Single particle artificial graphite and preparation method thereof, negative electrode material and negative electrode sheet
By using high-temperature graphitization treatment, crushing and chemical modification methods in lithium-ion batteries, the problem of insufficient capacity and rate performance of traditional graphite materials is solved, and efficient electrochemical performance and safety performance improvement is achieved.
Patent Information
- Application Number
- CN202311648364.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-04
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-12-04
AI Technical Summary
Traditional graphite materials have lower capacity and poor rate performance in lithium-ion batteries, which limits their development as negative electrode materials.
Micron-scale graphite powder was pulverized and prepared by graphitizing the coke at 2500℃~3000℃, chemical modification and surface etching were performed to prepare single-particle artificial graphite with high tap density and good conductivity, and used to prepare negative electrode materials. .
It improves the capacity and rate performance of lithium-ion batteries, enhances electrochemical and safety performance, and has good contact with the electrolyte.
Smart Images

Figure CN117658126B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of negative electrode materials, and in particular to a single-particle artificial graphite and a preparation method thereof, a negative electrode material and a negative electrode sheet. Background Art
[0002] Lithium-ion battery is a rechargeable secondary battery that mainly relies on the movement of lithium ions between the positive and negative electrodes. + Insertion and deintercalation back and forth between the two electrodes: During charging, L i+ It is deintercalated from the positive electrode and embedded in the negative electrode through the electrolyte, and the negative electrode is in a lithium-rich state; the opposite is true during discharge. Lithium-ion batteries are composed of positive and negative electrodes using active materials, and electrolytes, and the electrolytes are filled between the positive and negative electrodes. Lithium-ion batteries are widely used in consumer electronics, new energy vehicles, energy storage and other fields due to their advantages such as high energy density, low self-discharge, no memory effect, and good cycle performance.
[0003] The negative electrode active materials of lithium-ion batteries include graphite, silicon-based materials, metal oxide materials and carbon-based composite materials. Among them, graphite materials have the advantages of high stability, good conductivity and abundant resources, and are the more commonly used negative electrode active materials in lithium-ion batteries. However, traditional graphite materials still have problems such as low capacity and poor rate performance, which limits their development as negative electrode materials. Summary of the invention
[0004] Based on this, it is necessary to provide a single-particle artificial graphite with higher capacity and better rate performance and a preparation method thereof.
[0005] In addition, a negative electrode material and a negative electrode sheet containing the above-mentioned single-particle artificial graphite are also provided.
[0006] In one aspect of the present application, a method for preparing a single particle of artificial graphite is provided, comprising the following steps:
[0007] At 2500℃~3000℃, graphitizing the coke to prepare graphite material;
[0008] The graphite material is crushed to prepare graphite powder with a particle size of micrometers;
[0009] Chemically modifying the graphite powder to prepare an intermediate;
[0010] Etching the surface of the intermediate to prepare the single-particle artificial graphite;
[0011] The etching process is performed by using an oxidant or an electrochemical reaction.
[0012] In one embodiment, the oxidant includes at least one of hydrogen peroxide and potassium chlorate.
[0013] In one embodiment, the step of etching by electrochemical reaction includes:
[0014] The intermediate is used as a working electrode to form a three-electrode system with a reference electrode and a counter electrode;
[0015] The working electrode, the reference electrode and the counter electrode are immersed in an electrolyte, and under the action of a voltage, an oxidation reaction occurs on the surface of the intermediate to form an etched structure.
[0016] In one embodiment, the graphitization treatment time is 2 hours to 3 hours.
[0017] In one embodiment, the graphite powder has a particle size of 1 μm to 100 μm.
[0018] In one embodiment, the chemical modification treatment includes one of oxidation treatment, reduction treatment, and surface modification treatment;
[0019] The surface modification treatment comprises: coating the graphite powder with a surface modifier.
[0020] In a second aspect, the present application also provides artificial graphite prepared according to the method for preparing single-particle artificial graphite according to the first aspect.
[0021] In one embodiment, the particle size D10 of the single-particle artificial graphite is 4 μm to 6 μm; the particle size D50 of the single-particle artificial graphite is 9 μm to 15 μm; and the particle size D90 of the single-particle artificial graphite is 17 μm to 27 μm.
[0022] In a third aspect, the present application also provides a negative electrode material, comprising the single-particle artificial graphite of the second aspect above.
[0023] In a fourth aspect, the present application also provides a negative electrode sheet, comprising the negative electrode material of the third aspect mentioned above.
[0024] The method for preparing single-particle artificial graphite provided in the embodiment of the present application is to prepare a graphite material by graphitizing coke, and then crush, chemically modify, and perform surface etching to obtain single-particle artificial graphite; the obtained single-particle artificial graphite has a higher tap density, better surface contact with the electrolyte, better conductivity, and has a higher capacity and better rate performance when used as a negative electrode material. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 A scanning electron microscope photograph of a single particle of artificial graphite prepared in Example 1 of the present application;
[0026] Figure 2 This is a scanning electron microscope photograph of a single particle of artificial graphite prepared in Example 1 of the present application. DETAILED DESCRIPTION
[0027] In order to facilitate the understanding of the present application, the present application will be described more fully below with reference to the relevant drawings. The preferred embodiments of the present application are given in the drawings. However, the present application can be implemented in many different forms and is not limited to the embodiments described herein. On the contrary, the purpose of providing these embodiments is to make the understanding of the disclosure of the present application more thorough and comprehensive.
[0028] In this article, the technical features described in an open manner include closed technical solutions composed of the listed features, and also include open technical solutions containing the listed features.
[0029] Herein, when it comes to numerical ranges, unless otherwise specified, the numerical ranges are deemed to be continuous and include the minimum and maximum values of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values of the range is included. In addition, when multiple ranges are provided to describe features or characteristics, the ranges can be merged. In other words, unless otherwise specified, all ranges disclosed herein should be understood to include any and all subranges included therein.
[0030] In this article, when referring to the unit of a data range, if there is a unit only after the right endpoint, it means that the units of the left and right endpoints are the same. For example, 800-850nm means that the units of the left endpoint "800" and the right endpoint "850" are both nm (nanometers).
[0031] Only some numerical ranges are specifically disclosed herein. However, any lower limit can be combined with any upper limit to form an unspecified range; and any lower limit can be combined with other lower limits to form an unspecified range, and likewise any upper limit can be combined with any other upper limit to form an unspecified range. In addition, each separately disclosed point or single value can itself be combined as a lower limit or upper limit with any other point or single value or with other lower limits or upper limits to form an unspecified range.
[0032] The temperature parameters herein, unless otherwise specified, allow for both constant temperature treatment and treatment within a certain temperature range. The constant temperature treatment allows for temperature fluctuations within the precision range of instrument control.
[0033] In this article, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of the invention, the meaning of "multiple" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the description of this application, the meaning of "several" is at least one, such as one, two, etc., unless otherwise clearly and specifically defined.
[0034] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0035] If there is no special explanation, all steps of the present application can be performed sequentially or randomly, preferably sequentially. For example, the method includes steps (a) and (b), which means that the method may include steps (a) and (b) performed sequentially, or may include steps (b) and (a) performed sequentially. For example, the method may further include step (c), which means that step (c) may be added to the method in any order. For example, the method may include steps (a), (b) and (c), or may include steps (a), (c) and (b), or may include steps (c), (a) and (b), etc.
[0036] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art to which the present application belongs. The terms used herein in the specification of the present application are only for the purpose of describing specific embodiments and are not intended to limit the present application. The term "and / or" used herein includes any and all combinations of one or more of the related listed items.
[0037] An embodiment of the present application provides a method for preparing a single-particle artificial graphite, including the following steps S100 to S400.
[0038] Step S100: Graphitizing the coke at 2500°C to 3000°C to prepare a graphite material. By graphitizing at 2500°C to 3000°C, an artificial graphite material close to the structure of natural graphite can be obtained. Optionally, the temperature of the graphitization treatment is 2500°C, 2600°C, 2700°C, 2800°C, 2900°C, 3000°C or any range of the above values.
[0039] In some embodiments, the graphitization treatment time is 2 hours to 3 hours.
[0040] In some embodiments, the coke is prepared by calcining a carbon source, which includes one or more of petroleum coke and biomass.
[0041] Step S200: crushing the graphite material to prepare graphite powder with a particle size of micrometer level.
[0042] In some embodiments, the particle size of the graphite powder is 1 μm to 100 μm. Optionally, the particle size of the graphite powder is 1 μm, 2 μm, 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 80 μm, 90 μm, 100 μm or any range of the above values. Further, the particle size of the graphite powder is 1 μm to 30 μm.
[0043] In some embodiments, step S200 uses a high-energy ball mill or a jet mill to perform pulverization.
[0044] Step S300: chemically modifying graphite powder to prepare an intermediate.
[0045] In one embodiment, the chemical modification treatment includes one of oxidation treatment, reduction treatment and surface modification treatment. Further, the chemical modification treatment is surface modification treatment.
[0046] The oxidation treatment is to treat the graphite powder with an oxidant. Optionally, the oxidant includes one or more of concentrated sulfuric acid, nitric acid, and hydrogen peroxide.
[0047] In some embodiments, the oxidation treatment includes: in a cooling water bath, uniformly mixing an oxidant and graphite powder to carry out an oxidation reaction; after the oxidation reaction is completed, washing the solid product with deionized water until the washing liquid is neutral, thereby obtaining graphite oxide powder.
[0048] In some embodiments, the oxidizing agent for the oxidation treatment is concentrated sulfuric acid and nitric acid. The oxidation treatment is specifically as follows: in a cooling water bath, concentrated sulfuric acid is slowly added to the graphite powder, followed by the slow addition of nitric acid, and the mixture is stirred and mixed evenly. Under the cooling water bath conditions, the reaction is carried out for about 2 hours to ensure that the graphite powder is fully in contact with the oxidant. After the reaction is completed, the oxidized graphite powder is rinsed with deionized water and repeatedly rinsed until the pH value is close to neutral. The oxidized graphite powder is then dried under vacuum conditions to obtain oxidized graphite powder. In some embodiments, the mass ratio of graphite powder, concentrated sulfuric acid and nitric acid is 1:3:1.
[0049] In some embodiments, the oxidant of the oxidation treatment is hydrogen peroxide. The oxidation treatment is specifically as follows: the graphite powder is mixed evenly with a 30% hydrogen peroxide solution at a mass ratio of 1:5; and then stirred continuously at room temperature for about 3 hours. After the reaction is completed, the residual hydrogen peroxide on the surface of the oxidized graphite powder is washed with deionized water, and then the oxidized graphite powder is dried under vacuum conditions to obtain oxidized graphite powder.
[0050] In some embodiments, the reduction treatment includes: reducing the graphite powder with a reducing agent. Specifically, the reducing agent includes but is not limited to hydrogen and sodium hydride. The reduction treatment can reduce the oxidized graphite and improve its conductive properties.
[0051] In some embodiments, the reducing agent is hydrogen, and the reduction treatment is specifically as follows: the graphite powder is reacted at 500° C. to 900° C. for 2 to 3 hours in a hydrogen atmosphere.
[0052] In some embodiments, the reducing agent is sodium hydride, and the reduction treatment is specifically: mixing graphite powder and sodium hydride to allow the mixture to fully react with reduction. Specifically, the temperature of the reduction reaction can be room temperature or in the range of 800°C to 900°C. When the reduction treatment is carried out at room temperature, the graphite powder and sodium hydride are mixed and reacted in an ethanol solvent. When the reduction treatment temperature is 800°C to 900°C, the graphite powder and sodium hydride are evenly mixed and then placed in a heating furnace for heating and reduction treatment.
[0053] The surface modification treatment includes: coating the graphite powder with a surface modifier. In some embodiments, the surface modifier includes but is not limited to a silane coupling agent and polypyrrolidone. The surface of the graphite powder is modified by the surface modification treatment, so that the wettability of the graphite powder to the electrolyte can be improved.
[0054] In some embodiments, the surface modifier is a silane coupling agent, and the surface modification treatment is specifically as follows: adding graphite powder to a solution of a silane coupling agent, stirring at room temperature for 2 hours, so that the graphite surface fully reacts with the silane coupling agent. The modified graphite powder is then vacuum filtered to remove excess silane coupling agent solution, and dried to obtain surface-modified graphite powder. In some embodiments, the silane coupling agent solution is an ethanol solution of a silane coupling agent. Specifically, in the silane coupling agent solution, the volume percentage of the silane coupling agent is 1% (v / v). Silane coupling agents include but are not limited to γ-aminopropyltrimethoxysilane.
[0055] In some embodiments, the surface modifier is polypyrrolidone, and the surface modification treatment is specifically as follows: pyrrole and sulfuric acid solution are mixed evenly. Then graphite powder is added and stirred continuously, and the electrochemical reaction causes pyrrole to polymerize on the surface of the graphite powder to generate polypyrrolidone on the surface of the graphite powder. After the reaction is completed, the modified graphite powder is rinsed with deionized water to remove unreacted pyrrole and sulfuric acid, and then dried under vacuum conditions.
[0056] Step S400: etching the surface of the intermediate. The etching is performed by using an oxidant or an electrochemical reaction. By etching the surface of the intermediate, a micro-nano comb structure can be formed on the surface, thereby improving the contact area and conductivity between the graphite and the electrolyte and enhancing its electrochemical performance.
[0057] In one embodiment, the oxidant includes at least one of hydrogen peroxide and potassium chlorate.
[0058] In some embodiments, the oxidant is hydrogen peroxide, and the surface etching treatment is specifically as follows: the intermediate is added to a 30% hydrogen peroxide solution, the intermediate is completely immersed in the solution, and is kept for about 30 minutes, so that the surface of the intermediate reacts with the hydrogen peroxide to form a comb-like structure. After the reaction is completed, the reacted solid is rinsed with deionized water to remove the hydrogen peroxide residue on the surface and other oxides that may be produced.
[0059] In some embodiments, the oxidant is potassium chlorate, and the surface etching treatment is specifically as follows: the intermediate is added to a 0.5M potassium chlorate solution, the intermediate is completely immersed in the solution, and maintained for about 30 minutes, so that the intermediate reacts with potassium chlorate to form a comb-like structure. After the reaction is completed, the reacted solid is rinsed with deionized water to remove potassium chlorate and other possible chloride residues on the surface.
[0060] In one embodiment, the step of etching by electrochemical reaction includes:
[0061] (1) The intermediate is used as the working electrode to form a three-electrode system with the reference electrode and the counter electrode.
[0062] (2) The working electrode, the reference electrode and the counter electrode are immersed in an electrolyte, and under the action of voltage, an oxidation reaction occurs on the surface of the intermediate to form an etched structure. Specifically, the electrolyte can be a 1M sulfuric acid solution. The voltage is set to 2.0V. The reaction time is 20 minutes to 30 minutes.
[0063] In some embodiments, after step S400, the method further includes:
[0064] Step S500: ball milling the graphite material that has undergone surface etching treatment to prepare single-particle artificial graphite.
[0065] The method for preparing the above-mentioned single-particle artificial graphite is to prepare graphite material by graphitizing coke, and then crush, chemically modify, and perform surface etching to obtain the single-particle artificial graphite; the obtained single-particle artificial graphite has a higher tap density, better surface contact with the electrolyte, better conductivity, and has a higher capacity and better rate performance when used as a negative electrode material. In addition, the single-particle artificial graphite obtained according to the above-mentioned preparation method also has better safety performance.
[0066] Another embodiment of the present application also provides artificial graphite prepared according to the above-mentioned method for preparing single-particle artificial graphite. The above-mentioned single-particle artificial graphite has a higher capacity and better rate performance. At the same time, it also has better safety performance.
[0067] In one embodiment, the particle size D10 of a single particle of artificial graphite is 4 μm to 6 μm; the particle size D50 of a single particle of artificial graphite is 9 μm to 15 μm; and the particle size D90 of a single particle of artificial graphite is 17 μm to 27 μm.
[0068] In some embodiments, the tap density of a single particle of artificial graphite is ≥1.15 g / cm 3 Furthermore, the tap density of a single particle of artificial graphite is 1.15 g / cm 3 ~1.3g / cm 3 Optionally, the tap density of a single particle of artificial graphite is 1.15 g / cm 3 , 1.18g / cm 3 , 1.20g / cm 3 , 1.24g / cm 3 , 1.25g / cm 3 , 1.26g / cm 3 , 1.28g / cm 3 , 1.3g / cm 3 Or any range of the above values.
[0069] In some embodiments, the specific surface area of a single particle of artificial graphite is ≤2.5 m 2 / g. Furthermore, the specific surface area of a single particle of artificial graphite is 1.8m 2 / g~2.5m 2 / g. Optionally, the specific surface area of a single particle of artificial graphite is 1.8m 2 / g, 1.9m 2 / g, 2.0m 2 / g, 2.1m 2 / g, 2.2m 2 / g, 2.3m 2 / g, 2.4m 2 / g, 2.5m2 / g or any of the above values.
[0070] Another embodiment of the present application further provides a negative electrode material, comprising the above-mentioned single-particle artificial graphite.
[0071] Another embodiment of the present application further provides a negative electrode sheet, comprising the above-mentioned negative electrode material. Generally, the negative electrode sheet comprises a negative electrode current collector and an active material layer disposed on the surface of the negative electrode current collector. The active material layer comprises the above-mentioned negative electrode material. In addition, the active material layer may also optionally include a conductive agent, a binder and an auxiliary agent.
[0072] In some embodiments, the conductive agent includes one or more of Ketjen black, conductive carbon black, graphene, and carbon nanotubes.
[0073] In some embodiments, the binder includes one or more of acrylate, polyacrylonitrile, and styrene-butadiene rubber.
[0074] Another embodiment of the present application also provides a secondary battery, including the above-mentioned negative electrode sheet. The secondary battery including the above-mentioned negative electrode sheet uses the above-mentioned single-particle artificial graphite as the negative electrode active material, and the secondary battery has a higher capacity and better rate performance. At the same time, it also has better safety performance.
[0075] Specifically, the secondary battery also includes a positive electrode sheet, a separator and an electrolyte.
[0076] In some embodiments, secondary batteries include, but are not limited to, lithium ion batteries, lithium metal batteries, sodium ion batteries, solid-state batteries, and the like.
[0077] In order to make the purpose, technical solutions and advantages of the present application more concise and clear, the present application is described with the following specific embodiments, but the present application is by no means limited to these embodiments. The embodiments described below are only preferred embodiments of the present application and can be used to describe the present application, and cannot be understood as limiting the scope of the present application. It should be pointed out that any modifications, equivalent substitutions and improvements made within the spirit and principles of the present application should be included in the protection scope of the present application.
[0078] Embodiment 1:
[0079] The method for preparing the single-particle artificial graphite of this embodiment comprises the following steps:
[0080] (1) Graphite material was prepared by graphitizing coke at 2500°C for 3 hours.
[0081] (2) Mechanically crushing the graphite material to prepare graphite powder with a particle size of 1 μm to 20 μm.
[0082] (3) The graphite powder was reacted at 900° C. for 3 hours in a hydrogen atmosphere to prepare reduced graphite powder.
[0083] (4) Add the reduced graphite powder obtained in step (3) to the solution of silane coupling agent, and stir at room temperature for 2 hours to allow the graphite surface to fully react with the silane coupling agent. Then, the modified graphite powder is vacuum filtered to remove excess silane coupling agent solution, and dried to obtain surface-modified graphite powder. The silane coupling agent solution is 1% (v / v) γ-aminopropyltrimethoxysilane in ethanol.
[0084] (5) Add the surface-modified graphite powder to a 0.5 M potassium chlorate solution, completely immerse the graphite powder in the solution, and keep it for about 30 minutes to allow the graphite powder to react with the potassium chlorate to form a comb-like structure. After the reaction is completed, rinse the reacted graphite powder with deionized water to remove the potassium chlorate and other possible chloride residues on the surface, thereby obtaining a graphite powder with a comb-like structure on the surface.
[0085] (6) The graphite powder obtained in step (5) is ball-milled to obtain the single-particle artificial graphite of this embodiment.
[0086] See also Figure 1 , Figure 2 , is a scanning electron microscope photo of the single particle artificial graphite prepared in this example. The physical properties of the prepared single particle artificial graphite are recorded in Table 1.
[0087] Table 1
[0088]
[0089] Embodiment 2:
[0090] The method for preparing the single-particle artificial graphite of this embodiment comprises the following steps:
[0091] (1) Graphite material was prepared by graphitizing coke at 2500°C for 3 hours.
[0092] (2) Mechanically crushing the graphite material to prepare graphite powder with a particle size of 1 μm to 20 μm.
[0093] (3) Add graphite powder to the solution of silane coupling agent and stir at room temperature for 2 hours to allow the graphite surface to fully react with the silane coupling agent. Then, the modified graphite powder is vacuum filtered to remove excess silane coupling agent solution and dried to obtain surface-modified graphite powder. The silane coupling agent solution is 1% (v / v) γ-aminopropyltrimethoxysilane in ethanol.
[0094] (4) Add the surface-modified graphite powder to a 0.5M potassium chlorate solution, completely immerse the graphite powder in the solution, and keep it for about 30 minutes to allow the graphite powder to react with the potassium chlorate to form a comb-like structure. After the reaction is completed, rinse the reacted graphite powder with deionized water to remove the potassium chlorate and other possible chloride residues on the surface, thereby obtaining a graphite powder with a comb-like structure on the surface.
[0095] (5) The graphite powder obtained in step (4) is ball-milled to obtain the single-particle artificial graphite of this embodiment.
[0096] Comparative Example 1:
[0097] This comparative example uses commercially available natural graphite as the negative electrode active material.
[0098] Test example:
[0099] Preparation of working electrode: The negative electrode active material of the above embodiment or comparative example, the conductive agent SuperP and the binder PVDF are prepared into slurry in a mass ratio of 92:3:5. The slurry is then coated on a copper foil to prepare a working electrode.
[0100] Battery preparation: Lithium foil as counter electrode; electrolyte contains 1M LiPF 6 The solvent is a mixed solvent of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a volume ratio of 1:1:1, and the electrolyte also contains 1wt% of vinylene carbonate (VC) as an additive. The working electrode, the separator, and the counter electrode are stacked to prepare a battery cell, and then the electrolyte is injected to prepare a battery to be tested.
[0101] The prepared battery was subjected to electrochemical testing in the following manner. The test results are recorded in Table 2.
[0102] Capacity test method: Charge and discharge the battery to be tested to its rated voltage, test its discharge capacity under 1C charge and discharge conditions, and record its capacitance value under 1C.
[0103] First coulomb efficiency test method: Charge the test battery to full charge for the first time and record its charge capacity; then discharge it for the first time and record its discharge capacity. First coulomb efficiency = (first discharge capacity / first charge capacity) × 100%.
[0104] Resistance test method: Use a battery internal resistance tester to test the battery to be tested.
[0105] Cycle stability (200-cycle capacity retention) test method: Perform 200 charge and discharge cycles on the battery, and compare the discharge capacity after the 100th cycle with the initial discharge capacity. Capacity retention = (200th cycle discharge capacity / initial discharge capacity) * 100%.
[0106] Rate performance (2C vs 1C capacity retention) test method: Test the discharge capacity of the battery under test at different discharge rates (1C, 2C). 2C vs 1C capacity retention = (2C discharge capacity / 1C discharge capacity) × 100%.
[0107] Table 2
[0108]
[0109]
[0110] It can be seen from the relevant data in Table 2 that compared with the natural graphite in Comparative Example 1, the batteries prepared from the single-particle artificial graphite in Examples 1 and 2 have higher capacity, first coulombic efficiency, cycle stability and rate performance, and lower internal resistance. The batteries prepared in Examples 1 and 2 have better electrochemical performance.
[0111] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0112] The above-described embodiments only express several implementation methods of the present application, which is convenient for understanding the technical solutions of the present application in detail, but cannot be understood as limiting the scope of protection of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present application, several modifications and improvements can be made, which all belong to the protection scope of the present application. It should be understood that the technical solutions obtained by those skilled in the art through logical analysis, reasoning or limited experiments on the basis of the technical solutions provided in the present application are all within the protection scope of the attached claims described in the present application. Therefore, the protection scope of the patent of this application shall be based on the contents of the attached claims, and the description and drawings can be used to explain the contents of the claims.
Claims
1. A method for preparing single-particle artificial graphite, characterized in that: The following steps are involved: At 2500℃~3000℃, graphitization treatment is performed on coke to prepare graphite material; The graphite material is crushed to prepare graphite powder with a particle size of micrometers; Adding graphite powder to a solution of a silane coupling agent so that the surface of the graphite powder fully reacts with the silane coupling agent, filtering the reacted graphite powder by vacuum filtration to remove excess silane coupling agent solution, and drying to obtain a surface-modified graphite powder; The surface-modified graphite powder is added into a potassium chlorate solution to react the graphite powder with the potassium chlorate to form a comb-like structure. After the reaction is completed, the reacted graphite powder is rinsed with deionized water to remove the potassium chlorate and other possible chloride residues on the surface, thereby obtaining a graphite powder with a comb-like structure on the surface. The obtained graphite powder is ball-milled to obtain single-particle artificial graphite.
2. The method for preparing single-particle artificial graphite according to claim 1, characterized in that: The graphitization treatment time is 2 hours to 3 hours.
3. The method for preparing single-particle artificial graphite according to claim 1, characterized in that: The particle size of the graphite powder is 1 μm to 100 μm.
4. Single-particle artificial graphite obtained according to the method for preparing single-particle artificial graphite according to any one of claims 1 to 3.
5. The single-particle artificial graphite according to claim 4, characterized in that: The particle size D10 of the single-particle artificial graphite is 4 μm to 6 μm; the particle size D50 of the single-particle artificial graphite is 9 μm to 15 μm; and the particle size D90 of the single-particle artificial graphite is 17 μm to 27 μm.
6. A negative electrode material, characterized in that: The invention comprises the single-particle artificial graphite as claimed in claim 4 or 5.
7. A negative electrode sheet, characterized in that: Comprising the negative electrode material as claimed in claim 6.
Citation Information
Cited By
Micro-oxidation artificial graphite lithium ion battery negative electrode material and preparation method thereof
CN122091547A