A method for preparing a titanium-containing high-efficiency catalyst and its application in polyester synthesis

By preparing gel or solid catalysts by blending tetravalent titanium compounds and ethylene glycol hydroxy acids, the problems of easy hydrolysis and poor stability of titanium catalysts are solved, realizing efficient and stable polyester synthesis, which is suitable for the preparation of high-performance polyesters.

CN117659370BActive Publication Date: 2026-11-17SUZHOU UNIV +1
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202311505929.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-13
Publication Date
2026-11-17
Estimated Expiration
2043-11-13

AI Technical Summary

Technical Problem

Existing titanium-based catalysts are prone to hydrolysis, have poor stability, and produce many side reactions, making them difficult to promote and apply on a large scale. Furthermore, existing modification methods are complex and costly, making it difficult to prepare efficient and green polyester catalysts.

Method used

By blending tetravalent titanium compounds, ethylene glycol, and hydroxy acids, gel or solid titanium-containing high-efficiency catalysts can be prepared, simplifying the preparation process, increasing titanium content and catalytic activity, avoiding hydrolysis, and facilitating storage and transportation.

Benefits of technology

The prepared catalyst has high catalytic activity, fast polymerization rate, good color value and high molecular weight of polyester products, is easy to store and transport, reduces costs, and is suitable for the synthesis of high-performance polyesters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117659370B_ABST
    Figure CN117659370B_ABST
Patent Text Reader

Abstract

This invention relates to a titanium-containing high-efficiency catalyst, its preparation method, and its application in polyester synthesis, belonging to the field of catalyst preparation technology. This invention provides a titanium-containing high-efficiency catalyst comprising a tetravalent titanium compound, ethylene glycol, and a hydroxy acid. It is in a gel or solid state at room temperature, exhibits stable performance, does not hydrolyze, and is easy to store, transport, and use. The titanium content in the catalyst is 3wt%–12wt%. This invention obtains the titanium-containing high-efficiency catalyst by blending a tetravalent titanium compound, a hydroxy acid, and ethylene glycol. The preparation process is simple, resulting in high titanium content and high catalytic activity. Using the catalyst of this invention to synthesize polyester results in a fast reaction rate, short reaction time, high intrinsic viscosity, and good color value in the obtained polyester.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of catalyst preparation technology, specifically relating to a titanium-containing high-efficiency catalyst, its preparation method, and its application in polyester synthesis. Background Technology

[0002] Polyesters based on diacid glycols as monomers are a class of high-performance polymers with wide applications in production and daily life, including polyethylene terephthalate (PET) and poly(butylene terephthalate-co-butylene adipate) (PBAT). These polyesters are generally synthesized by condensation polymerization from corresponding diacids or their dimethyl ester derivatives and diols. Catalysts are required during the synthesis process to promote molecular weight growth. Currently, antimony, germanium, and titanium catalysts are commonly used, such as antimony trioxide, germanium dioxide, and tetrabutyl titanate. Antimony-based catalysts are the most widely used; for example, over 90% of aromatic polyester PET is produced using antimony-based catalysts. Antimony-based catalysts have advantages such as low cost and good stability, but also disadvantages such as low catalytic activity, physiological toxicity, grayish polyester products, and antimony being a heavy metal. Germanium-based catalysts have the advantage of good product color value, but are expensive and are currently often used in the preparation of high-end polyesters. In contrast, titanium-based catalysts are a green and environmentally friendly option for polyester production. These are primarily titanate catalysts, such as tetrabutyl titanate, tetraisobutyl titanate, and tetraisopropyl titanate. They exhibit high catalytic activity, require only small amounts, and leave a residue in polyester that is only a fraction of that of antimony. However, when using them to catalyze polyester production, numerous side reactions occur, resulting in poor product color. Furthermore, titanate catalysts are typically liquids, readily reacting with water to form titanium dioxide, which precipitates from the system. They also exhibit poor hydrolysis resistance, are difficult to store for extended periods, and are unsuitable for large-scale polyester synthesis. Therefore, addressing the issues of easy hydrolysis, poor stability, and numerous side reactions associated with titanium-based catalysts is crucial for their large-scale promotion and also addresses the current urgent industrial demand for green polyester products.

[0003] The modification processes for titanium-based catalysts can be broadly categorized into four types: compounding, hydrolysis, loading, and stabilization.

[0004] US Patent 7767612 discloses a method for preparing a novel titanium-based catalyst by compounding titanate with antimony compounds to reduce the use of heavy metals and for catalytic synthesis of polyesters with superior performance, suitable for processing into spun products and films. However, this catalyst still requires the use of the heavy metal antimony and is not a green catalyst.

[0005] Chinese patent CN115353614A discloses a modification method for preparing antimony-free polyester catalysts by compounding tetrabutyl titanate and zinc oxide as raw materials. Although the compound catalyst prepared by this method can be used to synthesize polyesters with good color values, the preparation method is relatively complex, and the final catalyst is a liquid with a low titanium content (<5%).

[0006] Chinese patent CN200410019331 discloses a method for preparing supported titanium dioxide catalysts by dissolving titanium metal compounds in anhydrous ethanol to prepare an impregnation solution, followed by mixing with a treated support, hydrolysis, drying, and calcination. However, titanium dioxide is a heterogeneous catalyst and tends to accumulate at the bottom of the reaction vessel, causing problems such as pipeline blockage and inconsistent product color.

[0007] Chinese patent CN103709383A discloses a method for preparing supported titanium catalysts using nano-silica as a support and titanium glycolate as a titanium source. This method improves the catalyst's resistance to hydrolysis, but polyester products still suffer from heterogeneous catalysis, easy pipeline blockage, numerous side reactions, and poor color values.

[0008] US Patent 20050148758A1 discloses a stable aqueous titanium-based catalyst comprising an organotitanium and zinc complex. This catalyst exhibits good catalytic activity, is environmentally friendly, does not easily clog the discharge orifice, and produces polyesters with good color. However, the catalyst solution containing titanium and zinc can only be stored stably at 60°C for about two weeks, exhibiting poor storage stability, making it difficult to transport, and its effective content is low, requiring large addition amounts during use.

[0009] Therefore, there is a need to develop a green polyester catalyst that is stable, not easily hydrolyzed, has high catalytic activity, high titanium content, low cost, and is easy to transport and store. Summary of the Invention

[0010] To address the aforementioned technical problems, this invention provides a titanium-containing high-efficiency catalyst, its preparation method, and its application in polyester synthesis. This invention obtains the titanium-containing high-efficiency catalyst by blending a tetravalent titanium compound, a hydroxy acid, and ethylene glycol. The titanium-containing high-efficiency catalyst of this invention is in gel or solid form, has a simple preparation process, high titanium content, high catalytic activity, stable performance, does not hydrolyze, and is easy to store, transport, and use. Using the catalyst of this invention to synthesize polyester results in a fast reaction rate, short reaction time, high intrinsic viscosity, and good color value in the obtained polyester.

[0011] This invention is achieved through the following technical solution:

[0012] The first objective of this invention is to provide a titanium-containing high-efficiency catalyst, wherein the catalyst comprises a tetravalent titanium compound, ethylene glycol and a hydroxy acid, and is in a gel or solid state at room temperature; the titanium content in the catalyst is 3wt% to 12wt%.

[0013] The second objective of this invention is to provide a method for preparing the aforementioned titanium-containing high-efficiency catalyst, comprising the following steps:

[0014] The tetravalent titanium compound, ethylene glycol, and hydroxy acid were mixed under stirring at room temperature and allowed to stand to obtain the titanium-containing high-efficiency catalyst.

[0015] In one embodiment of the present invention, the tetravalent titanium compound is a titanate; the titanate is selected from one or more of tetrabutyl titanate, tetraisobutyl titanate and tetraisopropyl titanate; the mass ratio of the tetravalent titanium compound to ethylene glycol is 12:1 to 1:5, preferably 10:1 to 2:1.

[0016] In one embodiment of the present invention, the hydroxy acid is selected from one or more of lactic acid, glycolic acid and 3-hydroxypropionic acid; the molar ratio of the tetravalent titanium compound to the hydroxy acid is 2:1 to 1:5, preferably 1:1 to 1:3.

[0017] In one embodiment of the present invention, the titanium-containing high-efficiency catalyst exhibits stable catalytic performance, and its performance remains unchanged after being placed at room temperature for one year.

[0018] A third objective of this invention is to provide the application of the aforementioned titanium-containing high-efficiency catalyst in polyester synthesis.

[0019] In one embodiment of the present invention, the polyester is one or more of polyethylene terephthalate, polyethylene terephthalate, polyethylene butylene terephthalate, polyethylene adipate, and polyethylene tridecanoate; the catalytic efficiency of the titanium-containing high-efficiency catalyst is higher than that of tetrabutyl titanate, and the titanium content in the titanium-containing high-efficiency catalyst is reduced by 20% to 60% when synthesizing polyester samples in the same time, and the synthesis time of the polyester is reduced by 20% to 30% under the same titanium feed amount.

[0020] In one embodiment of the present invention, the amount of titanium-containing high-efficiency catalyst added is 6ppm to 15ppm, preferably 8ppm to 12ppm.

[0021] In one embodiment of the present invention, the molecular weight of the polyester is 40,000 g / mol to 80,000 g / mol.

[0022] In one embodiment of the present invention, the synthesis temperature is 180°C to 300°C.

[0023] In existing technologies, modifying titanium compounds to adjust their activity typically requires neutralization, filtration, distillation, and other processes, making the preparation process cumbersome, energy-intensive, and time-consuming. Some patents require the use of highly volatile organic compounds, which does not align with the development concept of "green and environmentally friendly." Furthermore, the resulting catalysts are often in solution form, with low titanium content, and are prone to reacting with moisture in the air to form precipitates. This necessitates large addition amounts, relatively slow polymerization rates, and the reaction process is prone to side reactions that lead to color variations, making it difficult to apply to the preparation of high-value-added polyesters.

[0024] In this invention, a titanium-containing high-efficiency catalyst is obtained by reacting a tetravalent titanium compound, ethylene glycol, and a hydroxy acid, stirring until homogeneous, and then cooling and allowing to stand. This preparation method is simple, low-cost, requires no other solvents or post-treatment, and has a short preparation time. The catalyst prepared by this invention is in gel or solid form, exhibits stable performance, does not hydrolyze, is easy to store and transport, has a high titanium content, and exhibits high catalytic activity. It requires only a small amount to be added during use and can be used to prepare high-performance polyester films and bottle flakes, among other materials.

[0025] In one embodiment of the present invention, a diacid or its dimethyl ester derivative, a diol, and a titanium-containing high-efficiency catalyst are mixed and then subjected to an esterification reaction at a reaction temperature of 180°C to 250°C and a reaction pressure of 0 to 0.5 MPa; or a diacid or its dimethyl ester derivative is mixed with a diol and then subjected to an esterification reaction first, followed by the addition of a titanium-containing high-efficiency catalyst; then a polycondensation reaction is carried out under vacuum conditions at 250°C to 300°C and a reaction pressure of less than 200 Pa to obtain polyethylene terephthalate (PET) or poly(butylene terephthalate-copolymer-butylene adipate) ester (PBAT).

[0026] Based on the mass of the catalyst and its titanium content, the amount of titanium added in the synthesized polyesters such as polyethylene terephthalate (PET) and poly(butylene terephthalate-co-butylene adipate) (PBAT) can be calculated to be 6 ppm to 15 ppm. Preferably, the amount of titanium added is 8 ppm to 12 ppm.

[0027] In one embodiment of the present invention, musk T, decanediol and titanium-containing high-efficiency catalyst are mixed and subjected to ring-opening-condensation cascade polymerization reaction at a reaction temperature of 180℃~250℃ under nitrogen protection or vacuum conditions for 0.5h~3h to obtain poly(1,13-tridecanoic acid ethylene glycol-copoly-1,10-decanediol) ester (PEDB).

[0028] Based on the total mass of musk T and decanediol, the amount of titanium added to the titanium-containing high-efficiency catalyst is 6 ppm to 15 ppm. Preferably, the amount of titanium added is 8 ppm to 12 ppm.

[0029] The technical solution of the present invention has the following advantages compared with the prior art:

[0030] 1. The preparation method of the titanium-containing high-efficiency catalyst of the present invention uses ethylene glycol as a raw material. Ethylene glycol is one of the commonly used raw materials in the synthesis of polyester and will not introduce excess components into the synthesis of polyester. It does not require the use of other low-boiling-point, highly volatile organic solvents, making it a green and environmentally friendly preparation method.

[0031] 2. The preparation method of the titanium-containing high-efficiency catalyst of the present invention can obtain the titanium-containing high-efficiency catalyst by simply and conveniently mixing and settling. The preparation process is short and energy-efficient.

[0032] 3. The titanium-containing high-efficiency catalyst prepared by this invention is in gel or solid form, which is easy to store and transport;

[0033] 4. The titanium-containing high-efficiency catalyst prepared by this invention has a high titanium content, and the amount added during polyester synthesis is low, which can save costs;

[0034] 5. The titanium-containing high-efficiency catalyst prepared by the present invention has high catalytic efficiency, fast polymerization speed, can effectively reduce polymerization time, suppress side reactions, and the obtained polyester product has good color value and high molecular weight.

[0035] 6. The titanium-containing high-efficiency catalyst prepared by the present invention has good hydrolysis resistance. It does not deteriorate after being placed at room temperature for one year, and its catalytic efficiency is consistent with that of the newly prepared catalyst. Attached Figure Description

[0036] To make the content of this invention easier to understand, the invention will be further described in detail below with reference to specific embodiments and accompanying drawings, wherein...

[0037] Figure 1 The image shows the morphology of the high-efficiency catalyst solid (T-1) from Example 1.

[0038] Figure 2 The images show the morphology of the high-efficiency catalyst solid (T-2) from Example 2 and its morphology after one year of storage.

[0039] Figure 3 The image shows the morphology of the high-efficiency catalyst gel (T-3) in Example 3.

[0040] Figure 4 Here is the size exclusion chromatogram of PEDB in Example 10 (solvent: chloroform, concentration: 1 mg / mL);

[0041] Figure 5 Here is the size exclusion chromatogram of PEDB in Example 11 (solvent: chloroform, concentration: 1 mg / mL);

[0042] Figure 6 Here is the size exclusion chromatogram of PEDB in Example 12 (solvent: chloroform, concentration: 1 mg / mL);

[0043] Figure 7 Here is the size exclusion chromatogram of PEDB in Example 13 (solvent: chloroform, concentration: 1 mg / mL);

[0044] Figure 8 Here is the size exclusion chromatogram of PEDB in Example 14 (solvent: chloroform, concentration: 1 mg / mL);

[0045] Figure 9 Size exclusion chromatogram of PEDB in Example 15 (solvent: chloroform, concentration: 1 mg / mL);

[0046] Figure 10 Here is the size exclusion chromatogram of PBAT in Example 16 (solvent: chloroform, concentration: 1 mg / mL);

[0047] Figure 11 This is a diagram showing the precipitation of ethylene glycol and tetrabutyl titanate in control example 1.

[0048] Figure 12 The size exclusion chromatogram of PEDB (solvent: chloroform, concentration: 1 mg / mL) is shown in control example 3. Detailed Implementation

[0049] The present invention will be further described below with reference to the accompanying drawings and specific embodiments, so that those skilled in the art can better understand and implement the present invention. However, the embodiments described are not intended to limit the present invention.

[0050] Unless otherwise specified, the experimental methods used in the following examples are conventional methods, and the materials and reagents used are commercially available. PET polyester was tested according to GB / T14190-2017.

[0051] The CAS numbers of the organic reagents used in this invention are listed below:

[0052] Table 1

[0053]

[0054]

[0055] Example 1

[0056] 0.79 g of ethylene glycol (EG), 9.00 g of tetrabutyl titanate (TNBT), and 2.38 g of lactic acid (LA) were added to a 50 mL single-necked flask and stirred at room temperature for 1 min. After the reaction was complete, the mixture was allowed to stand at room temperature for 5 min to obtain a highly efficient catalyst solid (T-1) with a titanium content of 10.4%; its morphology is shown in the figure below. Figure 1 As shown.

[0057] Example 2

[0058] Ethylene glycol (EG) 0.79 g, tetrabutyl titanate (TNBT) 9.00 g, and lactic acid (LA) 7.14 g were added to a 50 mL single-necked flask and stirred at room temperature for 1 min. After the reaction was complete, the mixture was allowed to stand at room temperature for 5 min to obtain a highly efficient catalyst solid (T-2) with a titanium content of 7.48%. Its morphology and morphology after one year of storage are shown in the figure below. Figure 2 As shown.

[0059] Example 3

[0060] 16.20 g of ethylene glycol (EG), 9.00 g of tetrabutyl titanate (TNBT), and 7.14 g of lactic acid (LA) were added to a 50 mL single-necked flask and stirred at room temperature for 1 min. After the reaction was complete, the mixture was allowed to stand at room temperature for 5 min to obtain a highly efficient catalyst gel (T-3) with a titanium content of 3.91%; its morphology is shown in the figure below. Figure 3 As shown.

[0061] Example 4

[0062] 1.60 g of ethylene glycol (EG), 6.80 g of tetrabutyl titanate (TNBT), and 1.52 g of glycolic acid (GA) were added to a 50 mL single-necked flask and stirred at room temperature for 1 min. After the reaction was completed, the mixture was allowed to stand at room temperature for 5 min to obtain a high-efficiency catalyst solid (T-4) with a titanium content of 9.50%.

[0063] Example 5

[0064] 0.81 g of ethylene glycol (EG), 3.70 g of tetrabutyl titanate (TNBT), and 1.03 g of 3-hydroxypropionic acid (3-HPA) were added to a 50 mL single-necked flask and stirred at room temperature for 1 min. After the reaction was completed, the mixture was allowed to stand at room temperature for 5 min to obtain a high-efficiency catalyst solid (T-5) with a titanium content of 9.30%.

[0065] Example 6

[0066] 2.00 g of ethylene glycol (EG), 11.36 g of tetraisopropyl titanate (TIPT), and 3.60 g of lactic acid (LA) were added to a 50 mL single-necked flask and stirred at room temperature for 1 min. After the reaction was completed, the mixture was allowed to stand at room temperature for 5 min to obtain a high-efficiency catalyst solid (T-6) with a titanium content of 11.2%.

[0067] Example 7

[0068] 0.36 g of ethylene glycol (EG), 1.36 g of tetraisobutyl titanate (TOBT), and 0.36 g of lactic acid (LA) were added to a 50 mL single-necked flask and stirred at room temperature for 1 min. After the reaction was completed, the mixture was allowed to stand at room temperature for 5 min to obtain a high-efficiency catalyst solid (T-7) with a titanium content of 9.15%.

[0069] Example 8

[0070] Add 2000g of terephthalic acid (PTA), 896mL of ethylene glycol (EG), 0.12g of triphenyl phosphate (TPP), and 0.2g of the high-efficiency catalyst (T-1) from Example 1 to a polyester reactor. The esterification reaction was carried out for 120min at 200kPa and the temperature was gradually increased from 180℃ to 235℃. After the excess ethylene glycol was distilled off, vacuum was applied and the temperature was increased to 278℃ for polycondensation reaction for 120min. The reaction was stopped when the stirring power reached the preset value. The product was discharged and sliced ​​to obtain polyethylene terephthalate (PET).

[0071] The polyester chips have a carboxyl content of 6.22 mol / t, an intrinsic viscosity of 0.60 dL / g, a melting point of 252.9℃, a glass transition temperature of 80.2℃, an L value of 84.9, an a value of -1.2, and a b value of 2.4.

[0072] Example 9

[0073] Add 2000g of terephthalic acid (PTA), 896mL of ethylene glycol (EG), 0.12g of triphenyl phosphate (TPP), and 0.4g of the high-efficiency catalyst (T-3) from Example 3 to a polyester reactor. The esterification reaction was carried out for 130min at 200kPa and the temperature was gradually increased from 180℃ to 235℃. After the excess ethylene glycol was distilled off, vacuum pressure was applied and the temperature was increased to 278℃ for polycondensation reaction for 150min. The reaction was stopped when the stirring power reached the preset value. The product was discharged and sliced ​​to obtain polyethylene terephthalate (PET).

[0074] The polyester chips have an end carboxyl content of 4.27 mol / t, an intrinsic viscosity of 0.60 dL / g, a melting point of 251.9℃, a glass transition temperature of 79.5℃, an L value of 85.4, an a value of -0.9, and a b value of 1.9.

[0075] Example 10

[0076] 13.6 g of musk T(EB), 0.87 g of decanediol, and 3.2 mg of the high-efficiency catalyst (T-1) from Example 1 were added to a 250 mL single-necked flask. The mixture was heated until completely dissolved, and reacted at 220 °C for 180 min under nitrogen protection. After the reaction was complete, the mixture was cooled to room temperature to obtain poly(1,13-tridecanoic acid ethylene glycol-copoly-decanediol) ester (PEDB). The size exclusion chromatogram is shown below. Figure 4 The number-average molecular weight was measured to be 67,700 g / mol.

[0077] Example 11

[0078] 13.6 g of musk T(EB), 0.87 g of decanediol, and 3.2 mg of the high-efficiency catalyst (T-2) from Example 2 were added to a 250 mL single-necked flask. The mixture was heated until completely dissolved, and reacted at 220 °C for 180 min under nitrogen protection. After the reaction was complete, the mixture was cooled to room temperature to obtain poly(1,13-tridecanoic acid ethylene glycol-copoly-decanediol) ester (PEDB). The size exclusion chromatogram is shown below. Figure 5 The number-average molecular weight was measured to be 60600 g / mol.

[0079] Example 12

[0080] 13.6 g of musk T(EB), 0.87 g of decanediol, and 3.2 mg of the high-efficiency catalyst (T-4) from Example 4 were added to a 250 mL single-necked flask. The mixture was heated until completely dissolved, and reacted at 220 °C for 180 min under nitrogen protection. After the reaction was complete, the mixture was cooled to room temperature to obtain poly(1,13-tridecanoic acid ethylene glycol-copoly-decanoic acid) ester (PEDB). The size exclusion chromatogram is shown below. Figure 6 The number-average molecular weight was measured to be 57200 g / mol.

[0081] Example 13

[0082] 13.6 g of musk T(EB), 0.87 g of decanediol, and 3.5 mg of the high-efficiency catalyst (T-5) from Example 5 were added to a 250 mL single-necked flask. The mixture was heated until completely dissolved, and reacted at 220 °C for 180 min under nitrogen protection. After the reaction was complete, the mixture was cooled to room temperature to obtain poly(1,13-tridecanoic acid ethylene glycol-copoly-decanediol) ester (PEDB). The size exclusion chromatogram is shown below. Figure 7 The number-average molecular weight was measured to be 49200 g / mol.

[0083] Example 14

[0084] 13.6 g of musk T(EB), 0.87 g of decanediol, and 3.5 mg of the high-efficiency catalyst (T-6) from Example 6 were added to a 250 mL single-necked flask. The mixture was heated until completely dissolved, and reacted at 220 °C for 180 min under nitrogen protection. After the reaction was complete, the mixture was cooled to room temperature to obtain poly(1,13-tridecanoic acid ethylene glycol-copoly-decanediol) ester (PEDB). The size exclusion chromatogram is shown below. Figure 8 The number-average molecular weight was measured to be 42800 g / mol.

[0085] Example 15

[0086] 13.6 g of musk T(EB), 0.87 g of decanediol, and 3.5 mg of the high-efficiency catalyst (T-7) from Example 7 were added to a 250 mL single-necked flask. The mixture was heated until completely dissolved, and reacted at 220 °C for 180 min under nitrogen protection. After the reaction was complete, the mixture was cooled to room temperature to obtain poly(1,13-tridecanoic acid ethylene glycol-copoly-decanediol) ester (PEDB). The size exclusion chromatogram is shown below. Figure 9 The number-average molecular weight was measured to be 41400 g / mol.

[0087] Example 16

[0088] 19.4 g of dimethyl terephthalate (DMT), 14.6 g of adipic acid (AA), 23.4 g of 1,4-butanediol (BDO), and 5 mg of the high-efficiency catalyst (T-1) from Example 1 were added to a 250 mL single-necked flask. Esterification was carried out at 185 °C for 90 min, then the temperature was increased to 220 °C and the esterification was continued for another 30 min. Esterification was terminated when the water output reached 90% of the theoretical value. Vacuum was then introduced to reduce the pressure, and the temperature was increased to 260 °C for a polycondensation reaction for 180 min. After the reaction, the product was cooled and discharged to obtain poly(terephthalic acid-copoly-butylene adipate) ester (PBAT). The size exclusion chromatogram is shown below. Figure 10 The number-average molecular weight was measured to be 43700 g / mol.

[0089] Compare with Example 1

[0090] 0.79 g of ethylene glycol (EG) and 9.00 g of tetrabutyl titanate (TNBT) were added to a 50 mL single-necked flask and stirred at room temperature for 1 min. After the reaction was completed and allowed to stand at room temperature, tetrabutyl titanate formed a white precipitate at the bottom of the flask, indicating that it could not form a homogeneous and stable catalyst. (Details are as follows...) Figure 11 As shown.

[0091] Compare with Example 2

[0092] 2000g of terephthalic acid (PTA), 896mL of ethylene glycol (EG), 0.12g of triphenyl phosphate (TPP), and 0.34g of titanium-based catalyst (brand name 638) from CTL Corporation (UK) were added to a polyester reactor. The esterification reaction was carried out for 135min at 200kPa and the temperature was gradually increased from 180℃ to 235℃. After the excess ethylene glycol was distilled off, the pressure was reduced by vacuuming, and the temperature was increased to 278℃ for polycondensation reaction for 155min. The reaction was stopped when the stirring power reached the preset value. The product was discharged and sliced ​​to obtain polyethylene terephthalate (PET).

[0093] The polyester chips have a carboxyl content of 5.18 mol / t, an intrinsic viscosity of 0.60 dL / g, a melting point of 251.0℃, a glass transition temperature of 78.3℃, an L value of 61.0, an a value of -2.4, and a b value of 3.9.

[0094] Compare with Example 3

[0095] 13.6 g of musk T(EB), 0.87 g of decanediol, and 3.2 mg of tetrabutyl titanate (14% titanium content, higher than other highly efficient catalysts at the same dosage) were added to a 250 mL single-necked flask. The mixture was heated until completely dissolved, and reacted at 220 °C for 180 min under nitrogen protection. After the reaction was complete, the mixture was cooled to room temperature to obtain poly(1,13-tridecanoic acid ethylene glycol-copoly-decanediol) ester (PEDB). The size exclusion chromatogram is shown below. Figure 12 The number-average molecular weight was measured to be 34900 g / mol.

[0096] Obviously, the above embodiments are merely illustrative examples for clear explanation and are not intended to limit the implementation. Those skilled in the art will recognize that other variations or modifications can be made based on the above description. It is neither necessary nor possible to exhaustively list all possible implementations here. However, obvious variations or modifications derived therefrom are still within the scope of protection of this invention.

Claims

1. A titanium-containing high-efficiency catalyst, characterized in that, The catalyst comprises a tetravalent titanium compound, ethylene glycol, and a hydroxy acid, and is in a gel or solid state at room temperature; the titanium content in the titanium-containing high-efficiency catalyst is 3 wt% to 12 wt%. The preparation method of the titanium-containing high-efficiency catalyst includes the following steps: The tetravalent titanium compound, ethylene glycol and hydroxy acid were mixed under stirring at room temperature and allowed to stand to obtain the titanium-containing high-efficiency catalyst. The hydroxy acid is selected from one or more of lactic acid, glycolic acid, and 3-hydroxypropionic acid; the molar ratio of the tetravalent titanium compound to the hydroxy acid is 2:1 to 1:

5. The tetravalent titanium compound is a titanate; the titanate is selected from one or more of tetrabutyl titanate, tetraisobutyl titanate, and tetraisopropyl titanate; the mass ratio of the tetravalent titanium compound to ethylene glycol is 12:1 to 1:

5.

2. The titanium-containing high-efficiency catalyst according to claim 1, characterized in that, The titanium-containing high-efficiency catalyst exhibits stable catalytic performance, and its performance remains unchanged after being placed at room temperature for one year.

3. The application of the titanium-containing high-efficiency catalyst according to claim 1 in polyester synthesis.

4. The application of the titanium-containing high-efficiency catalyst according to claim 3 in polyester synthesis, characterized in that, The polyester is one or more of polyethylene terephthalate, polyethylene terephthalate, polyethylene butylene terephthalate, polyethylene adipate, and polyethylene tridecanoate.

5. The application of the titanium-containing high-efficiency catalyst according to claim 3 in polyester synthesis, characterized in that, The amount of titanium-containing high-efficiency catalyst added is 6 ppm to 15 ppm.

6. The application of the titanium-containing high-efficiency catalyst according to claim 3 in polyester synthesis, characterized in that, The molecular weight of the polyester is 40,000 g / mol to 80,000 g / mol.

7. The application of the titanium-containing high-efficiency catalyst according to claim 3 in polyester synthesis, characterized in that, The synthesis temperature is 180 ℃~300 ℃.

Citation Information

Patent Citations

  • Titanium-based polyester catalyst as well as preparation method and application thereof

    CN103709383A

  • Composite catalyst, preparation method thereof and application of composite catalyst in antimony-free polyester synthesis

    CN115353614A

  • Preparing method for loaded titania catalyst of ester interchange synthetic phenyl ester oxalate

    CN1255210C

  • Stable aqueous solutions comprising titanium and zinc and process therewith

    US20050148758A1

  • Esterification catalyst, polyester process and polyester article

    US7767612B2