiber prepreg reinforcement can also be glass fiber or high silica glass fiber.
[0024] Furthermore, the reinforcement of the short fiber prepreg is chopped quartz fiber.
[0025] In this invention, the reinforcement of the short fiber prepreg can be selected from chopped quartz fiber, ordinary glass fiber or high silica glass fiber. In the embodiments and comparative examples of this invention, chopped quartz fiber is selected.
[0026] Furthermore, the reinforcement of the mesh prepreg is a continuous mesh fabric made of quartz fiber.
[0027] The short fiber prepreg of the present invention uses Istar-H3001, and the mesh prepreg uses Istar-H3001-1. Both use magnetic powder modified phenolic resin as the base material. The reinforcement of the short fiber prepreg is chopped quartz fiber, and the reinforcement of the mesh prepreg is a continuous mesh made of quartz fiber. Both are purchased from the market.
[0028] Furthermore, in step (1), the packing can be pre-compressed multiple times in stages.
[0029] Repeated pre-compression of filler material, with small amounts of pre-compression applied multiple times, can enhance the compaction effect of short fiber prepreg.
[0030] Prepreg is a composition of resin matrix and reinforcement, prepared by impregnating continuous fibers or fiber fabrics under strictly controlled conditions. It is an intermediate material in the manufacture of composite materials. Prepregs can be classified in many ways according to their physical state and chemical properties: By physical state, prepregs are divided into unidirectional prepregs, unidirectional fabric prepregs, and fabric prepregs; by resin matrix, prepregs are divided into thermosetting resin prepregs and thermoplastic resin prepregs; by reinforcement material, they are divided into carbon fiber (fabric) prepregs, glass fiber (fabric) prepregs, and aramid (fabric) prepregs; by fiber length, they are divided into short fiber prepregs, prepregs, and continuous fiber prepregs; and by curing temperature, they are divided into medium-temperature curing (120°C) prepregs, high-temperature curing (180°C) prepregs, and prepregs with curing temperatures exceeding 200°C, etc. Our business unit also has a wide range of applications in prepregs. Different types of materials are used depending on the product and performance. Commonly used prepregs include unidirectional carbon fiber prepregs, glass fiber fabric prepregs, carbon fiber fabric prepregs, phenolic glass fiber fabric prepregs, etc.
[0031] There are two methods for preparing prepregs: dry and wet. Dry methods include powder methods and hot-melt methods. Powder prepregs refer to composites in which resin powder adheres to fibers, partially melts, forming a discontinuous resin layer where the fibers are not fully impregnated. Hot-melt prepregs are prepared by heating and melting the resin system into a fluid state, then impregnating fibers or fabrics with it. Wet prepregs are prepared by impregnating fiber bundles or fabrics with a resin solution; the prepreg of this invention belongs to the wet-process prepreg category.
[0032] The beneficial effects of this invention are:
[0033] This invention involves molding and curing short-fiber prepregs and mesh prepregs using inorganic particle-modified phenolic resin as the matrix and chopped quartz fibers as reinforcement. This process embeds the mesh prepreg into the short-fiber prepreg blank, forming a continuous fiber layer on the product surface. This results in a more uniform material composition, reduces internal stress, minimizes microcracks, and prevents crack propagation. Simultaneously, the molding process employs low pressure and long-term heat preservation parameters to fully evaporate the solvent and small molecule products generated during the phenolic polymerization reaction. This combined physical and chemical approach effectively improves the product's appearance quality and increases the product qualification rate. Attached Figure Description
[0034] Figure 1 Example 1: Actual product appearance image;
[0035] Figure 2 Comparative Example 1: Product appearance drawing. Detailed Implementation
[0036] The technical solution of the present invention is described clearly and completely below. Obviously, the embodiments described herein are only a part of the present invention, and not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the protection scope of the present invention.
[0037] Example 1
[0038] A method for preparing an ablation-resistant resin-based composite material, wherein the matrix of the composite material is ceramic powder modified phenolic resin, the reinforcement of the short fiber prepreg is chopped quartz fiber, and the reinforcement of the mesh prepreg is quartz fiber. The steps of the method for preparing the ablation-resistant resin-based composite material are as follows:
[0039] (1) Weigh 500±50g of short fiber prepreg and fill it into the prepared pre-compression mold cavity. Use a mold temperature of 38-42℃ to pre-compact the short fiber prepreg. The filling can be done in steps and pre-compressed multiple times.
[0040] (2) Use a cutting machine to cut the mesh prepreg to the same size as the mold.
[0041] (3) Clean the molding mold and attach the release cloth. Lay a layer of mesh prepreg flat on the bottom surface of the mold, put in the short fiber prepreg blank pre-compacted in step (1), and then lay a layer of mesh prepreg flat on the upper surface of the blank. Close the mold.
[0042] (4) Molding and curing are performed according to the curing process in Table 1. The product is then demolded and its appearance is as shown in Table 1. Figure 1 As shown.
[0043] Table 1 Curing process parameters for Comparative Example 1
[0044]
[0045] like Figure 1 As shown, the ablation-resistant resin-based composite material prepared by this invention has a smooth and dense surface without cracks. This demonstrates that the preparation method of this invention can effectively improve the appearance quality of the product and increase the product qualification rate.
[0046] Comparative Example 1
[0047] A method for preparing an ablation-resistant resin-based composite material, wherein the matrix of the composite material is inorganic particle-modified phenolic resin, and the reinforcement of the short fiber prepreg is chopped quartz fiber, and the method steps for preparing the ablation-resistant resin-based composite material are as follows:
[0048] (1) Weigh 500±50g of short fiber prepreg and fill it into the prepared pre-compression mold cavity. Use a mold temperature of 38-42℃ to pre-compact the short fiber prepreg. The filling can be done in steps and pre-compressed multiple times.
[0049] (2) Clean the molding mold and attach the release cloth, then put in the short fiber prepreg blank pre-compacted in step (1) and close the mold.
[0050] (3) Molding and curing are carried out according to the curing process in Table 2. After demolding, the product is obtained. The appearance of the product is as follows: Figure 2 As shown.
[0051] Table 2 Curing process parameters for Comparative Example 1
[0052]
[0053] like Figure 2 As shown, the composite material demolded product prepared by conventional methods in Comparative Example 1 has a rough surface, obvious cracks, and the cracks have a tendency to propagate.
[0054] Example 2
[0055] Following the methods of Example 1 and Comparative Example 1, 50 demolded products were prepared respectively, for a total of 100 products. The appearance of the 100 products was compared, and the comparison results are shown in Table 3.
[0056] Table 3 Appearance of 100 products
[0057]
[0058] As shown in Table 3, the ablation-resistant resin-based composite material products prepared by the method of the present invention using low pressure and long-term heat preservation curing process have significant appearance advantages compared with the composite material products prepared in Comparative Example 1, and the pass rate is twice that of the composite material products prepared in Comparative Example 1.
Claims
1. A method for preparing an ablation-resistant resin-based composite material, characterized in that, Ablation-resistant resin-based composite material was prepared using modified phenolic resin as the matrix and quartz fiber as the reinforcement, including the following: (1) Fill the short fiber prepreg into the cavity of the pre-compression mold and pre-compact the short fiber prepreg with a mold temperature of 38-42℃; (2) Use a cutting machine to cut the mesh prepreg into the specified size and shape; (3) Set a release cloth in the molding mold, lay a layer of mesh prepreg flat on the release cloth, put in the short fiber prepreg blank pre-compacted in step (1), lay a layer of mesh prepreg flat on the upper surface of the blank, and close the mold. (4) The press is subjected to low pressure and long-term heat preservation parameters at a specific temperature point for molding and curing, and then demolded to obtain the product; The long-term heat preservation parameters include: 10-70 min, 60-60℃; 80-220 min, 100-100℃; The reinforcement of the prepreg is a continuous mesh fabric made of quartz fiber.
2. The preparation method according to claim 1, characterized in that, The low pressure in step (4) is: 0-260 min, 0.5 MPa; 260-400 min, 0.5-5 MPa; 400-760 min, 5 MPa.
3. The preparation method according to claim 2, characterized in that, The low pressure in step (4) is: 260-280 min, 0.5 MPa; 280-300 min, 0.5-5 MPa; 300-400 min, 5 MPa.
4. The preparation method according to claim 1, characterized in that, The long-term heat preservation parameters also include 0-10min, 40-60℃; 70-80min, 60-100℃; 220-260min, 100-125℃; 260-400min, 125-125℃; 400-440min, 125-160℃; 440-580min, 160-160℃; 580-600min, 160-180℃; 600-760min, 180-180℃.
5. The preparation method according to claim 1, characterized in that, The modified phenolic resin is an inorganic particle-modified phenolic resin.
6. The preparation method according to claim 5, characterized in that, The inorganic particles are ceramic powder.
7. The preparation method according to claim 1, characterized in that, The short fiber prepreg reinforcement is glass fiber or high silica glass fiber.
8. The preparation method according to claim 1, characterized in that, The short fiber prepreg reinforcement is chopped quartz fiber.
9. The preparation method according to claim 1, characterized in that, In step (1), the packing can be pre-compressed multiple times in stages.
Citation Information
Patent Citations
Copper-clad plate with two flexible surfaces and preparation method of copper-clad plate with two flexible surfaces
CN103612464A
Ablation-resistant lightweight heatproof integrated composite material with thermal insulation function and preparation method thereof
CN109968757A