A pressure-sensitive adhesive for power battery and a method for manufacturing the same

By introducing modified inorganic particles and alkylene polyether ether ketone and other materials into acrylic pressure-sensitive adhesive, the problem of insufficient high temperature resistance and flame retardancy of acrylic pressure-sensitive adhesive has been solved, and its high temperature resistance and flame retardancy have been significantly improved. performance and enhanced safety of power batteries.

CN117659914BActive Publication Date: 2024-10-01东莞市欣美电子材料有限公司
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202311682233.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-08
Publication Date
2024-10-01
Estimated Expiration
2043-12-08

AI Technical Summary

Technical Problem

Existing acrylic pressure-sensitive adhesives have poor high-temperature resistance and flame-retardant properties, which may cause degradation and loss of viscosity under the high-temperature conditions of power batteries, causing safety hazards and risks of spontaneous combustion.

Method used

By preparing acrylate pressure-sensitive adhesive containing modified inorganic particles, using materials such as alkylene polyether ether ketone and boron nitride for cross-linking and flame retardant coating, the bonding strength and flame retardant properties are improved, and the high temperature resistance is enhanced .

Benefits of technology

Significantly improves the high temperature resistance and flame retardant properties of pressure-sensitive adhesives, extends the service life at high temperatures, enhances the safety of power batteries, and avoids the risk of spontaneous combustion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117659914B_ABST
    Figure CN117659914B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of adhesive technology, and discloses a pressure-sensitive adhesive for power batteries and a method for manufacturing the same. The pressure-sensitive adhesive is prepared by using acrylic pressure-sensitive adhesive liquid, modified inorganic particles and curing agent aziridine as raw materials through a mixing process. The cross-linked acrylic structure with polyetheretherketone as the core is formed by preparing olefinated polyetheretherketone as a copolymer and in-situ polymerization with other acrylic monomers. The cross-linked acrylic structure is used as the main raw material of the pressure-sensitive adhesive, which can improve the bonding strength and high temperature resistance of the pressure-sensitive adhesive. In addition, by grafting a flame retardant coating layer on the surface of nano-boron nitride to prepare modified inorganic particles, and mixing them with acrylic pressure-sensitive adhesive liquid, the flame retardant performance of the pressure-sensitive adhesive can be enhanced, thereby making the power battery safer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of adhesives, and in particular to a pressure-sensitive adhesive used in power batteries and a method for manufacturing the same. Background Art

[0002] In recent years, vigorously developing new energy vehicles to replace traditional fuel vehicles is an important means to achieve sustainable development, and has gradually become the mainstream of the automotive industry. The power battery pack of new energy vehicles is formed by assembling individual batteries, and pressure-sensitive adhesives are needed to bond and fix the batteries. Since pressure-sensitive adhesives are relatively simple to construct and have strong viscosity, they are often used in the production of power batteries. Since power batteries generate heat during the charging and discharging process, pressure-sensitive adhesives need to work at relatively high temperatures for a long time. Moreover, a large proportion of safety accidents involving power batteries are caused by spontaneous combustion of batteries. Therefore, pressure-sensitive adhesives used in power batteries should have good high temperature resistance and flame retardant properties to avoid degradation and loss of adhesion of pressure-sensitive adhesives under high temperature conditions, causing safety hazards, and rapid spontaneous combustion of power batteries, which poses a huge threat to the life safety of users.

[0003] At present, the commonly used type of pressure-sensitive adhesive on the market is acrylate pressure-sensitive adhesive, but the high temperature resistance and flame retardant properties of acrylate pressure-sensitive adhesive are poor, and there are still major defects in practical applications. The invention patent with application number CN202210792497.X discloses a phosphorus-containing monomer and a cyclic monomer grafted modified acrylate pressure-sensitive adhesive and a high-performance flame-retardant pressure-sensitive adhesive prepared therefrom. Through the graft copolymerization process, phosphorus-containing monomers and cyclic monomers are introduced at the same time to prepare a modified acrylate pressure-sensitive adhesive with good basic flame retardant effect. Therefore, the comprehensive properties of acrylate pressure-sensitive adhesives such as flame retardancy can be enhanced by optimizing the structure of acrylate.

[0004] Based on this, the present invention provides an acrylic pressure-sensitive adhesive, which has good high temperature resistance and flame retardancy and can be directly applied to power batteries. Summary of the invention

[0005] The purpose of the present invention is to provide a pressure-sensitive adhesive for use in power batteries and a method for manufacturing the same, which solves the problem of poor high temperature resistance and flame retardancy of acrylic pressure-sensitive adhesives.

[0006] The purpose of the present invention can be achieved by the following technical solutions:

[0007] A pressure-sensitive adhesive for power batteries, comprising the following raw materials by weight: 70-85 parts of acrylic pressure-sensitive adhesive liquid, 6-8.5 parts of modified inorganic particles, and 10-20 parts of curing agent aziridine;

[0008] The preparation method of the acrylic pressure-sensitive adhesive comprises the following steps:

[0009] Step 1: Pour olefinated polyetheretherketone and N,N-dimethylformamide into a reaction kettle, stir until a uniform solution is formed, then add butyl acrylate, methyl methacrylate and acrylic acid, pass nitrogen protection, stir at a temperature of 75-80°C for 20-40 minutes to form a monomer reaction solution;

[0010] Step 2: Add azobisisobutyronitrile to the monomer reaction solution, raise the temperature of the reactor to 85-90°C, stir and react for 3-6 hours, and discharge the material after it is naturally cooled to obtain an acrylic pressure-sensitive adhesive solution;

[0011] The modified inorganic particles are nano boron nitride with a flame retardant coating layer grafted on the surface.

[0012] Furthermore, in step 1, the preparation method of the olefinated polyetheretherketone is as follows:

[0013] The polyetheretherketone and N,N-dimethylacetamide are stirred and mixed evenly, nitrogen is introduced for deoxygenation, chloroethyl isocyanate and tin tetrachloride are added, and after the addition is completed, hydroxyethyl methacrylate and an organic tin catalyst are added and mixed evenly at 60-65°C, and the mixture is kept warm and stirred for 12-18 hours. The temperature is raised to 70-75°C, and the mixture is kept warm and stirred for 4-6 hours. The mixture is poured into ethanol for precipitation, and the solid material is separated to obtain olefinated polyetheretherketone.

[0014] Furthermore, the molecular weight of the polyetheretherketone is 4000.

[0015] Furthermore, the organic tin catalyst is any one of stannous octoate or dibutyltin dilaurate.

[0016] By adopting the above technical scheme, under the action of tin tetrachloride, polyetheretherketone can undergo Friedel-Crafts alkylation reaction with chloroethyl isocyanate, thereby introducing isocyanate groups into the polyetheretherketone structure. Under the action of an organic tin catalyst, the isocyanate groups can undergo amine esterification reaction with the hydroxyl groups in the hydroxyethyl methacrylate structure, thereby introducing unsaturated olefinic functional groups into the polyetheretherketone structure to obtain olefinic polyetheretherketone.

[0017] Furthermore, the preparation method of the modified inorganic particles comprises the following steps:

[0018] Step ①: Mix hydroxylated boron nitride and 1,4-dioxane to form a uniform dispersion, add 3-isopropyl-dimethylbenzyl isocyanate to the dispersion, pass nitrogen protection, keep warm at 80-90°C for 6-12h, and centrifuge to separate the solid material to obtain a boron nitride intermediate;

[0019] Step ②: Mix and disperse the boron nitride intermediate and N,N-dimethylformamide, add phosphorus-containing monomers, raise the system temperature to 90-100°C under nitrogen protection, keep warm and stir for 12-16 hours, discharge the material, centrifuge the solid product, wash and vacuum dry it, and obtain modified inorganic particles.

[0020] Furthermore, in step ①, the preparation method of the hydroxylated boron nitride is specifically as follows: after ultrasonically mixing boron nitride with 30% hydrogen peroxide by mass for 20-40 minutes, stirring at 80-85°C for 1-2 hours, heating to 90-95°C, stirring for 4-6 hours, cooling to 80-85°C, keeping warm for 8-12 hours, discharging, filtering out the solid, washing and vacuum drying.

[0021] Furthermore, the average particle size of the boron nitride is 50 nm.

[0022] Furthermore, in step ①, the mass ratio of the hydroxylated boron nitride to 3-isopropyl-dimethylbenzyl isocyanate is 1:0.4-0.5.

[0023] Furthermore, in step ②, the phosphorus-containing monomer is any one of dimethyl phosphite, diethyl phosphite or dibenzyl phosphite.

[0024] By adopting the above technical scheme, after the boron nitride is oxidized with hydrogen peroxide, the surface of the boron nitride is rich in hydroxyl groups, which can undergo an amine esterification reaction with the isocyanate group in the structure of 3-isopropyl-dimethylbenzyl isocyanate, thereby modifying the unsaturated olefinic functional group on the surface of the boron nitride to obtain a boron nitride intermediate. Under high temperature conditions, the unsaturated olefinic group can undergo an addition reaction with the PH bond in the phosphorus-containing monomer structure, thereby modifying the nitrogen-phosphorus synergistic flame retardant coating on the surface of the boron nitride to obtain modified inorganic particles.

[0025] A method for manufacturing a pressure-sensitive adhesive for a power battery is specifically as follows:

[0026] Step 1: Accurately weigh 70-85 parts of acrylic pressure-sensitive adhesive, 6-8.5 parts of modified inorganic particles and 10-20 parts of curing agent aziridine, and set aside;

[0027] Step 2: Pour the acrylic pressure-sensitive adhesive liquid and modified inorganic particles into a planetary mixer, set the speed to 500-1000r / min, stir for 30-60min, add the curing agent aziridine, continue stirring for 2-4h, and then discharge the material to obtain the pressure-sensitive adhesive.

[0028] Beneficial effects of the present invention:

[0029] 1) The present invention prepares olefinated polyetheretherketone as a copolymer, and in-situ polymerizes it with other acrylic monomers to form a cross-linked acrylic ester structure with polyetheretherketone as the core, and uses it as the main raw material of the pressure-sensitive adhesive, which can effectively improve the cross-linking density of the pressure-sensitive adhesive after curing, which is not only conducive to improving the bonding strength of the pressure-sensitive adhesive, but also can enhance the high temperature resistance of the pressure-sensitive adhesive by inhibiting the movement of the molecular chain. In addition, the polyetheretherketone structure contains a large number of rigid benzene ring structures, which can show excellent high temperature resistance, thereby further improving the high temperature resistance of the pressure-sensitive adhesive by optimizing the structure of the molecular chain.

[0030] 2) The present invention prepares modified inorganic particles by grafting a flame retardant coating layer on the surface of nano boron nitride, and mixes the particles with acrylic pressure-sensitive adhesive as fillers. Since the coating layer is an organic substance, it is equivalent to forming an organic bonding layer on the surface of boron nitride, which can effectively inhibit the agglomeration of boron nitride in acrylic pressure-sensitive adhesive, promote its uniform dispersion, and then form a heat conduction path in the pressure-sensitive adhesive to achieve heat conduction, which is conducive to heat dissipation, thereby ensuring the service life of the pressure-sensitive adhesive at high temperatures. In addition, the nitrogen-phosphorus synergistic flame retardant in the flame retardant coating layer can effectively enhance the flame retardant properties of the pressure-sensitive adhesive and avoid violent combustion, thereby making the power battery safer.

[0031] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0033] Figure 1 This is the infrared characterization diagram of the olefinated polyetheretherketone prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0034] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0035] Example 1

[0036] 1. Preparation of olefinated polyetheretherketone

[0037] 1.2 g of polyetheretherketone with a molecular weight of 4000 and N,N-dimethylacetamide were stirred and mixed evenly, nitrogen was introduced for deoxygenation, 1.5 g of chloroethyl isocyanate and 1.5 g of tin tetrachloride were added, and after the addition was completed, 2 g of hydroxyethyl methacrylate and 0.01 g of dibutyltin dilaurate were added and mixed evenly, the temperature was raised to 75 ° C, and after stirring for 5 hours, the mixture was poured into ethanol for precipitation, and the solid material was separated to obtain olefinated polyetheretherketone.

[0038] The olefinated polyetheretherketone was characterized by infrared, and the test results were as follows: Figure 1 As shown, analysis shows that 3267cm -1 NH stretching vibration peak in the amide group, 3000-3100 cm -1 The peak of CH stretching vibration in benzene ring and carbon-carbon double bond is 1748 cm -1 is the C=O stretching vibration peak in the ketone carbonyl group, 1652 cm -1 It is the C=O stretching vibration peak in the amide group.

[0039] 2. Preparation of modified inorganic particles

[0040] Step ①: Ultrasonic mix 5g of boron nitride with an average particle size of 50nm and 30% hydrogen peroxide with a mass fraction for 30min, stir at 80℃ for 2h, heat to 90℃, stir for 6h, cool to 80℃, keep warm for 9h, discharge, filter out the solid, wash and vacuum dry.

[0041] Step ②: 1.8 g of hydroxylated boron nitride was mixed with 1,4-dioxane to form a uniform dispersion, and 0.8 g of 3-isopropyl-dimethylbenzyl isocyanate was added to the dispersion. After the addition was completed, nitrogen was passed through the dispersion, and the mixture was kept at 85° C. for 8 h, and then the solid material was separated by centrifugation to obtain a boron nitride intermediate.

[0042] 0.2g of boron nitride intermediate was dispersed in chloroform as a sample, and then 15mL of Wei's solution was added and stirred. After standing in the dark for 1h, 10mL of 15% potassium iodide solution and 80mL of purified water were added and mixed. The sample was titrated quickly with 0.1M sodium thiosulfate standard solution. The titration was stopped after the dispersion changed color. 1mL of 1% starch was added as an indicator and titrated until the dispersion color disappeared. The volume of the standard solution used (mL) was recorded. A blank experiment was performed and the volume of the standard solution used (mL) was recorded. The unsaturated value of the sample was calculated using the formula [(V1-V)×0.1] / 0.2. The result was 0.518 mmol / g.

[0043] Step ③: Mix and disperse 1g of the boron nitride intermediate with N,N-dimethylformamide, add 0.8g of diethyl phosphite, and under nitrogen protection, raise the system temperature to 95°C. After stirring for 12 hours, discharge the material, centrifuge the solid product, wash and vacuum dry it, and obtain modified inorganic particles.

[0044] The method is the same as step ②. The unsaturation value of 0.2g modified inorganic particles is tested again, and the result is 0.105mmol / g. This is because the addition reaction of diethyl phosphite and boron nitride intermediates results in a large consumption of alkenyl functional groups, resulting in a decrease in the unsaturation value.

[0045] 3. Preparation of acrylic pressure-sensitive adhesive

[0046] Step 1: Pour 2.5g of olefinated polyetheretherketone and N,N-dimethylformamide into a reaction kettle, stir until a uniform solution is formed, then add 15g of butyl acrylate, 1g of methyl methacrylate, and 0.5g of acrylic acid, pass nitrogen protection, and stir at a temperature of 80°C for 30min to form a monomer reaction solution;

[0047] Step 2: Add 0.1 g of azobisisobutyronitrile to the monomer reaction solution. After the addition is completed, raise the temperature of the reactor to 90° C., stir and react for 4 hours, and after the material is naturally cooled, discharge the material to obtain an acrylic pressure-sensitive adhesive solution.

[0048] 4. Preparation of pressure-sensitive adhesive

[0049] Step 1: Accurately weigh 70 parts of acrylic pressure-sensitive adhesive, 6 parts of modified inorganic particles and 10 parts of curing agent aziridine for later use;

[0050] Step 2: Pour the acrylic pressure-sensitive adhesive liquid and modified inorganic particles into a planetary mixer, set the speed to 500r / min, stir for 60 minutes, add the curing agent aziridine, continue stirring for 4 hours, and then discharge the material to obtain the pressure-sensitive adhesive.

[0051] Example 2

[0052] Preparation of pressure sensitive adhesive

[0053] Step 1: Accurately weigh 80 parts of acrylic pressure-sensitive adhesive, 8 parts of modified inorganic particles and 16 parts of curing agent aziridine for later use;

[0054] Step 2: Pour the acrylic pressure-sensitive adhesive liquid and modified inorganic particles into a planetary mixer, set the speed to 800r / min, stir for 40 minutes, add the curing agent aziridine, continue stirring for 3 hours, and then discharge the material to obtain the pressure-sensitive adhesive.

[0055] The preparation method of the acrylic pressure-sensitive adhesive and the modified inorganic particles is the same as that in Example 1.

[0056] Example 3

[0057] Preparation of pressure sensitive adhesive

[0058] Step 1: Accurately weigh 85 parts of acrylic pressure-sensitive adhesive, 8.5 parts of modified inorganic particles and 20 parts of curing agent aziridine for later use;

[0059] Step 2: Pour the acrylic pressure-sensitive adhesive liquid and modified inorganic particles into a planetary mixer, set the speed to 1000r / min, stir for 30 minutes, add the curing agent aziridine, continue stirring for 2 hours, and then discharge the material to obtain the pressure-sensitive adhesive.

[0060] The preparation method of the acrylic pressure-sensitive adhesive and the modified inorganic particles is the same as that in Example 1.

[0061] Comparative Example 1

[0062] Preparation of pressure sensitive adhesive

[0063] Step 1: Accurately weigh 80 parts of acrylic pressure-sensitive adhesive, 8 parts of boron nitride and 16 parts of curing agent aziridine, and set aside;

[0064] Step 2: Pour the acrylic pressure-sensitive adhesive liquid and modified inorganic particles into a planetary mixer, set the speed to 800r / min, stir for 40 minutes, add the curing agent aziridine, continue stirring for 3 hours, and then discharge the material to obtain the pressure-sensitive adhesive.

[0065] The preparation method of the acrylic pressure-sensitive adhesive solution is the same as that in Example 1.

[0066] Comparative Example 2

[0067] Preparation of pressure sensitive adhesive

[0068] Step 1: Accurately weigh 80 parts of acrylic pressure-sensitive adhesive and 16 parts of curing agent aziridine and set aside;

[0069] Step 2: Pour the acrylic pressure-sensitive adhesive liquid and curing agent aziridine into a planetary mixer, set the speed to 800r / min, stir for 3 hours, and then discharge the material to obtain the pressure-sensitive adhesive.

[0070] The preparation method of the acrylic pressure-sensitive adhesive solution is the same as that in Example 1.

[0071] Comparative Example 3

[0072] 1. Preparation of acrylic pressure-sensitive adhesive

[0073] Step 1: Pour N,N-dimethylformamide, 15g butyl acrylate, 1g methyl methacrylate, and 0.5g acrylic acid into a reaction kettle, pass nitrogen protection, and stir at a temperature of 80°C for 30 minutes to form a monomer reaction solution;

[0074] Step 2: Add 0.1 g of azobisisobutyronitrile to the monomer reaction solution. After the addition is completed, raise the temperature of the reactor to 90° C., stir and react for 4 hours, and after the material is naturally cooled, discharge the material to obtain an acrylic pressure-sensitive adhesive solution.

[0075] 2. Preparation of pressure-sensitive adhesive

[0076] Step 1: Accurately weigh 80 parts of acrylic pressure-sensitive adhesive, 8 parts of modified inorganic particles and 16 parts of curing agent aziridine for later use;

[0077] Step 2: Pour the acrylic pressure-sensitive adhesive liquid and modified inorganic particles into a planetary mixer, set the speed to 800r / min, stir for 40 minutes, add the curing agent aziridine, continue stirring for 3 hours, and then discharge the material to obtain the pressure-sensitive adhesive.

[0078] The preparation method of the modified inorganic particles is the same as that in Example 1.

[0079] a) The pressure-sensitive adhesives prepared in Examples 1 to 3 and Comparative Examples 1 to 3 of the present invention were uniformly coated on one side of the PET film, the thickness of the coated dry adhesive was controlled to be 25 μm, and the samples were cured in an oven at 80° C. to prepare test samples, and the following performance tests were performed:

[0080] Refer to standard GB / T 2792-2014 for peel strength test;

[0081] The samples were placed in an oven at 120°C, taken out after 24 hours, and subjected to a peel strength test. The test results are recorded in the following table:

[0082]

[0083]

[0084] It can be seen from the test results in the above table that the pressure-sensitive adhesives prepared in Examples 1 to 3 of the present invention have excellent bonding properties, and after high-temperature treatment, the peel strength decreases less, so the high-temperature resistance is good.

[0085] The pressure-sensitive adhesive prepared in Comparative Example 1 uses unmodified boron nitride as filler, which may be partially agglomerated, affecting the bonding performance of the pressure-sensitive adhesive, and the high temperature resistance is also greatly affected.

[0086] No filler was added to the pressure-sensitive adhesive prepared in Comparative Example 2, and the bonding performance and high temperature resistance performance were acceptable.

[0087] The acrylic pressure-sensitive adhesive liquid used in the pressure-sensitive adhesive prepared in Comparative Example 3 does not contain polyetheretherketone, so the cross-linking density of the pressure-sensitive adhesive after curing is low, and the structure does not contain rigid benzene rings, so the bonding performance and high temperature resistance performance are poor.

[0088] b) The pressure-sensitive adhesives prepared in Examples 1 to 3 and Comparative Examples 1 to 3 of the present invention were poured into a mold and cured in an oven at 80° C. to prepare test specimens. The flame retardancy test was performed according to the standard GB / T 2408-2021. The test results are shown in the following table:

[0089]

[0090]

[0091] It can be seen from the above table that the pressure-sensitive adhesive to which modified inorganic particles are added can exhibit excellent flame retardant properties, while the pressure-sensitive adhesives prepared in Comparative Examples 1 and 2 do not use modified inorganic particles, and therefore have poor flame retardant properties.

[0092] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0093] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A pressure-sensitive adhesive for power batteries, characterized in that: The following raw materials are included by weight: 70-85 parts of acrylic pressure-sensitive adhesive, 6-10 parts of modified inorganic particles, and 10-20 parts of curing agent aziridine; The preparation method of the acrylic pressure-sensitive adhesive comprises the following steps: Step 1: Pour olefinated polyetheretherketone and N,N-dimethylformamide into a reaction kettle, stir until a uniform solution is formed, then add butyl acrylate, methyl methacrylate and acrylic acid, pass nitrogen protection, stir at a temperature of 75-80°C for 20-40 minutes to form a monomer reaction solution; Step 2: Add azobisisobutyronitrile to the monomer reaction solution, raise the temperature of the reactor to 85-90°C, stir and react for 3-6 hours, and discharge the material after it is naturally cooled to obtain an acrylic pressure-sensitive adhesive solution; The preparation method of the olefinated polyetheretherketone is as follows: The polyetheretherketone and N,N-dimethylacetamide are stirred and mixed evenly, nitrogen is introduced to deoxygenate, chloroethyl isocyanate and tin tetrachloride are added, and after the addition is completed, hydroxyethyl methacrylate and an organic tin catalyst are added and mixed evenly at 60-65°C, and the mixture is stirred at this temperature for 12-18 hours, and then the mixture is heated to 70-75°C, stirred at this temperature for 4-6 hours, and then poured into ethanol for precipitation, and the solid material is separated to obtain olefinated polyetheretherketone; The modified inorganic particles are nano boron nitride with a flame retardant coating layer grafted on the surface; The preparation method of the modified inorganic particles comprises the following steps: Step ①: Mix hydroxylated boron nitride and 1,4-dioxane to form a uniform dispersion, add 3-isopropyl-dimethylbenzyl isocyanate to the dispersion, pass nitrogen protection, keep warm at 80-90°C for 6-12h, and centrifuge to separate the solid material to obtain a boron nitride intermediate; Step ②: Mix and disperse the boron nitride intermediate and N,N-dimethylformamide, add phosphorus-containing monomers, raise the system temperature to 90-100°C under nitrogen protection, keep warm and stir for 12-16 hours, discharge the material, centrifuge the solid product, wash and vacuum dry it, and obtain modified inorganic particles.

2. A pressure-sensitive adhesive for power batteries according to claim 1, characterized in that: The molecular weight of the polyetheretherketone is 4000.

3. The pressure-sensitive adhesive for power batteries according to claim 1, characterized in that: The organic tin catalyst is any one of stannous octoate or dibutyltin dilaurate.

4. The pressure-sensitive adhesive for power batteries according to claim 1, characterized in that: In step ①, the preparation method of hydroxylated boron nitride is specifically as follows: after ultrasonically mixing boron nitride with 30% hydrogen peroxide by mass for 20-40 minutes, stirring at 80-85°C for 1-2 hours, heating to 90-95°C, stirring for 4-6 hours, cooling to 80-85°C, keeping warm for 8-12 hours, discharging, filtering out the solid, washing and vacuum drying.

5. The pressure-sensitive adhesive for power batteries according to claim 4, characterized in that: The average particle size of the boron nitride is 50 nm.

6. The pressure-sensitive adhesive for power batteries according to claim 1, characterized in that: In step ①, the mass ratio of the hydroxylated boron nitride to 3-isopropyl-dimethylbenzyl isocyanate is 1:0.4-0.

5.

7. The pressure-sensitive adhesive for power batteries according to claim 1, characterized in that: In step ②, the phosphorus-containing monomer is any one of dimethyl phosphite, diethyl phosphite or dibenzyl phosphite.

8. A method for manufacturing a pressure-sensitive adhesive for a power battery according to any one of claims 1 to 7, characterized in that: The manufacturing method is specifically as follows: Step 1: Accurately weigh 70-85 parts of acrylic pressure-sensitive adhesive, 6-8.5 parts of modified inorganic particles and 10-20 parts of curing agent aziridine, and set aside; Step 2: Pour the acrylic pressure-sensitive adhesive liquid and modified inorganic particles into a planetary mixer, set the speed to 500-1000r / min, stir for 30-60min, add the curing agent aziridine, continue stirring for 2-4h, and then discharge the material to obtain the pressure-sensitive adhesive.

Citation Information

Patent Citations

  • Fire-retarding hexagonal boron nitride / thermosetting resin composite material and preparation method thereof

    CN103059567A

  • Carboxyl-containing polyetheretherketone-modified acrylic water-based resin

    CN109337020A

  • EVA hot melt adhesive with high bonding strength

    CN110330901A

  • Polyetheretherketone photosensitive material as well as preparation method and application thereof

    CN111154050A

  • Insulating flame-retardant pressure-sensitive adhesive applied to power battery, adhesive tape and preparation method of insulating flame-retardant pressure-sensitive adhesive

    CN112126384A