A water-absorbing and water-retaining double-layer coated film urea slow-release fertilizer and preparation method thereof
By adopting water-absorbing and water-retaining double-layer coating technology on urea, and using coating film made of materials such as epoxy resin and corn cob powder, the problems of low urea utilization and insufficient envelope strength are solved, and efficient slowing down Controlled release fertilizer effect and green and environmentally friendly resource utilization.
Patent Information
- Application Number
- CN202311635646.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-01
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-12-01
AI Technical Summary
In the prior art, the current utilization rate of urea is low, and it is prone to volatilization, swelling and runoff, resulting in waste of fertilizer and water resources pollution. The coating strength of the enveloped slow-release fertilizer is low, making it easy to cause sudden swelling and explosions. , poor slow control performance.
Adopting water-absorbing and water-retaining double-layer coating technology, the inner coating is made of epoxy resin and diisopropylaminoethyl methacrylate, and the outer coating is made of corn coin powder, bentonite, sodium alginate, acrylic acid Made of other materials and add microbial bacterial agents to enhance compression and antibacterial properties.
显著提高了尿素的缓控释能,延长了养分释放时间,提高了肥料的利用率和作物产量,增强了土壤的抗压性和保水性,同时实现了绿色环保的资源利用。
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of slow-release fertilizers, and in particular relates to a water-absorbing and water-retaining double-layer coated urea slow-release fertilizer and a preparation method thereof. Background Art
[0002] The amount of agricultural fertilizer applied has been increasing year by year. However, the utilization rate of fertilizers in the current season is generally low, especially for urea. Due to volatilization, leaching and runoff, the utilization rate in the current season is even lower. High fertilizer application rate not only causes waste of fertilizers, but also pollutes water resources, causes soil compaction, and leads to serious problems.
[0003] Rice husks and corn cobs are abundant agricultural by-products in my country. They have a hard surface and are not easily decomposed by bacteria. Rice husks contain about 40% crude fiber, 20% pentose polymers, 20% ash and a small amount of crude protein, crude fat and other nutrients. However, most rice husks are wasted or directly applied to the fields, resulting in a waste of resources. Corn cobs are the by-product of corn cob threshing. They have the advantages of uniform texture, appropriate hardness, good toughness, strong water absorption and good wear resistance. However, most corn cobs cannot be effectively utilized. In rural areas, most of them are directly discarded or dried and used as firewood, with low utilization rate.
[0004] With the progress of science, the concept of slow-release fertilizers has been gradually applied to agricultural production. Slow-release fertilizers are divided into three categories: coated, wrapped, and synthetic. Among them, coated slow-release fertilizers are the main ones. Coated slow-release fertilizers are composed of "fertilizer core + coating layer". On the other hand, water is also an important factor restricting agricultural development. It not only affects the growth of crops, but also plays an important role in the effectiveness of fertilizers. Therefore, combining coated slow-release fertilizers with water-retaining agents to develop water-absorbing and water-retaining slow-release fertilizers to achieve mutual promotion of water and fees, improve soil structure, and increase fertilizer utilization has become the main trend in fertilizer production development.
[0005] Patent CN107162747B discloses a method for preparing a multifunctional composite water-retaining slow-release fertilizer. The coating material is made of cyclodextrin, water-soluble monomer, urea-loaded halloysite, cross-linking agent, and initiator as raw materials, and is formed by free radical polymerization. Although the water-soluble monomer absorbs a large amount of water when the nutrients are released, the coating film has low strength, which will cause sudden swelling and explosion, resulting in a large amount of nutrient release. Moreover, the coating film is a single-layer coating film, which only retains water absorption performance, poor slow-control performance, short slow-control time and difficult to control. Although the organic polymer coated fertilizer has a good nutrient controlled release effect, after the nutrients are released, the organic polymer shell remaining in the soil is difficult to degrade, and it will still cause pollution to the soil environment after being applied for many years. Therefore, it is of great significance to prepare a coated film slow-release fertilizer with green and environmental protection, high water absorption and water retention, high compressive strength, and good slow-release fertilizer for the development of agricultural fertilizers. . Summary of the invention
[0006] The invention overcomes the shortcomings of the prior art and discloses a water-absorbing and water-retaining double-layer coating film slow-release fertilizer. Rice husks and corn cob powder are used as raw materials for the outer coating film. The inner coating film is modified with epoxy resin and diisopropylaminoethyl methacrylate to be hydrophobic and controllably modified. The outer coating film uses palm kernel oil diethanolamide as a promoter to enhance the compression resistance and water-absorbing and water-retaining performance of the outer coating film. Microbial agents are added to enhance the insect and antibacterial effects of crops, improve fertilizer utilization, and increase crop yield and quality.
[0007] In order to achieve the above technical objectives, the technical solution adopted by the present invention is:
[0008] The invention discloses a water-absorbing and water-retaining double-layer coated slow-release fertilizer, which comprises 60-80 parts of urea as an inner core, 10-15 parts of epoxy-hydrophobically modified rice husk fiber resin as an inner coating film, and an outer coating film of a composite highly absorbent resin prepared from 20-30 parts of corn cob powder, 12-15 parts of bentonite, 8-10 parts of sodium alginate, 13-18 parts of acrylic acid, 5-8 parts of an accelerator, 2-5 parts of an initiator, 3-8 parts of a cross-linking agent, 3-5 parts of a solubilizing agent, and 6-8 parts of a microbial agent.
[0009] The preparation method of the above-mentioned epoxy hydrophobically modified rice husk fiber resin is as follows:
[0010] 40-60 parts by weight of rice husks are washed and impurity-removed, dried to a water content of less than 5%, crushed and ground, passed through a 200-mesh sieve, soaked in 1.5% hydrochloric acid for 24 hours, filtered and added to a reaction container, 2-3 times the volume of distilled water are added, heated and stirred at 53-68° C. for 30 minutes, 10-20 parts by weight of epoxy resin, 15-30 parts by weight of rosin, and 2-5 parts by weight of diisopropylaminoethyl methacrylate are added in sequence, the pH value is adjusted to 8-10 with a sodium hydroxide solution with a mass concentration of 1 mol / L, heated and stirred at 110-150° C. for 2-5 hours, the pH value is adjusted to neutral with a 1.5% hydrochloric acid solution, heated and stirred at 80-85° C. until the solution is viscous, dried and crushed to obtain epoxy hydrophobically modified rice husk fiber resin.
[0011] The preparation method of the above-mentioned composite super absorbent resin is:
[0012] Add corn cob powder and bentonite into a reactor, add 3-5 times volume of distilled water, stir at 85°C for 30-45min, add maleic anhydride, stir at 40-45°C for 15-20min, add acrylic acid and palm kernel oil diethanolamide in sequence, heat and stir at 40-60°C for 2-3h, add sodium alginate, initiator potassium persulfate, cross-linking agent N,N-methylenebisacrylamide in sequence, heat and stir at 70-90°C for 2-3h, dry, crush and sieve, add microbial agent to obtain a composite super absorbent resin;
[0013] The above-mentioned microbial agent is a mixture of Bacillus subtilis and Bacillus licheniformis in a culture solution mass ratio of 1:1. The preparation method is: Bacillus subtilis and Bacillus licheniformis are cultured in a liquid seed culture medium at 30°C for 24 hours, and then inoculated into LB culture medium at a 10% inoculation rate, respectively, and cultured with shaking at 30°C until the bacterial concentration is OD600≈3.0, and then mixed evenly at a culture solution mass ratio of 1:1, and freeze-dried into freeze-dried powder to obtain a microbial agent.
[0014] Preferably, the accelerator is palm kernel oil diethanolamide.
[0015] Preferably, the initiator is potassium persulfate.
[0016] Preferably, the cross-linking agent is N,N-methylenebisacrylamide.
[0017] Preferably, the solubilizing agent is maleic anhydride.
[0018] The present invention also provides a method for preparing a water-absorbing and water-retaining double-layer coated slow-release fertilizer, the steps of which are as follows:
[0019] Add urea to the coating machine, spray atomized water to evenly wet the urea, add molten epoxy hydrophobically modified rice husk fiber resin for coating in 3-5 times, so that the epoxy hydrophobically modified rice husk fiber resin is evenly coated on the surface of the urea, and dry for 24-48 hours after the coating is completed; add the coated dry particles to the coating machine, wet the particle surface with atomized linseed oil, add molten composite super absorbent resin for coating in 3-5 times, so that the composite super absorbent resin is evenly coated on the particle surface, and dry for 24-48 hours after the coating is completed to obtain a water-absorbing and water-retaining double-layer coated film slow-release fertilizer with a particle size of 3-5 mm.
[0020] The water-absorbing and water-retaining double-layer coated slow-release fertilizer provided by the present invention has the following beneficial effects:
[0021] The present invention coats urea with inner and outer double layers, wherein the inner coating film performs hydrophobic and controllable modification on the fertilizer, and the outer coating film is made of corn cob powder, bentonite, sodium alginate, and acrylic acid as raw materials, and a promoter is added to prepare a water-absorbing and water-retaining resin for coating. Compared with the prior art, a pH-sensitive hydrophobic monomer diisopropylaminoethyl methacrylate is added during the hydrophobic modification of the inner coating film, thereby increasing the hydrophobic degree of the hydrophobic modification and ensuring the controllability of the fertilizer release. When the crops lack nutrients, the roots secrete citric acid, reduce the pH around the roots, and promote the accelerated release of nutrients; when the crops do not lack nutrients and no acidic components are generated around the roots, the inner coating film controls and reduces the release of nutrients; and the outer During the preparation process of the coating film, surfactant palm kernel oil diethanolamide is added as a promoter, which enhances the firmness of the cross-linking bond of the graft copolymer corn cob powder, bentonite, sodium alginate and acrylic acid, increases the compressive strength of the fertilizer, and significantly increases the water absorption and water retention of the coating film; the selected raw materials rice husks and corn cob powder are natural and environmentally friendly, and waste resources are utilized; the added microbial agents improve the insect and antibacterial properties of crops; the inner and outer coating films are used in combination to double-coat the fertilizer, nutrients are not easily lost, the fertilizer effect is more lasting, and the nutrient release is in line with the growth law of crops, which greatly improves the utilization rate of the fertilizer, and improves the water absorption and water retention characteristics, promotes crop income and yield, and improves planting benefits. DETAILED DESCRIPTION
[0022] The present invention is further explained below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention. After reading the present invention, various equivalent modifications to the present invention by those skilled in the art all fall within the scope of protection of the claims of this application.
[0023] Example 1
[0024] (1) Preparation of microbial agents:
[0025] Bacillus subtilis and Bacillus licheniformis were cultured in a liquid seed culture medium at 30°C for 24 hours, respectively, and then inoculated into LB culture medium at a 10% inoculation rate, respectively, and cultured under shaking at 30°C until the bacterial concentration reached OD600≈3.0, and then mixed evenly at a mass ratio of 1:1, and freeze-dried into freeze-dried powder to obtain a microbial agent;
[0026] (2) Preparation of epoxy-hydrophobically modified rice husk fiber resin:
[0027] 50 g of rice husk was washed and impurities were removed, and then dried under ventilation until the moisture content was less than 5%, crushed and ground, passed through a 200-mesh sieve, and soaked in 1.5% hydrochloric acid for 24 hours. The mixture was filtered and added to a reaction container, and 3 times the volume of distilled water was added. The mixture was heated and stirred at 53° C. for 30 minutes. 15 g of epoxy resin, 20 g of rosin, and 3 g of diisopropylaminoethyl methacrylate were added in sequence. A sodium hydroxide solution with a mass concentration of 1 mol / L was added to adjust the pH to 8, and the mixture was heated and stirred at 110° C. for 2 hours. A hydrochloric acid solution with a mass fraction of 1.5% was used to adjust the pH to neutral, and the mixture was heated and stirred at 80° C. until the solution became viscous. The mixture was dried and crushed and passed through a 100-mesh sieve to obtain an epoxy-hydrophobically modified rice husk fiber resin.
[0028] (3) Preparation of composite super absorbent resin:
[0029] Add 25g corncob powder and 15g bentonite into a reactor, add 3 times the volume of distilled water, stir at 85°C for 30min, add 5g maleic anhydride, stir at 40°C for 15min, add 15g acrylic acid and 5g palm kernel oil diethanolamide in sequence, heat and stir at 40°C for 2h, add 10g sodium alginate, 2g initiator potassium persulfate, and 5g cross-linking agent N,N-methylenebisacrylamide in sequence, heat and stir at 70°C for 2h, dry and crush through a 100-mesh sieve to obtain a composite super absorbent resin;
[0030] (4) Encapsulation
[0031] Add 80g of urea into a coating machine, spray atomized water to evenly moisten the urea, add molten epoxy hydrophobically modified rice husk fiber resin for coating three times, so that the epoxy hydrophobically modified rice husk fiber resin is evenly coated on the surface of the urea, and dry for 24 hours after the coating is completed; add the coated dry particles into a coating machine, moisten the particle surface with atomized linseed oil, add molten composite super absorbent resin for coating five times, so that the composite super absorbent resin is evenly coated on the particle surface, and dry for 48 hours after the coating is completed to obtain a water-absorbing and water-retaining double-layer coated film controlled-release fertilizer with a particle size of 5 mm.
[0032] Example 2
[0033] (1) Preparation of microbial agents:
[0034] Bacillus subtilis and Bacillus licheniformis were cultured in a liquid seed culture medium at 30°C for 24 hours, respectively, and then inoculated into LB culture medium at a 10% inoculation rate, respectively, and cultured under shaking at 30°C until the bacterial concentration reached OD600≈3.0, and then mixed evenly at a mass ratio of 1:1, and freeze-dried into freeze-dried powder to obtain a microbial agent;
[0035] (2) Preparation of epoxy-hydrophobically modified rice husk fiber resin:
[0036] 60 g of rice husk was washed and impurities were removed, and then dried under ventilation until the moisture content was less than 5%, crushed and ground, passed through a 200-mesh sieve, soaked in 1.5% hydrochloric acid for 24 hours, filtered and added to a reaction container, 3 volumes of distilled water were added, heated and stirred at 53° C. for 30 minutes, 20 g of epoxy resin, 15 g of rosin, and 5 g of diisopropylaminoethyl methacrylate were added in sequence, and a sodium hydroxide solution with a mass concentration of 1 mol / L was added to adjust the pH to 9, heated and stirred at 110° C. for 2 hours, and a hydrochloric acid solution with a mass fraction of 1.5% was used to adjust the pH to neutral, heated and stirred at 80° C. until the solution was viscous, dried and crushed, and passed through a 100-mesh sieve to obtain an epoxy-hydrophobically modified rice husk fiber resin;
[0037] (3) Preparation of composite super absorbent resin:
[0038] Add 20g corncob powder and 12g bentonite into a reactor, add 5 times the volume of distilled water, stir at 85°C for 30min, add 5g maleic anhydride, stir at 40°C for 15min, add 13g acrylic acid and 8g palm kernel oil diethanolamide in sequence, heat and stir at 40°C for 2h, add 8g sodium alginate, 5g potassium persulfate, and 3g N,N-methylenebisacrylamide in sequence, heat and stir at 70°C for 2h, dry and crush through a 100-mesh sieve to obtain a composite super absorbent resin;
[0039] (4) Encapsulation
[0040] Add 80g of urea into a coating machine, spray atomized water to evenly wet the urea, add molten epoxy hydrophobically modified rice husk fiber resin for coating three times, so that the epoxy hydrophobically modified rice husk fiber resin is evenly coated on the surface of the urea, and dry for 24 hours after the coating is completed; add the coated dry particles into a coating machine, wet the particle surface with atomized linseed oil, add molten composite super absorbent resin for coating five times, so that the composite super absorbent resin is evenly coated on the particle surface, and dry for 48 hours after the coating is completed to obtain a water-absorbing and water-retaining double-layer coated film controlled-release fertilizer with a particle size of 3mm.
[0041] Example 3
[0042] (1) Preparation of microbial agents:
[0043] Bacillus subtilis and Bacillus licheniformis were cultured in a liquid seed culture medium at 30°C for 24 hours, respectively, and then inoculated into LB culture medium at a 10% inoculation rate, respectively, and cultured under shaking at 30°C until the bacterial concentration reached OD600≈3.0, and then mixed evenly at a mass ratio of 1:1, and freeze-dried into freeze-dried powder to obtain a microbial agent;
[0044] (2) Preparation of epoxy-hydrophobically modified rice husk fiber resin:
[0045] 40 g of rice husk was washed and impurities were removed, and then ventilated and dried until the moisture content was less than 5%, crushed and ground, passed through a 200-mesh sieve, soaked in 1.5% hydrochloric acid for 24 hours, filtered and added to a reaction container, and 2 times the volume of distilled water was added, heated and stirred at 53° C. for 30 minutes, and 10 g of epoxy resin, 30 g of rosin, and 2 g of diisopropylaminoethyl methacrylate were added in sequence, and a sodium hydroxide solution with a mass concentration of 1 mol / L was added to adjust the pH to 10, heated and stirred at 110° C. for 2 hours, and a hydrochloric acid solution with a mass fraction of 1.5% was used to adjust the pH to neutral, heated and stirred at 80° C. until the solution was viscous, dried and crushed, and passed through a 100-mesh sieve to obtain an epoxy-hydrophobically modified rice husk fiber resin;
[0046] (3) Preparation of composite super absorbent resin:
[0047] Add 30g corncob powder and 15g bentonite into a reactor, add 3 times the volume of distilled water, stir at 85°C for 30min, add 3g maleic anhydride, stir at 40°C for 15min, add 18g acrylic acid and 5g palm kernel oil diethanolamide in sequence, heat and stir at 40°C for 2h, add 10g sodium alginate, 3g potassium persulfate, and 8g N,N-methylenebisacrylamide in sequence, heat and stir at 70°C for 2h, dry and crush through a 100-mesh sieve to obtain a composite super absorbent resin;
[0048] (4) Encapsulation
[0049] Add 80g of urea into a coating machine, spray atomized water to evenly moisten the urea, add molten epoxy hydrophobically modified rice husk fiber resin for coating three times, so that the epoxy hydrophobically modified rice husk fiber resin is evenly coated on the surface of the urea, and dry for 24 hours after the coating is completed; add the coated dry particles into a coating machine, moisten the particle surface with atomized linseed oil, add molten composite super absorbent resin for coating five times, so that the composite super absorbent resin is evenly coated on the particle surface, and dry for 48 hours after the coating is completed to obtain a water-absorbing and water-retaining double-layer coated film controlled-release fertilizer with a particle size of 5 mm.
[0050] Comparative Example 1
[0051] Compared with Example 1, in this comparative example, diisopropylaminoethyl methacrylate and rosin were not added during the preparation of the epoxy-hydrophobically modified rice husk fiber resin, and the rest of the operation process was exactly the same as that of Example 1.
[0052] Comparative Example 2
[0053] Compared with Example 1, in this comparative example, acrylic acid and potassium persulfate were not added during the preparation of the composite super absorbent resin, and the rest of the operation process was exactly the same as that of Example 1.
[0054] Comparative Example 3
[0055] Compared with Example 1, in this comparative example, maleic anhydride and sodium alginate were not added during the preparation of the composite super absorbent resin, and the rest of the operation process was exactly the same as that of Example 1.
[0056] Comparative Example 4
[0057] Compared with Example 1, in this comparative example, no palm kernel oil diethanolamide and N,N-methylenebisacrylamide were added during the preparation of the composite super absorbent resin, and the rest of the operation process was exactly the same as that of Example 1.
[0058] Comparative Example 5
[0059] The commercially available sulfur-coated urea (total nitrogen content ≥ 26%) produced by Shandong Zhongwo International Fertilizer Co., Ltd. is a urea-coated fertilizer commonly found on the market.
[0060] Detection experiment
[0061] 30 g of each of the coated urea controlled-release fertilizers prepared in Examples 1-3 and Comparative Examples 1-5 were taken to test the properties of each coated urea controlled-release fertilizer in terms of controlled-release period, water absorption, water retention, annual biodegradation, and mechanical strength.
[0062] The controlled release period test was carried out according to the national standard "Slow-release Fertilizer" (GB / T 23348-2009) to test the fertilizer 24-hour release rate, 7-day cumulative release rate, 28-day cumulative release rate, and 80% release time of fertilizer; the fertilizer water absorption was tested by the nylon mesh bag method to calculate the value of the mass change before and after water absorption saturation (g / g); the soil column method was used to determine the effect of fertilizer on the infiltration amount at the same infiltration distance, and the infiltration amount was based on the height of the water level drop in the Malchnitz flask (cm); the annual biodegradability was tested by the soil burial method to determine the mass loss rate (%) after one year of burial; the mechanical strength test was tested by a fertilizer particle strength tester (sensitivity 0.1N) to test the pressure that the fertilizer particles could withstand when crushed; the specific test results are shown in Table 1:
[0063] Table 1 Performance test table
[0064]
[0065]
[0066] According to the test results, the water-absorbing and water-retaining double-layer coated urea slow-release fertilizer prepared in Examples 1-3 of the present invention significantly improves the slow-release performance of urea. The average release time of 80% of the fertilizer nutrients in 25°C static water is 43 days, which is better than the commercially available sulfur-coated urea. The initial nutrient release rate is 8% after immersion in 5°C static water for 24 hours, and the cumulative nutrient release rate is 52% after 28 days. According to the national standard "Slow-release Fertilizer" (GB / T 23348-2009) stipulates that the initial nutrient release rate of slow-release fertilizers should be less than 15% after being immersed in static water at 25°C for 24 hours, and the cumulative nutrient release rate should be less than 80% after 28 days, which meets the national standard; the double-layer coated urea slow-release fertilizer of the present invention can absorb 5-6 times the weight of the fertilizer itself, and has excellent water retention effect, which is significantly better than the control group; the coating film prepared from a large amount of rice husks and corn cob powder used can be decomposed by microbial agents, with an annual degradation rate of nearly 90%, which is green and environmentally friendly; and the fertilizer has high compressive strength and can withstand a pressure of 30-35N, with excellent performance and high urea nutrient utilization rate.
[0067] Field experiment
[0068] The urea coated fertilizers prepared in Examples 1-3 and Comparative Examples 1-5 of the present invention were used in 40 mu of land at Shuofengxuan Family Farm in Linzhang Line, Luozhuang District, Linyi City. The 40 mu of land on the farm was divided into 8 plots, each with 5 mu, all used to plant corn (corn seeds were purchased from Chongqing Jinde Seed Co., Ltd. - Jinnuo No. 1). The coated urea slow-release fertilizers prepared in Examples 1-3 and Comparative Examples 1-5 were applied to the 8 plots of land at a rate of 35 kg per mu. During spring sowing, the fertilizers were applied together, once a year, with a time interval between seeds and fertilizers. The distance between the fertilizers was 6-8 cm to avoid burning the seeds. The nutrients of phosphorus fertilizer and potash fertilizer were supplemented by applying 30 kg of potassium dihydrogen phosphate (purchased from Shandong Xinborui Biotechnology Co., Ltd., KH2PO4 content ≥ 98%) per mu. The 8 test fields in this experiment used urea-coated slow-release fertilizers prepared in Examples 1-3 and Comparative Examples 1-5 of the present invention, except for the nitrogen fertilizers used, and the other field management was exactly the same, all of which were daily field management. After harvest, the fullness of the grains, per mu yield, insect pests, and plant and seedling deaths were counted, and the results are shown in Table 2:
[0069] Table 2 Corn growth and harvest
[0070]
[0071] By comparing the experimental results, the water-absorbing and water-retaining double-layer coated urea controlled-release fertilizer prepared by the present invention in Examples 1-3 is compared with Comparative Examples 1-5, and the utilization rate of urea fertilizer effect is higher, the grains are fuller, and the microbial agents and pesticides are introduced in the process of coating film preparation to enhance the antibacterial and insect pest effects of each seedling. The thousand-grain weight, per-acre yield, insect pests and seedling mortality of corn cultivated in the field in Examples 1-3 are better than the application effects of the coated urea in the commercially available Comparative Example 5, the number of rotten and dead seedlings is significantly reduced, and the yield is significantly improved. According to statistical results, the water-absorbing and water-retaining double-layer coated urea controlled-release fertilizer prepared by Examples 1-3 of the present invention is applied, and the average per-acre yield of corn is 773 kg. Compared with the application effect of the coated urea in Comparative Example 5, the per-acre yield is increased by 19.2%, and the fertilizer effect is better.
[0072] It should be noted that the above embodiments are only partial embodiments of the preferred methods of implementing the present invention, rather than all embodiments. Obviously, based on the above embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
Claims
1. A water-absorbing and water-retaining double-layer coating slow-release fertilizer, with 60-80 parts of urea as the inner core, 10-15 parts of epoxy-hydrophobically modified rice husk fiber resin as the inner coating, and a composite superabsorbent resin prepared from 20-30 parts of corn cob powder, 12-15 parts of bentonite, 8-10 parts of sodium alginate, 13-18 parts of acrylic acid, 5-8 parts of accelerator, 10-12 parts of linseed oil, 2-5 parts of initiator, 3-8 parts of cross-linking agent, 3-5 parts of solubilizer, and 6-8 parts of microbial agent as the outer coating; The preparation method of the epoxy-hydrophobically modified rice husk fiber resin is as follows: 40-60 parts by weight of rice husk are washed and impurity-removed, dried to a water content of less than 5%, crushed and ground, passed through a 200-mesh sieve, soaked in 1.5% hydrochloric acid for 24 hours, filtered and added to a reaction container, 2-3 times the volume of distilled water are added, heated and stirred at 53-68° C. for 30 minutes, 10-20 parts by weight of epoxy resin, 15-30 parts by weight of rosin, and 2-5 parts by weight of diisopropylaminoethyl methacrylate are added in sequence, the pH is adjusted to 8-10 with a sodium hydroxide solution with a mass concentration of 1 mol / L, heated and stirred at 110-150° C. for 2-5 hours, the pH is adjusted to neutral with a hydrochloric acid solution with a mass fraction of 1.5%, heated and stirred at 80-85° C. until the solution is viscous, dried and crushed to obtain the epoxy-hydrophobically modified rice husk fiber resin; The preparation method of the composite super absorbent resin is as follows: add corn cob powder and bentonite into a reaction kettle, add 3-5 times the volume of distilled water, stir at 85°C for 30-45min, add a solubilizer, stir at 40-45°C for 15-20min, add acrylic acid and an accelerator in sequence, heat and stir at 40-60°C for 2-3h, add sodium alginate, an initiator, and a cross-linking agent in sequence, heat and stir at 70-90°C for 2-3h, dry, crush, and sieve, add a microbial agent, and obtain a composite super absorbent resin; the accelerator is palm kernel oil diethanolamide, the initiator is potassium persulfate, the cross-linking agent is N,N-methylenebisacrylamide, and the solubilizer is maleic anhydride; The microbial agent is a mixture of Bacillus subtilis and Bacillus licheniformis in a culture solution mass ratio of 1:1; the preparation method of the microbial agent is: Bacillus subtilis and Bacillus licheniformis are cultured in a liquid seed culture medium at 30°C for 24 hours respectively, and then inoculated into LB culture medium at a 10% inoculation rate respectively, and cultured at 30°C with shaking until the bacterial concentration is OD600≈3.0, and then mixed evenly in a culture solution mass ratio of 1:1, and freeze-dried into freeze-dried powder to obtain the microbial agent.
2. A method for preparing the water-absorbing and water-retaining double-layer coated slow-release fertilizer according to claim 1, comprising the following steps: Add urea to the coating machine, spray atomized water to evenly wet the urea, add molten epoxy hydrophobically modified rice husk fiber resin for coating in 3-5 times, so that the epoxy hydrophobically modified rice husk fiber resin is evenly coated on the surface of the urea, and dry for 24-48 hours after the coating is completed; add the coated dry particles to the coating machine, wet the particle surface with atomized linseed oil, add molten composite super absorbent resin for coating in 3-5 times, so that the composite super absorbent resin is evenly coated on the particle surface, and dry for 24-48 hours after the coating is completed to obtain a water-absorbing and water-retaining double-layer coated film slow-release fertilizer with a particle size of 3-5 mm.
Citation Information
Patent Citations
A method for preparing a multifunctional composite water-retaining slow-release fertilizer
CN107162747B
Slow-release material taking traditional Chinese medicine waste as raw material, slow-release fertilizer and preparation method thereof
CN112645754A