Small punch test method for fracture toughness and ductile-brittle transition temperature of anisotropic materials
By setting a square groove and an arc-shaped punch on a small punch test device, single-stress extrusion is applied only to the impact zone of the sample, solving the testing problem of fracture toughness and ductile-brittle transition temperature of anisotropic materials, and realizing an efficient and low-cost testing method.
Patent Information
- Application Number
- CN202311526002.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-11-16
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-11-16
AI Technical Summary
Existing technologies are insufficient for testing the fracture toughness and ductile-brittle transition temperature of anisotropic materials, especially when the material size is too small to prepare standard specimens or when irradiation costs are too high, making standard small punch test methods ineffective.
A small punch test device was used. By setting two symmetrically distributed square grooves and arc-shaped punches on the specimen, the specimen was squeezed only in the impact zone, so that the specimen was subjected to only a single stress. The fracture energy and ductile-brittle transition temperature were calculated by combining the force-displacement curve.
It enables accurate testing of fracture toughness and ductile-brittle transition temperature of anisotropic materials under single stress conditions, simplifies the sample preparation process, and reduces irradiation costs.
Smart Images

Figure CN117664756B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of material performance testing technology, specifically to a small punch test method for the fracture toughness and ductile-brittle transition temperature of anisotropic materials. Background Technology
[0002] Fracture toughness and ductile-brittle transition temperature play a crucial role in structural design and structural integrity assessment. While these parameters can be measured using standard specimens, determining them becomes challenging when material sizes are too small to prepare standard specimens. Furthermore, for in-service equipment, large-area sampling for standard specimen preparation is not feasible. Additionally, for nuclear materials research, the high cost of irradiation necessitates the use of micro-sample testing methods whenever possible.
[0003] The small punch test uses a micro-sample. The standard small punch test typically uses a circular sample with a diameter of 10 mm and a thickness of 0.5 mm; alternatively, a circular sample with a diameter of 3 mm and a thickness of 0.25 mm can be used. The standard small punch test method is widely used for testing fracture toughness and the ductile-brittle transition temperature. However, because the sample used in the standard small punch test is subjected to dual stresses during the test, it becomes extremely difficult to study the fracture toughness and ductile-brittle transition temperature of anisotropic materials. Summary of the Invention
[0004] To address the technical problems existing in the prior art, the purpose of this invention is to provide a small punch test method for the fracture toughness and ductile-brittle transition temperature of anisotropic materials subjected to only a single stress.
[0005] To achieve the above objectives, the present invention adopts the following technical solution:
[0006] A small punch test method for the fracture toughness and ductile-brittle transition temperature of anisotropic materials includes the following steps:
[0007] S1: Multiple specimens are prepared in a certain direction of the test material. The specimens are notched or unnotched. The specimens have two symmetrically distributed square grooves, and the area between the two square grooves is the impact zone.
[0008] S2: Perform small-blower tests on multiple specimens using a small-blower testing device. The contact surface between the blower and the impact zone of the small-blower testing device is an arc surface. Record the data during the test, including the force applied by the blower to the specimen, the displacement of the blower, and the notch opening displacement of the notched specimen. The force-displacement curve is obtained by plotting the force applied to the specimen by the punch and the displacement of the punch.
[0009] S3: Calculate the fracture energy and fracture toughness of the specimen based on the data obtained in step S2 and the force-displacement curve;
[0010] S4: Repeat steps S2-S3 at different temperatures to obtain the fracture energy of the sample at different temperatures, and draw a fracture energy temperature diagram to obtain the ductile-brittle transition temperature of the tested material in this direction.
[0011] S5: Prepare multiple specimens of the same size in other directions of the test material, and repeat steps S2-S4 to obtain the fracture toughness and ductile-brittle transition temperature of the test material in different directions.
[0012] As a preferred embodiment, in step S2, the small punch test device includes an upper die, a lower die, and a punch. Both the upper die and the lower die are provided with guide grooves. The punch slides relative to the guide grooves. The upper die and the lower die are connected to clamp the sample.
[0013] As a preferred option, in step S3, the fracture energy of the specimen is obtained by calculating the shaded area of the force-displacement curve and the horizontal axis.
[0014] As a preferred option, in step S4, the fracture energy temperature diagram is obtained by curve fitting of the fracture energy of the sample at different temperatures. In the fracture energy temperature diagram, the straight line fitted to the curve transition region and the oblique line of the upper platform are extended to obtain the intersection point A. The temperature corresponding to point A is the ductile-brittle transition temperature of the tested material in this direction.
[0015] As a preferred option, in step S3, the method for calculating the fracture toughness of the notched specimen is as follows: first, obtain the maximum force based on the force-displacement curve. Then, the sample was subjected to a small punch test again until the force applied by the punch to the sample reached... Stop at this time; the notch opening displacement of the test specimen at this time is... Then, the fracture toughness of the tested sample material is calculated according to the formula:
[0016] (1),
[0017] In the formula and It is a material-related coefficient, determined by calibration based on the results of standard fracture toughness tests and small punch tests.
[0018] As a preferred option, in step S3, the method for calculating the fracture toughness of the unnotched specimen is as follows: based on the results of the small punch test, the equivalent fracture strain of the failed specimen is measured. The fracture toughness of the tested sample material is:
[0019] (3)
[0020] The parameters k and J0 in the formula are material-related coefficients, which are determined by calibration based on the results of standard fracture toughness tests and small punch tests.
[0021] In summary, the present invention has the following advantages:
[0022] The present invention sets two square grooves and a punch with an arc surface on the sample. The punch with the arc surface directly squeezes the impact zone between the two square grooves, so that the sample is subjected to only a single stress. Therefore, it is possible to test the fracture toughness and ductile-brittle transition temperature of anisotropic materials. Attached Figure Description
[0023] Figure 1 A schematic diagram of a quarter-inch punch test apparatus.
[0024] Figure 2 This is a schematic diagram of a notched sample with a diameter of 10 mm.
[0025] Figure 3 This is a schematic diagram of a 10mm diameter unnotched specimen.
[0026] Figure 4 This is a schematic diagram of the force distribution in the impact zone of a notched specimen.
[0027] Figure 5 This is a schematic diagram of the force distribution in the impact zone of an unnotched specimen.
[0028] Figure 6 This is a force-displacement curve.
[0029] Figure 7 This is a fracture energy temperature diagram.
[0030] Figure 8 The diagram shows the displacement measurement of the gap opening.
[0031] Figure 9 This is a schematic diagram of the test h after the impact zone of the specimen fractures.
[0032] Among them, 1 is the sample, 2 is the punch, 3 is the upper die, 4 is the arc surface, 5 is the lower die, 6 is the guide groove, 7 is the square groove, 8 is the impact zone, and 9 is the notch. Detailed Implementation
[0033] The present invention will now be described in further detail with reference to specific embodiments.
[0034] This embodiment provides a small punch test method for the fracture toughness and ductile-brittle transition temperature of anisotropic materials, including the following steps:
[0035] S1: Multiple specimens 1 of the same size are prepared in a certain direction of the material of test 1. Specimen 1 includes specimen 1 with notch 9 and specimen 1 without notch 9. Specimen 1 is provided with two symmetrically distributed square grooves 7, and the area between the two square grooves 7 is the impact zone 8.
[0036] S2: A small punch test is performed on multiple specimens 1 using a small punch test device. The contact surface between the punch and the impact zone 8 of the small punch test device is an arc surface 4. Data during the test is recorded, including the force applied by the punch to the specimen 1, the displacement of the punch, and the opening displacement of the notch 9 of the specimen 1 with the notch 9. The force-displacement curve was obtained by plotting the force applied to specimen 1 by the punch and the displacement of the punch.
[0037] S3: Calculate the fracture energy and fracture toughness of specimen 1 based on the data obtained in step S2 and the force-displacement curve;
[0038] S4: Repeat steps S2-S3 at different temperatures to obtain the fracture energy of sample 1 at different temperatures, and draw the fracture energy temperature diagram to obtain the ductile-brittle transition temperature of the tested material in this direction.
[0039] S5: Prepare multiple specimens of the same size in other directions of the material of specimen 1, and repeat steps S2-S4 to obtain the fracture toughness and ductile-brittle transition temperature of the tested material in different directions.
[0040] In this embodiment, using Figure 1 The small punch test apparatus shown tests the fracture toughness and ductile-brittle transition temperature of anisotropic materials. The upper die 3 and lower die 5 are matched with the sample 1 to clamp it. The punch 2 with the arc surface 4 has a radius of 1 mm and a thickness of 2.6 mm. The upper die 3 has a guide groove 6 to facilitate the movement of the punch. The upper punch hole is a 2.6 mm × 2 mm square hole, and the lower punch hole is a 4 mm × 4 mm square hole. Figure 2 and Figure 3 The diagram shows two possible specimens 1 used in the test: specimen 1 with a notch 9 and specimen 1 without a notch 9. For specimen 1 with a notch 9, the diameter is 10 mm and the thickness is 0.5 mm. The notch 9 is located in the middle of specimen 1, with a radius of 0.14 mm and a depth of 0.15 mm. For specimen 1 without a notch 9, the diameter is 10 mm and the thickness is 0.5 mm. The impact zone 8 is the same for both types of specimen 1. The specific dimensions of specimen 1 and the notch 9 can differ.
[0041] Invention Principle: The deformation diagrams of the impact zone 8 of the notched (9) and unnotched (9) specimens after being subjected to force are shown. The specimen 1 is equipped with two square grooves 7 and a punch 2 with an arc surface 4. The punch 2 with the arc surface 4 directly compresses the impact zone 8 between the two square grooves 7. (See figure) Figure 4 and Figure 5 .from Figure 4 It can be seen that for specimen 1 with notch 9, triaxial stress exists in the region of notch 9. In areas farther from notch 9, due to the thinness of specimen 1, bending stress can be neglected according to thin film theory; therefore, specimen 1 is only subjected to a single stress. Thus, the stress state of specimen 1 is similar to that of the standard three-point bending impact specimen 1. Figure 5 For specimen 1 without a notch (9), specimen 1 is subjected to only a single stress in the impact zone (8). Therefore, for anisotropic materials, specimen 1 only measures the mechanical properties of the material in a certain direction, making this small punch test device suitable for testing the anisotropic mechanical properties of materials.
[0042] In step S2, the small punch testing device includes an upper die 3, a lower die 5, and a punch. Both the upper die 3 and the lower die 5 are provided with guide grooves 6. The punch slides relative to the guide grooves 6. The upper die 3 and the lower die 5 are connected to clamp the sample 1. The lower die 5 is fixedly installed on the small punch testing machine. The punch is connected to the drive shaft of the small punch testing machine. The upper die 3 can be connected to the lower die 5 by bolts and nuts.
[0043] like Figure 6 As shown, in step S3, the fracture energy of sample 1 is obtained by calculating the shaded area of the force-displacement curve and the horizontal axis.
[0044] like Figure 7 As shown, in step S4, see Figure 7 For each point in the curve, a curve fitting is performed on these points. That is, the fracture energy-temperature diagram is obtained by curve fitting the fracture energy of sample 1 at different temperatures. See the fracture energy-temperature diagram for details. Figure 7 The black curve in the figure is used to extend the straight line fitted to the curve transition region and the oblique line of the upper platform to obtain the intersection point A. The temperature corresponding to point A is the ductile-brittle transition temperature of the tested material in that direction.
[0045] For specimen 9 without a notch, a similar result can be obtained by performing a small punch test. Figure 4 and Figure 5 This allows us to determine the ductile-brittle transition temperature of the tested material.
[0046] like Figure 6 In step S3, the specific method for calculating the fracture toughness of specimen 1 with notch 9 is as follows: first, obtain the maximum force based on the force-displacement curve. Then, the small punch test was performed on sample 1 again until the force applied by the punch to sample 1 reached... Stop at time, such as Figure 8 The displacement of notch 9 in test specimen 1 at this time is... Then, the fracture toughness of the tested sample 1 material is calculated according to the formula: The formula for fracture toughness is:
[0047] (1)
[0048] In the formula and This is a material-related coefficient, determined by standard fracture toughness tests and small punch tests. Studies show that for P91, CrMoV, G20Mn5QT, and 20MnMoNi55 materials, if the friction coefficient between the test apparatus and sample 1 is 0.3, and... When the unit is mm, then N / mm 2 ,as well as N / mm.
[0049] In step S3, the specific method for calculating the fracture toughness of specimen 1 without notch 9 is as follows: Based on the results of the small punch test, the equivalent fracture strain of the failed specimen 1 is measured. The formula for calculating the equivalent fracture strain is as follows:
[0050] (2)
[0051] In the formula, h is the thickness of the impact zone 8 of specimen 1 at the time of fracture, and h0 is the initial thickness of specimen 1. h can be directly measured from the failed specimen 1; the test results are shown in [reference needed]. Figure 8 To ensure accurate measurement, the measurement should be repeated several times at different locations on the fracture surface, and the average value should be calculated.
[0052] The fracture toughness of the tested sample 1 material is:
[0053] (3)
[0054] In the formula, parameters k and J0 are material-related constants, determined by standard fracture toughness tests and small punch tests. In this embodiment, as... Figure 9 As shown, the thickness of specimen 1 after fracture failure can be directly measured on the failed specimen 1, unlike the standard small punch test, which requires first finding the minimum thickness of specimen 1 after fracture failure, then cutting it, and finally measuring the thickness of specimen 1 after fracture failure. Therefore, this method is simple and highly accurate in measuring the thickness of specimen 1 after fracture failure.
[0055] The above embodiments are preferred embodiments of the present invention, but the embodiments of the present invention are not limited to the above embodiments. Any changes, modifications, substitutions, combinations, or simplifications made without departing from the spirit and principle of the present invention shall be considered equivalent substitutions and shall be included within the protection scope of the present invention.
Claims
1. A small punch test method for the fracture toughness and ductile-brittle transition temperature of anisotropic materials, characterized in that, Includes the following steps: S1: Multiple specimens of the same size are prepared in a certain direction of the test material. The specimens are notched or unnotched. The specimens have two symmetrically distributed square grooves, and the area between the two square grooves is the impact zone. S2: Small punch tests were conducted on multiple specimens using a small punch testing device. The contact surface between the punch and the impact zone of the device was an arc surface. The arc-shaped punch directly compressed the impact zone between the two square slots, causing the specimen to be subjected to only a single stress. Data from the test process were recorded, including the force applied by the punch to the specimen, the displacement of the punch, and the notch opening displacement of the notched specimen. The force-displacement curve is obtained by plotting the force applied to the specimen by the punch and the displacement of the punch. S3: Calculate the fracture energy and fracture toughness of the specimen based on the data obtained in step S2 and the force-displacement curve; S4: Repeat steps S2-S3 at different temperatures to obtain the fracture energy of the sample at different temperatures, and draw a fracture energy temperature diagram to obtain the ductile-brittle transition temperature of the tested material in this direction. S5: Prepare multiple specimens of the same size in other directions of the test material, and repeat steps S2-S4 to obtain the fracture toughness and ductile-brittle transition temperature of the test material in different directions. In step S3, the specific method for calculating the fracture toughness of the notched specimen is as follows: first, obtain the maximum force based on the force-displacement curve. Then, the sample was subjected to a small punch test again until the force applied by the punch to the sample reached... Stop at this time; the notch opening displacement of the test specimen at this time is... Then, the fracture toughness of the tested sample material is calculated according to the formula: (1), In the formula and It is a material-related coefficient, determined by calibration based on the results of standard fracture toughness tests and small punch tests; In step S3, the specific method for calculating the fracture toughness of the unnotched specimen is as follows: based on the results of the small punch test, the equivalent fracture strain of the failed specimen is measured. The fracture toughness of the tested sample material is: (3) The parameters k and J0 in the formula are material-related coefficients, which are determined by calibration based on the results of standard fracture toughness tests and small punch tests.
2. The small punch test method for fracture toughness and ductile-brittle transition temperature of anisotropic materials according to claim 1, characterized in that: In step S2, the small punch test device includes an upper die, a lower die, and a punch. Both the upper die and the lower die are provided with guide grooves. The punch slides relative to the guide grooves. The upper die and the lower die are connected to clamp the sample.
3. The small punch test method for fracture toughness and ductile-brittle transition temperature of anisotropic materials according to claim 1, characterized in that: In step S4, the fracture energy temperature diagram is obtained by curve fitting of the fracture energy of the sample at different temperatures. In the fracture energy temperature diagram, the straight line fitted to the curve transition region and the oblique line of the upper platform are extended to obtain the intersection point A. The temperature corresponding to point A is the ductile-brittle transition temperature of the tested material in this direction.
Citation Information
Patent Citations
Method for testing circumferential tensile property of nuclear fuel cladding tube based on small punch test