Insulated gate bipolar transistor, manufacturing method thereof and electronic device

By designing oblique angle-shaped gate trenches and protective trenches in silicon carbide insulated gate bipolar transistors, and using a P+ doping layer, the problem of low reliability of silicon carbide insulated gate bipolar transistors in high-power scenarios is solved. , improving its breakdown resistance and stability.

CN117712155BActive Publication Date: 2024-10-01深圳平湖实验室
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311719807.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-13
Publication Date
2024-10-01
Estimated Expiration
2043-12-13

AI Technical Summary

Technical Problem

Silicon carbide insulated gate bipolar transistors are prone to breakdown in reliability in high-power scenarios, especially in reverse withstand voltage, short circuit and avalanche scenarios, where the insulating layer between the gate and channel region is prone to breakdown.

Method used

The gate trench and protective trench structure with an inclined angle shape are used, combined with the design of the P+ doped layer, to reduce the electric field intensity near the gate trench and improve the breakdown resistance of the insulating layer.

Benefits of technology

It effectively improves the reliability of the insulated gate bipolar transistor, reduces the risk of failure due to breakdown, and enhances its stability in high-voltage power applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117712155B_ABST
    Figure CN117712155B_ABST
Patent Text Reader

Abstract

The present invention discloses an insulated gate bipolar transistor, a manufacturing method thereof and an electronic device provided by an embodiment of the present invention, wherein the manufacturing material of the substrate includes P+ type silicon carbide, a buffer layer is arranged on the substrate, the manufacturing material of the buffer layer includes P-type silicon carbide, and a silicon carbide layer is arranged on the buffer layer; a gate groove is arranged in the silicon carbide layer, and protection grooves are respectively arranged on both sides of the gate groove, and a first P+ doping layer is arranged between each protection groove and the substrate, and the bottom of the protection groove is in contact with the corresponding first P+ doping layer. In this way, the protection groove and the first P+ doping layer can reduce the electric field strength near the gate groove, so that the insulated gate bipolar transistor is not easy to fail due to breakdown, thereby improving the reliability of the insulated gate bipolar transistor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor technology, and in particular to an insulated gate bipolar transistor, a manufacturing method thereof and an electronic device. Background Art

[0002] Silicon carbide insulated gate bipolar transistors have high reverse withstand voltage capability, high operating junction temperature, and excellent switching characteristics. They have great potential in high-voltage power electronics technology, such as high-voltage transmission, transformerless smart substations, and smart grid conversion.

[0003] However, since the operating power of SiC IGBT is relatively high, scenarios such as reverse withstand voltage, short circuit, and avalanche can easily cause the gate insulation layer between the gate and the channel region to be broken down, thereby reducing the reliability of SiC IGBT.

[0004] Therefore, how to improve the reliability of silicon carbide insulated gate bipolar transistors has become a technical problem that needs to be solved urgently in this field. Summary of the invention

[0005] The embodiment of the present invention provides an insulated gate bipolar transistor, a manufacturing method thereof and an electronic device, so as to improve the reliability of the silicon carbide insulated gate bipolar transistor.

[0006] In a first aspect, an embodiment of the present invention provides an insulated gate bipolar transistor, comprising: a substrate, and a buffer layer and a silicon carbide layer stacked in sequence on the substrate, wherein the substrate is made of P+ type silicon carbide, the buffer layer is made of P type silicon carbide, and the silicon carbide layer is made of N type silicon carbide;

[0007] A gate trench is provided in the silicon carbide layer, the gate trench has a sidewall, the sidewall includes a channel region, the sidewall has an inclination angle relative to the substrate surface, and the inclination angle makes the gate trench present a shape that is narrower on a side facing the substrate and wider on a side away from the substrate;

[0008] Protection trenches are respectively arranged on both sides of the gate trench, a first P+ doping layer is arranged between each of the protection trenches and the substrate, and the bottom of the protection trench is in contact with the corresponding first P+ doping layer.

[0009] In a second aspect, an embodiment of the present invention provides a method for manufacturing an insulated gate bipolar transistor as described in the first aspect, comprising:

[0010] Forming a buffer layer on a substrate, wherein the substrate is made of P+ silicon carbide, and the buffer layer is made of P silicon carbide;

[0011] forming a silicon carbide layer including a first P+ doped layer on the buffer layer, wherein the silicon carbide layer is made of N-type silicon carbide;

[0012] A gate trench and protection trenches on both sides of the gate trench are formed on the surface of the silicon carbide layer; the gate trench has a sidewall, the sidewall includes a channel region, and the sidewall has an inclination angle relative to the substrate surface, and the inclination angle makes the gate trench narrower on a side facing the substrate and wider on a side away from the substrate; the first P+ doped layer is located between each of the protection trenches and the substrate, and the bottom of the protection trench is in contact with the corresponding first P+ doped layer.

[0013] In a third aspect, an embodiment of the present invention provides an electronic device, including: an insulated gate bipolar transistor as described in the first aspect above.

[0014] The beneficial effects of the present invention are as follows:

[0015] An insulated gate bipolar transistor, a manufacturing method thereof and an electronic device provided by an embodiment of the present invention, wherein the manufacturing material of the substrate includes P+ type silicon carbide, a buffer layer is arranged on the substrate, the manufacturing material of the buffer layer includes P-type silicon carbide, and a silicon carbide layer is arranged on the buffer layer; a gate groove is arranged in the silicon carbide layer, and protection grooves are respectively arranged on both sides of the gate groove, and a first P+ doping layer is arranged between each protection groove and the substrate, and the bottom of the protection groove is in contact with the corresponding first P+ doping layer. In this way, the protection groove and the first P+ doping layer can reduce the electric field strength near the gate groove, so that the insulated gate bipolar transistor is not easy to fail due to breakdown, thereby improving the reliability of the insulated gate bipolar transistor. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 is a cross-sectional view of an insulated gate bipolar transistor provided in an embodiment of the present invention;

[0017] Figure 2 is a cross-sectional view of another insulated gate bipolar transistor provided in an embodiment of the present invention;

[0018] Figure 3 is a cross-sectional view of another insulated gate bipolar transistor provided in an embodiment of the present invention;

[0019] Figure 4 is a cross-sectional view of another insulated gate bipolar transistor provided in an embodiment of the present invention;

[0020] Figure 5 A cross-sectional view of a gate trench provided in an embodiment of the present invention;

[0021] Figure 6A schematic diagram of equivalent elements in an insulated gate bipolar transistor provided in an embodiment of the present invention;

[0022] Figure 7 A top view of an insulated gate bipolar transistor provided in an embodiment of the present invention;

[0023] Figure 8 A flow chart of a method for manufacturing an insulated gate bipolar transistor provided in an embodiment of the present invention;

[0024] Fig. 9 A schematic diagram of a partial manufacturing process of an insulated gate bipolar transistor provided in an embodiment of the present invention;

[0025] Fig.10 A schematic diagram of another part of the manufacturing process of an insulated gate bipolar transistor provided in an embodiment of the present invention;

[0026] Fig.11 The figure is a schematic diagram of the structure of an electronic device provided in an embodiment of the present invention. DETAILED DESCRIPTION

[0027] The following will be combined with the accompanying drawings to describe in detail the specific implementation of an insulated gate bipolar transistor, a method for manufacturing the same, and an electronic device provided by an embodiment of the present invention. It should be noted that the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] An embodiment of the present invention provides an insulated gate bipolar transistor, such as Figure 1 As shown, it includes: a substrate 13, and a buffer layer 12 and a silicon carbide layer 11 stacked on the substrate 13 in sequence, the substrate 13 is made of P+ type silicon carbide, the buffer layer 12 is made of P type silicon carbide, and the silicon carbide layer 11 is made of N type silicon carbide;

[0029] A gate trench 18 is provided in the silicon carbide layer 11. The gate trench 18 has a sidewall 15. The sidewall 15 includes a channel region ( Figure 1 The sidewall 15 has an inclination angle relative to the surface of the substrate 13, and the inclination angle makes the gate trench 18 narrower on the side facing the substrate 13 and wider on the side away from the substrate 13, that is, Figure 1 As shown in (b), the gate trench 18 is wide at the top and narrow at the bottom;

[0030] Protection trenches 9 are respectively disposed on both sides of the gate trench 18 . A first P+ doping layer 10 is disposed between each protection trench 9 and the substrate 13 , and the bottom of the protection trench 9 is in contact with the corresponding first P+ doping layer 10 .

[0031] The substrate may be a P+ heavily doped conductive substrate having a hexagonal crystal structure, and its doping concentration may be, but is not limited to, set to 1×10 19 / cm 3 The silicon carbide layer can be an intrinsic N-drift layer, which is a breakdown voltage holding layer of the insulated gate bipolar transistor. Its doping concentration can be, but is not limited to, set to 5×10 15 / cm 3 Up to 1×10 16 / cm 3 The doping concentration of the first P+ doping layer can be, but is not limited to, set to 1×10 18 / cm 3 Up to 1×10 19 / cm 3 .

[0032] In this way, when the insulated gate bipolar transistor is in the on state, the substrate injects holes into the silicon carbide layer, causing the insulated gate bipolar transistor to produce an injection enhancement effect, thereby reducing the on-state voltage drop and improving the performance of the insulated gate bipolar transistor; in addition, the protection trench and the first P+ doped layer can also reduce the electric field strength near the gate trench, making the insulated gate bipolar transistor less likely to fail due to breakdown, thereby improving the reliability of the insulated gate bipolar transistor.

[0033] The structures of the insulated gate bipolar transistor are introduced below.

[0034] 1. Gate trench.

[0035] Optionally, the sidewalls of the gate trench include: a first sidewall and a second sidewall opposite to each other, the first sidewall and the second sidewall both belong to the {0-33-8} crystal plane family or the {01-1-4} crystal plane family in the case of the hexagonal crystal system, and the inclination angle of the first sidewall relative to the substrate surface is different from the inclination angle of the second sidewall relative to the substrate surface.

[0036] Among them, Figure 1 As shown, the side wall on the right side of the gate trench 18 shown in the figure may be the first side wall 15a, and the side wall on the left side of the gate trench 18 shown in the figure may be the second side wall 15b; or, the side wall on the left side of the gate trench 18 shown in the figure may be the first side wall 15a, and the side wall on the right side of the gate trench 18 shown in the figure may be the second side wall 15b ( Figure 1 The first side wall 15a and the second side wall 15b may correspond to the same crystal plane family or different crystal plane families. In addition, the first side wall 15a is relative to the substrate surface (eg Figure 1 The inclination angle α1 of the surface indicated by the dotted line N in (b) is different from the inclination angle α2 of the second side wall 15b relative to the substrate surface (eg Figure 1 , as shown in (b) in the figure).

[0037] In this way, the first sidewall and the second sidewall both use the {0-33-8} crystal plane family or the {01-1-4} crystal plane family as channels, and both have higher carrier mobility, thereby improving the performance of the insulated gate bipolar transistor.

[0038] Alternatively, if Figure 5 As shown in (a), only the gate trench is shown in the figure, and the gate trench has a connecting side wall 15c, and the connecting side wall 15c is arranged between the first side wall 15a and the second side wall 15b. The angle between the connecting side wall 15c and the first side wall 15a, and the angle between the connecting side wall 15c and the second side wall 15b are both greater than 0°, and the width d1 of the connecting side wall 15c in the direction shown by F2 can be set to be no greater than 0.5μm, and the F2 direction can be understood as the arrangement direction of the gate trench and the protection trench. In this way, the gate insulating layer at the bottom of the gate trench of the insulated gate bipolar transistor will be subjected to smaller electric field stress when the reverse withstand voltage is applied, and the bottom gate insulating layer is not easily broken down and fails, thereby improving the reliability of the insulated gate bipolar transistor.

[0039] Or, if Figure 5 As shown in (b), only the gate trench is shown in the figure, and the gate trench may not be provided with a connecting sidewall 15c (that is, the width d1 of the connecting sidewall 15c in the direction indicated by F2 is set to 0), and the first sidewall 15a is directly connected to the second sidewall 15b. In this way, the channel density of the insulated gate bipolar transistor is higher, the current density is larger, and the performance of the insulated gate bipolar transistor will be better.

[0040] Optionally, the sidewalls of the gate trench include: a first sidewall and a second sidewall opposite to each other. In addition to being of the {0-33-8} crystal plane family or the {01-1-4} crystal plane family, the first sidewall and the second sidewall can also be set to: the first sidewall or the second sidewall belongs to the {11-20} crystal plane family in the case of a hexagonal crystal system.

[0041] Among them, Figure 3 As shown, when one sidewall is of the {11-20} crystal plane family, the other sidewall may be a vertical or nearly vertical sidewall. In this case, the morphology of the gate trench may be considered as a "U"-shaped trench with nearly vertical sidewalls.

[0042] Thus, one of the first sidewall and the second sidewall uses the {11-20} crystal plane family as a channel and also has a higher carrier mobility, thereby improving the performance of the insulated gate bipolar transistor.

[0043] Alternatively, if Figure 1 As shown, a gate insulating layer 6 is also disposed in the gate trench 18 , and the gate insulating layer 6 is used to isolate the gate 7 from the silicon carbide layer 11 .

[0044] 2. Protect the groove.

[0045] Alternatively, if Figure 2 As shown, a gate insulating layer 6 and a conductive material 8 are provided in the protection trench 9, and a through hole (such as Figure 2 In the embodiment shown in the dashed box Q2, the conductive material 8 is connected to the first P+ doped layer 10 through a through hole. The conductive material 8 may be, but is not limited to, grounded or used as a floating electrode. In this way, the first P+ doped layer 10 can be self-clamped by controlling the potential of the conductive material 8, which is beneficial to the protection of the gate trench by the first P+ doped layer 10 and improves the reliability of the insulated gate bipolar transistor.

[0046] It should be understood that in order to distinguish from the through holes in the electrode insulation layer described later, the through holes in the gate insulation layer can be referred to as first through holes, and the through holes in the electrode insulation layer described later can be referred to as second through holes. In the following text, the first through holes are used to represent the through holes in the gate insulation layer, and the second through holes are used to represent the through holes in the electrode insulation layer.

[0047] Alternatively, if Figure 4 As shown, the silicon carbide layer 11 is also provided with: along the direction from the substrate 13 to the buffer layer 12, as shown in Figure 4 In the F1 direction shown in FIG, the N-doped layer 17 and the second P+-doped layer 4 are sequentially stacked on the first P+-doped layer 10 ; the N-doped layer 17 and the second P+-doped layer 4 are both located on both sides of the protection trench 9 .

[0048] The N-doped layer 17 and the second P+ doped layer 4 on both sides of each protection trench 9 are in contact with the protection trench 9; the doping concentration of the N-doped layer 17 can be, but is not limited to, set to 1×10 16 / cm 3 Up to 1×10 17 / cm 3 The doping concentration of the second P+ doping layer 4 can be, but is not limited to, set to 1×10 18 / cm 3 Up to 1×10 19 / cm 3 .

[0049] In addition, if Figure 3 As shown, the silicon carbide layer 11 is also provided with an N+ doped layer 3 (i.e., the source of the insulated gate bipolar transistor) and a P- doped layer 5, and the concentration of the P- doped layer 5 can be, but is not limited to, set to 2×10 16 / cm 3 Up to 1×10 17 / cm 3 , each second P+ doped layer 4 is electrically connected to the P− doped layer 5 .

[0050] So, combined Figure 4 As shown, the N-doped layer 17 can be used as a hole blocking layer for the first P+ doped layer 10 in contact therewith, and the higher the doping concentration of the N-doped layer 17, the higher the barrier height of the hole blocking layer, and the lower the on-state voltage drop of the insulated gate bipolar transistor, thereby improving the on-state performance of the insulated gate bipolar transistor; Figure 3 As shown, the P-doped layer 5 is electrically connected to multiple second P+ doped layers 4, so that when the second P+ doped layer 4 is connected to the outside world, the potential of the P-doped layer 5 can be reduced by controlling the potential of the second P+ doped layer 4, thereby suppressing the parasitic BJT (Bipolar Transistor) misconduction effect of the insulated gate bipolar transistor body, thereby improving the performance of the insulated gate bipolar transistor.

[0051] Alternatively, if Figure 4 As shown, a gate insulating layer and a conductive material are provided in the protection trench 9, and the conductive material and the N-doped layer 17, the conductive material and the first P+ doped layer 10, and the conductive material and the second P+ doped layer 4 are all isolated by the gate insulating layer. Figure 2 Compared with the structure of the insulated gate bipolar transistor shown in Figure 4 The insulated gate bipolar transistor shown does not need to be provided with a first through hole on the gate insulating layer at the bottom of the protection trench, thereby reducing the process cost of the insulated gate bipolar transistor.

[0052] Furthermore, if Figure 4 As shown, the orthographic projections of the N-doped layer 17 and the second P+-doped layer 4 on the substrate 13 are both located within the orthographic projection of the first P+-doped layer 10 on the substrate 13. In this way, the second P+-doped layer 4, the N-doped layer 17, and the first P+-doped layer 10 can form an equivalent PMOS and an equivalent PNP structure, thereby forming an equivalent element in the insulated gate bipolar transistor, thereby improving the performance of the insulated gate bipolar transistor.

[0053] Specifically, when the insulated gate bipolar transistor has an N-doped layer and the gate insulating layer at the bottom of the protection trench is not provided with a first through hole, Figure 6As shown, the equivalent element formed in the insulated gate bipolar transistor includes: the equivalent PMOS formed by the second P+ doped layer 4 (equivalent drain of PMOS), the conductive material 8 (equivalent gate metal of PMOS), the gate insulating layer 6 in the protection groove 9 (equivalent gate insulating layer of PMOS), the first P+ doped layer 10 (equivalent source of PMOS), and the N-doped layer 17 (equivalent inversion channel position of PMOS); the second P+ doped layer 4 (equivalent collector of transistor PNP1), the N-doped layer 17 (equivalent inversion channel position of PMOS); The equivalent transistor PNP1 with a free base is formed by the first P+ doped layer 17 (the base of the equivalent transistor PNP1), and the first P+ doped layer 10 (the emitter of the equivalent transistor PNP1); the equivalent transistor PNP2 with hole injection function is formed by the P+ substrate 13 (the emitter of the equivalent transistor PNP2), the silicon carbide layer 11 between the first P+ doped layer 10 and the substrate 13 (the base of the equivalent transistor PNP2), and the first P+ doped layer 10 (the collector of the equivalent transistor PNP2). It should be understood that Figure 6 Only part of the equivalent PMOS, part of the equivalent transistor PNP1, and part of the equivalent transistor PNP2 are shown. The setting position and setting quantity of the equivalent PMOS, the equivalent transistor PNP1, and the equivalent transistor PNP2 can be determined according to the setting position and setting quantity of the corresponding component structure.

[0054] In this way, when the insulated gate bipolar transistor is in a reverse withstand voltage state, since the equivalent PMOS clamp is turned on, the first P+ doped layer 10 is equivalently grounded, thereby improving the reliability of the insulated gate bipolar transistor; when the insulated gate bipolar transistor is in a saturation region, the collector voltage of the insulated gate bipolar transistor is low, and the emitter-to-base voltage drop inside the equivalent transistor PNP1 is low. At this time, the first P+ doped layer 10 is a floating region, and the N-doped layer 17 forms a hole blocking layer. At this time, the insulated gate bipolar transistor is in the on state, and the electrons in the N+ doped layer are injected into the silicon carbide layer 11 between the first P+ doped layer 10 and the substrate 13, forming the base current of the equivalent transistor PNP2, and the holes injected by the P+ substrate 13 produce a hole aggregation effect in the first P+ doped layer 10 and the silicon carbide layer 11 region near it, thereby improving the injection enhancement effect of the insulated gate bipolar transistor, reducing the on-state voltage drop of the insulated gate bipolar transistor, and improving the performance of the insulated gate bipolar transistor; when the insulated gate bipolar transistor is in the amplification region, the collector voltage of the insulated gate bipolar transistor is relatively high, and the voltage of the N-doped layer 17 increases, which is related to the The depletion region between the second P+ doped layers 4 is further expanded, and after contacting the first P+ doped layer 10, the first P+ doped layer 10 is clamped due to the punch-through of the equivalent transistor PNP1, and the first P+ doped layer 10 produces a JFET effect, which reduces the saturation current of the insulated gate bipolar transistor; when the insulated gate bipolar transistor is in the transient process of switching, the voltage of the N-doped layer 17 is relatively high, and the first P+ doped layer 10 is clamped due to the punch-through of the equivalent transistor PNP1, thereby reducing the Miller capacitance of the insulated gate bipolar transistor in the transient process of switching, reducing the switching loss of the insulated gate bipolar transistor, and increasing the switching frequency of the insulated gate bipolar transistor.

[0055] It should be understood that when the insulated gate bipolar transistor has a periodic structure, the number of the protection trench between two adjacent gate trenches can be one, and of course, can also be two, three or more, which is not limited here.

[0056] 3. Other structures.

[0057] Alternatively, if Figure 3 As shown, there is a gap Y between the first P+ doped layers 10 corresponding to two adjacent protection trenches 9. In this way, the silicon carbide layer, ie, the drift layer, of the insulated gate bipolar transistor is turned on, so that the insulated gate bipolar transistor can work normally.

[0058] Alternatively, if Figure 3 As shown, a third P+ doped layer 16 is provided between the gate trench and the substrate 13, and the bottom of the gate trench contacts the third P+ doped layer 16. In this way, the third P+ doped layer 16 can reduce the electric field strength of the gate insulating layer 6 at the bottom of the gate trench, reduce the probability of the gate insulating layer 6 being broken down, and thus improve the reliability of the insulated gate bipolar transistor.

[0059] Furthermore, if Figure 2 As shown, the insulated gate bipolar transistor further includes: a metal layer 1 disposed on the silicon carbide layer 11, and an electrode insulating layer 2 disposed between the metal layer 1 and the gate 7. The electrode insulating layer 2 is provided with a second through hole ( Figure 2 The metal layer 1 includes a gate metal, and the gate metal is electrically connected to the gate 7 through the second through hole. In this way, the metal layer 1 and the gate 7 can be isolated through the electrode insulating layer 2, and the gate 7 can be electrically connected to the gate metal through the second through hole, so that the gate voltage signal can be transmitted to the gate 7.

[0060] It should be understood that Figure 4 As shown, the region X between the vertical dotted lines is a repeating unit of the insulated gate bipolar transistor, that is, the structure included in the region X can be repeatedly extended to both sides.

[0061] Alternatively, if Figure 7 As shown, Figure 7 FIG. 1 is a top view of the silicon carbide layer away from the substrate surface, wherein the P-doped layer 5 cannot be observed due to the viewing angle, but in order to reflect the P-doped layer 5 corresponding to the channel of the gate trench, the P-doped layer 5 is displayed in FIG. Figure 7 The silicon carbide layer is also provided with: a plurality of second P + doped layers 4 disposed on both sides of the gate trench, and the second P + doped layers 4 located on both sides of the gate trench are arranged in an alternating manner.

[0062] In this way, the P-doped layer is electrically connected to multiple second P+ doped layers, and the second P+ doped layers located on both sides of the gate trench are arranged in an alternating manner, which makes it easier to suppress the parasitic BJT misconduction effect of the insulated gate bipolar transistor body, thereby improving the performance of the insulated gate bipolar transistor.

[0063] In addition, if Figure 3 As shown, a surface of the substrate 13 away from the silicon carbide layer 11 may be provided with a back metal, and the back metal may serve as a drain 14 and form an ohmic contact with the substrate 13 to improve the performance of the insulated gate bipolar transistor.

[0064] Based on the same inventive concept, an embodiment of the present invention also provides a method for manufacturing an insulated gate bipolar transistor. The implementation principle of the manufacturing method is similar to the implementation principle of the aforementioned insulated gate bipolar transistor. The specific implementation method of the manufacturing method can refer to the embodiment of the aforementioned insulated gate bipolar transistor, and the repeated parts will not be repeated.

[0065] Specifically, an embodiment of the present invention provides a method for manufacturing an insulated gate bipolar transistor, such as Figure 8 As shown, including:

[0066] S801. Form a buffer layer on a substrate, wherein the substrate is made of P+ silicon carbide and the buffer layer is made of P silicon carbide.

[0067] In step S801, a CVD (chemical vapor deposition) process may be used, using methane or propane as a material growth gas and hydrogen as a carrier gas to epitaxially grow a buffer layer. Of course, the buffer layer may also be obtained by other methods well known to those skilled in the art, which are not limited here.

[0068] S802 , forming a silicon carbide layer including a first P+ doped layer on the buffer layer, wherein the silicon carbide layer is made of N-type silicon carbide.

[0069] In step S802, a CVD process may be used, using methane or propane as a material growth gas and hydrogen as a carrier gas for epitaxial growth to obtain a silicon carbide layer. Of course, the silicon carbide layer may also be obtained by other methods well known to those skilled in the art, which are not limited here.

[0070] S803. Form a gate trench and protection trenches on both sides of the gate trench on the surface of the silicon carbide layer; the gate trench has a sidewall, the sidewall includes a channel region, and the sidewall has an inclination angle relative to the substrate surface, and the inclination angle makes the gate trench narrower on the side facing the substrate and wider on the side away from the substrate; the first P+ doped layer is located between each protection trench and the substrate, and the bottom of the protection trench is in contact with the corresponding first P+ doped layer.

[0071] In step S803 , when forming the gate trench and the protection trench, both can be fabricated by using an ICP (Inductively Coupled Plasma) etching method.

[0072] In this way, a buffer layer and a silicon carbide layer are formed on the substrate, so that when the insulated gate bipolar transistor is in an on state, the substrate injects holes into the silicon carbide layer, and the insulated gate bipolar transistor produces an injection enhancement effect, thereby reducing the on-state voltage drop and improving the performance of the insulated gate bipolar transistor; in addition, the formed protection trench and the first P+ doped layer can also reduce the electric field strength near the gate trench, so that the insulated gate bipolar transistor is not easy to fail due to breakdown, thereby improving the reliability of the insulated gate bipolar transistor.

[0073] Optionally, forming a silicon carbide layer including a first P+ doped layer on the buffer layer includes: forming a first silicon carbide layer on the buffer layer; forming a first P+ doped layer on the surface of the first silicon carbide layer by ion implantation; forming a second silicon carbide layer on the first silicon carbide layer having the first P+ doped layer; the first silicon carbide layer and the second silicon carbide layer constitute a silicon carbide layer;

[0074] A gate trench and protection trenches on both sides of the gate trench are formed on the surface of the silicon carbide layer, including: forming a gate trench and protection trenches on both sides of the gate trench on the surface of the second silicon carbide layer.

[0075] In this way, a first P+ doped layer is formed on the surface of the first silicon carbide layer, and then a second silicon carbide layer is formed, which reduces the energy required for ion implantation when forming the first P+ doped layer, weakens damage to the silicon carbide layer, and reduces the manufacturing cost of the insulated gate bipolar transistor.

[0076] Optionally, forming a second silicon carbide layer on a first silicon carbide layer having a first P+ doped layer, comprises: forming a first layer on the first silicon carbide layer having the first P+ doped layer; forming an N-doped layer in the first layer by an ion implantation method, wherein the N-doped layer is located on the first P+ doped layer; forming a second layer on the first layer having the N-doped layer, wherein the first layer and the second layer constitute a second silicon carbide layer; forming a second P+ doped layer in the second layer by an ion implantation method, wherein the second P+ doped layer is located on the N-doped layer;

[0077] Forming a protection groove on the surface of the silicon carbide layer includes: etching the second P+ doped layer and the N doped layer to obtain a protection groove that penetrates the second P+ doped layer and the N doped layer.

[0078] In this way, an N-doped layer is formed in the first layer, and then the second layer is formed, which reduces the energy required for ion implantation when forming the N-doped layer, weakens the damage to the silicon carbide layer, and reduces the manufacturing cost of the insulated gate bipolar transistor; and the formed N-doped layer can serve as a hole blocking layer for the first P+ doped layer in contact with it, and the higher the doping concentration of the N-doped layer, the higher the barrier height of the hole blocking layer, and the lower the on-state voltage drop of the insulated gate bipolar transistor, which can improve the performance of the insulated gate bipolar transistor.

[0079] Optionally, the method for manufacturing the insulated gate bipolar transistor further includes: forming a gate insulating layer in the protection trench; etching the gate insulating layer in the protection trench to form a first through hole, wherein the first through hole exposes the first P+ doped layer; and filling the protection trench with a conductive material so that the conductive material is connected to the first P+ doped layer through the first through hole. In this way, the first through hole formed by etching can connect the conductive material to the first P+ doped layer, and the potential of the first P+ doped layer can be clamped by controlling the potential of the conductive material, thereby facilitating the first P+ doped layer to protect the gate trench and improving the reliability of the insulated gate bipolar transistor.

[0080] Optionally, the method for manufacturing the insulated gate bipolar transistor further includes: after forming the gate trench, forming a third P+ doped layer between the gate trench and the substrate, and the bottom of the gate trench is in contact with the third P+ doped layer. In this way, the third P+ doped layer can be formed by lower ion implantation energy, thereby reducing the manufacturing cost of the insulated gate bipolar transistor and improving the reliability of the insulated gate bipolar transistor.

[0081] The insulated gate bipolar transistor and the manufacturing method thereof provided by the embodiments of the present invention are explained below in conjunction with specific embodiments.

[0082] Embodiment 1:

[0083] like Figure 4 As shown, the substrate 13 is a P+ conductive substrate made of silicon carbide with a hexagonal crystal structure, and its main surface (i.e., the surface in contact with the buffer layer 12) has a deviation angle of less than 5° relative to the reference plane {000-1} crystal plane family; in the <1-100> crystal direction family direction, the deviation angles of the first side wall relative to the {0-33-8} crystal plane family and the {01-1-4} crystal plane family, and the deviation angles of the second side wall relative to the {0-33-8} crystal plane family and the {01-1-4} crystal plane family are both greater than -3° and less than 3°. If the side wall projection is defined as: the normal of the side wall is at the angle between <1-100> and <0001> The projection on the plane defined by the crystal orientation family, the projection of the {0-33-8} or {01-1-4} crystal plane family is defined as: the normal of the corresponding crystal plane of the {0-33-8} crystal plane family and the {01-1-4} crystal plane family is between <1-100> and <0001> When projecting on the plane defined by the crystal direction family, the deviation angle can be defined as: the angle between the side wall projection and the {0-33-8} or {01-1-4} crystal plane family projection, and the larger the absolute value of the deviation angle, the more the side wall projection is biased towards the <1-100> crystal direction family compared to the {0-33-8} or {01-1-4} crystal plane family projection, and vice versa. Since the angle between the first side wall and the {0-33-8} or {01-1-4} crystal plane family, and the angle between the second side wall and the {0-33-8} or {01-1-4} crystal plane family are relatively small, it can be considered that each of the first side wall and the second side wall belongs to the {0-33-8} crystal plane family or the {01-1-4} crystal plane family in the case of the hexagonal crystal system; and when these two angles are greater than 0°, it means that the plane where the first side wall is located is not the plane where the {0-33-8} or {01-1-4} crystal plane family is located, and the plane where the second side wall is located is not the plane where the {0-33-8} or {01-1-4} crystal plane family is located. Both of them have an angle with the plane where the {0-33-8} or {01-1-4} crystal plane family is located. The angle limits the effective channel length of the insulated gate bipolar transistor. In this way, the lengths of the first side wall and the second side wall can be set according to the required effective channel length.

[0084] like Figure 4 The manufacturing method of the insulated gate bipolar transistor shown includes multiple epitaxial processes. First, a first silicon carbide layer 11a is epitaxially formed on the buffer layer 12 once, and a first P+ doped layer 10 is formed to protect the gate insulating layer 6 at the bottom of the gate trench 18; then, a first layer 11b1 is epitaxially formed on the first silicon carbide layer 11a for a second time, and an N-doped layer is formed, and the thickness of the N-doped layer 17 along the direction indicated by F1 is the thickness of the first layer 11b1 along the direction indicated by F1, and the first silicon carbide layer 11a has the same doping concentration as the first layer 11b1; finally, a second layer 11b2 is epitaxially formed on the first layer 11b1 for three times, and a second P+ doped layer 4 is formed, and the thickness of the second P+ doped layer 4 along the direction indicated by F1 is approximately the thickness of the second layer 11b2 along the direction indicated by F1, and the first layer 11b1 has the same doping concentration as the second layer 11b2.

[0085] The manufacturing method and process implementation of the insulated gate bipolar transistor of the first embodiment include the following steps:

[0086] S1, such as Fig. 9 As shown in (a), a buffer layer 12, a first silicon carbide layer 11a, and a first P+ doped layer 10 are formed.

[0087] The specific process may include: in P+ heavy doping (doping concentration can be 1×10 19 / cm 3 ) conductive substrate by CVD process, using propane or methane as material growth gas, hydrogen as carrier gas, first grow a buffer layer with P-type conductivity, and then epitaxially grow an intrinsic low-doped N-type drift layer (nitrogen doping concentration can be 5×10 15 / cm 3 Up to 1×10 16 / cm 3 ), namely the first silicon carbide layer, which is also the breakdown voltage holding layer of the insulated gate bipolar transistor. In addition, the main surface of the substrate has an offset angle of less than 5° relative to the reference plane {000-1}. Next, a mask layer with a predetermined pattern is obtained by using a photolithography process, and a first P+ doped layer is formed as a protection for the gate insulating layer at the bottom of the gate trench by multiple high-energy aluminum ion implantations with different energies and different doses.

[0088] The specific process of forming the first P+ doped layer may include: forming a first mask layer with a predetermined pattern on the surface of the first silicon carbide layer; then, using an ion implantation method to implant aluminum ions into the area exposed by the first mask layer, wherein the maximum implantation energy may be 400keV to 600keV, thereby forming a first P+ doped layer with a vertically distributed concentration at a specific position; finally, removing the first mask layer and cleaning it to facilitate the fabrication of other structures.

[0089] Wherein, forming a first mask layer having a predetermined pattern may specifically include:

[0090] Silicon nitride is deposited on the surface of the first silicon carbide layer and used as an etching barrier layer; a silicon oxide layer is produced on the surface of the etching barrier layer and used as a first mask layer by a PECVD (Plasma Enhanced Chemical Vapor Deposition) method; a photoresist is formed on the surface of the first mask layer, and the photoresist is patterned to obtain a photoresist having a predetermined pattern; an area exposed by the photoresist is etched to transfer the predetermined pattern to the first mask layer, thereby forming a first mask layer having a predetermined pattern.

[0091] Furthermore, when removing the first mask layer, the method may specifically include: performing wet etching using hydrofluoric acid to remove the first mask layer and the etching stop layer.

[0092] S2, such as Fig. 9 As shown in (b), the first layer 11b1, the N-doped layer 17, and the second layer 11b2 are formed.

[0093] The specific process may include: first, epitaxially growing an intrinsic low-doped n-type drift layer (nitrogen doping concentration may be 5×10 15 / cm 3 Up to 1×10 16 / cm 3 ), i.e., the first layer, which is also the breakdown voltage holding layer of the insulated gate bipolar transistor; then, the same process as in step S1 is adopted to obtain a second mask layer with a predetermined pattern, and an N-doped layer is formed by multiple high-energy nitrogen ion implantations with different energies and different doses (the maximum implantation energy can be 400 keV to 1 MeV), and when forming the N-doped layer, a channeling effect can be used to obtain deep ion implantation, and the preferred doping concentration is 1×10 16 / cm 3 Up to 1×10 17 / cm 3 , wherein the higher the doping concentration of the N-doped layer, the higher the barrier height of the hole blocking layer as the first P+ doped layer, and the lower the on-state voltage drop when the insulated gate bipolar transistor is in the saturation region; then, the same process as that for growing the first layer is used to epitaxially grow an intrinsic low-doped n-type drift layer, i.e., the second layer.

[0094] S3, such as Fig. 9 As shown in (c), a P-doped layer 5, a second P+ doped layer 4, and an N+ doped layer 3 are formed.

[0095] The specific process may include: First, using the ion implantation method, aluminum ions are implanted into the surface of the second layer, so that a P-doped layer with a vertically distributed concentration is formed on the entire surface of the second layer; then, using the same process as in step S1 above, a third mask layer with a predetermined pattern is obtained, and through multiple high-energy aluminum ion implantations with different energies and different doses, the maximum implantation energy can be 400 keV to 600 keV, to form a P+ body contact layer with a vertically distributed concentration, that is, a second P+ doped layer, and the doping concentration can be 1×10 18 / cm 3 to 1×10 19 / cm 3 ; Next, using the same process as in step S1 above, a fourth mask layer with a predetermined pattern is obtained, and through multiple high-energy nitrogen ion implantations with different energies and different doses, the maximum implantation energy can be 100 keV to 200 keV, to form an N+ source region with a vertically distributed concentration, that is, an N+ doped layer.

[0096] S4. As shown in (d) of Fig. 9 above, the gate trench 18 is formed.

[0097] The specific process may include: Using the same process as in step S1 above, a fifth mask layer with a predetermined pattern is obtained, and using predetermined etching conditions, through ICP etching, the N+ doped layer 3, the P-doped layer 5, and the first layer 11b1 are etched to form the gate trench 18.

[0098] Among them, in this step S4, the etching conditions may include the following two types:

[0099] The first etching condition: First, use a mixed gas of HBr, SF6, and O2 for ICP etching, and the angle between the side wall of the etched trench and the substrate surface is at least 88°; then, in a chlorine gas atmosphere, the process temperature is 900 °C, and etching is continued to facilitate the formation of a V-shaped gate trench. Among them, chlorine reacts with silicon carbide on the inner surface of the trench, and the generated carbon atoms react with O2 to become CO x gas, 1.0 < x < 2.0, and SiCl with a boiling point of 56.8 °C is generated y , 0.5 < y < 2.0, SiCl y and CO2 are gases at high temperatures and leave the trench surface, thereby forming the gate trench. In this etching condition, since chlorine is used, the material for making the fifth mask layer can be photoresist.

[0100] At this time, the principles of the V-shaped gate groove include: as the depth of the etched groove increases, the concentration of the reaction gas decreases, and the rate of lateral etching decreases with the depth, a V-shaped groove can be obtained, and by adjusting the flow rate of each gas and the ratio of chlorine to oxygen, an ideal gate groove with the first side wall and the second side wall of the {0-33-8} crystal plane family or the {01-1-4} crystal plane family can be obtained, and the ratio of the oxygen flow rate to the chlorine flow rate can be set to 0.1 to 2.0.

[0101] The second etching condition: ICP etching is performed using a mixed gas of HBr, N2, and Ar, wherein when the thickness of the fifth mask layer is 2 μm to 3 μm, a gate trench with an angle of at most 80° between the sidewall and the substrate surface can be etched by adjusting the etching process. In this etching condition, since chlorine gas is not used, the material for making the fifth mask layer can be photoresist or silicon oxide.

[0102] At this time, the principles of the V-shaped gate groove include: the mixed gas can be used as the source of the ion bombardment effect. By bombarding the surface of the film layer with the mixed gas, the surface of the film layer can be etched to form a groove; and during the etching process, the presence of HBr can produce a polymer and adhere to the side wall of the groove. The polymer can prevent the side wall from being further etched, thereby obtaining a V-shaped gate groove.

[0103] Of course, in the second etching condition, in addition to the mixed gas of HBr, N2, and Ar, other mixed gases may also be used, such as but not limited to the mixed gas of SF6, O2, and HBr.

[0104] S5, such as Fig.10 As shown in (a), a protection trench 9 and a third P+ doped layer 16 are formed.

[0105] The specific process of forming the protection groove may include: adopting the same process as in the above step S1 to obtain a sixth mask layer with a predetermined pattern; adopting predetermined etching conditions to perform ICP etching on the area exposed by the sixth mask layer to form protection grooves located on both sides of the gate groove and with a depth of 2μm to 4μm, the width of the protection groove opening is preferably 1μm to 4μm, and the preferred width needs to take into account the etching selectivity and the depth-to-width ratio of the conductive material filling, the depth-to-width ratio of the conductive material filling is preferably 2.5:1, and the distance between the adjacent side walls of the second surface gate trench and the protection groove can be set to 0.6μm to 2μm.

[0106] It is worth noting that when making the protection groove, when a mixed gas of HBr, SF6, and O2 is used for etching, SF6 provides F radicals, which accelerates the reaction rate with silicide, and O2 also accelerates the reaction rate with carbide. However, since the ions are ejected by the side walls, energy loss will be caused, which will cause the ions to collide with the position where the bottom of the etched groove and the side wall are connected. This will cause deeper etching of the connection between the bottom and the side wall of the etched groove, thus forming a sub-groove at the junction of the side wall and the bottom of the groove. The appearance of the sub-groove is not conducive to controlling the morphology of the protection groove, so the generation of the sub-groove should be avoided.

[0107] Moreover, under the same process pressure in the reaction chamber, reducing the O2 flow rate means a higher concentration of HBr, and the polymer on the sidewall will increase. Therefore, when the oxygen flow rate is less than 30sccm, the protective trench sidewall deposition is more obvious; when the oxygen flow rate is greater than 50sccm, SiF will form on the silicon carbide surface and sidewall. x O y The film layer is more likely to accumulate charges and attract more charged ions to the bottom of the protection trench, which accelerates the etching rate near the side wall of the bottom of the protection trench and aggravates the generation of sub-grooves.

[0108] In addition, the ICP power during protection groove etching directly determines the plasma density of the reaction chamber. The increase in power leads to an increase in plasma density, more intense scattering of the sidewalls of the protection groove, and more serious charge accumulation on the sidewalls, which will attract more ions to the junction of the sidewalls and the bottom of the protection groove, resulting in the appearance of sub-grooves at the bottom of the protection groove.

[0109] Therefore, when etching is performed using a mixed gas of HBr, SF6, and O2, by adjusting the flow rate of O2 and the ICP etching power, a protection groove with a vertical sidewall can be obtained, and the obtained protection groove can avoid the generation of sub-grooves. Preferably, the etching conditions include: the flow rate of O2 is 30 sccm to 50 sccm, and the ICP etching power is 500 W to 700 W.

[0110] The specific process of forming the third P+ doped layer may include: using the same process as in step S1 above to obtain a seventh mask layer having a predetermined pattern, and using an ion implantation method to implant aluminum ions into the exposed area of ​​the seventh mask layer (i.e., the area where the bottom of the gate trench is located), with a maximum implantation energy of 0.4 MeV to 1 MeV, so that a doping concentration of 1×10 18 / cm 3 Up to 1×10 19 / cm 3 A third P+ doped layer.

[0111] In addition, after forming the protection groove and the third P+ doping layer according to the above specific process, all the doping layers formed (such as the first P+ doping layer, the second P+ doping layer, the third P+ doping layer, the N doping layer, the N+ doping layer, and the P- doping layer) are activated to make the doping layer change from amorphous to crystallized, thereby realizing the corresponding function. Wherein, the activation process includes: using RF-PECVD (Radio Frequency Plasma Enhanced Chemical Vapor Deposition) method or other methods well known to those skilled in the art, which are not limited here. Taking the RF-PECVD method as an example, a carbon film with a thickness of about 50nm is deposited on the surface of the structure obtained in the above steps, and annealed at 1700°C for 30min. The carbon film can prevent the doping atoms from diffusing outward during the annealing activation process, so that the doping layer changes from amorphous to crystallized. Then, an ashing treatment is performed to remove the carbon film, and the surface of the structure obtained in the above steps is subjected to sacrificial oxidation treatment to remove impurities on the surface, and then a standard RCA (industrial standard wet cleaning process) cleaning is performed.

[0112] S6: Fig.10 As shown in (b), a gate insulating layer 6, a gate electrode 7, and a conductive material 8 are formed.

[0113] The specific process may include: performing a thermal oxidation treatment at 800°C to 1000°C on the structure obtained in the above steps, so that a silicon oxide layer with a thickness of about 50nm to 110nm is generated in the gate trench and the protection trench, as well as other locations; or using chemical vapor deposition to deposit a silicon oxide layer on the surface of the structure obtained in the above steps. Then, a conductive material is deposited on the silicon oxide layer so that the gate trench and the protection trench are filled; wherein the conductive material may be, but is not limited to, an in-situ doped polysilicon material. Afterwards, the silicon oxide layer and the conductive material outside the gate trench and the protection trench are removed; wherein, a dry etching method or a CMP (Chemical Mechanical Polish) method may be used.

[0114] The conductive material in the gate trench can be used as a gate, and the silicon oxide layer in the gate trench and the protection trench can be used as a gate insulating layer.

[0115] S7, such as Fig.10 As shown in (c), an electrode insulating layer 2 and a second through hole ( Fig.10 not shown).

[0116] The specific process may include: using a CVD method to deposit an insulating layer with a thickness of 0.6μm to 1.0μm on the entire surface of the silicon carbide layer away from the substrate; using the same process as in the above step S1 to obtain an eighth mask layer with a predetermined pattern, and then etching the exposed position of the eighth mask layer to form an electrode insulating layer covering the gate and a second through hole penetrating the electrode insulating layer.

[0117] S8, such as Fig.10 As shown in (d), a metal layer 1 is formed (including the formation of gate metal and source metal, Fig.10 ), and a drain 14.

[0118] The specific process may include: depositing a metal layer on the entire surface of the silicon carbide layer away from the substrate; using the same process as in the above step S1, after obtaining a ninth mask layer with a predetermined pattern, etching the exposed position of the ninth mask layer, so as to etch the gate metal and the source metal in the metal layer, and the gate metal is electrically connected to the gate through the second through hole in the electrode insulating layer, the source metal is electrically connected to the N+ doped layer, the second P+ doped layer, and the conductive material located near the gate groove, and an ohmic contact is formed between the source metal and the N+ doped layer, wherein the N+ doped layer located near the gate groove can be regarded as the source of the insulated gate bipolar transistor; after thinning the substrate, a back metal is formed on the surface of the substrate away from the silicon carbide layer 11, and the back metal serves as the drain of the insulated gate bipolar transistor, and then laser annealing is performed to form an ohmic contact between the drain and the substrate. It should be understood that the drain can be made of other materials and structures that are well known to those skilled in the art and can form an ohmic contact with the substrate, which is not limited here.

[0119] Thus, the insulated gate bipolar transistor in the first embodiment can be manufactured through the above steps S1 to S8. The effects and principles of the insulated gate bipolar transistor are as follows:

[0120] The insulated gate bipolar transistor in the first embodiment does not need to etch a first through hole on the gate insulating layer at the bottom of the protection trench for contact between the conductive material and the first P+ doped layer, thereby reducing the process cost of the insulated gate bipolar transistor; at the same time, through various equivalent elements inside the insulated gate bipolar transistor, the performance improvement of the insulated gate bipolar transistor can be comprehensively achieved.

[0121] like Figure 6 As shown, the equivalent elements formed in the insulated gate bipolar transistor include: equivalent PMOS, equivalent transistor PNP1, and equivalent transistor PNP2. In this way, the above three equivalent elements are parasitic in the insulated gate bipolar transistor, which will have different effects on the insulated gate bipolar transistor in different working states, as follows:

[0122] When the insulated gate bipolar transistor is in the off state and the conductive material is grounded, that is, the potential is 0V, the potential of the N-doped layer (equivalent PMOS inversion channel position) increases, and the equivalent PMOS clamp is turned on, so that the first P+ doped layer is in an equivalent grounded state, so that the first P+ doped layer plays an electric field shielding role for the gate insulating layer in the gate trench, effectively protecting the gate insulating layer in the gate trench, and improving the reliability of the insulated gate bipolar transistor. It should be understood that the above-mentioned off state includes but is not limited to the reverse withstand voltage state.

[0123] When the insulated gate bipolar transistor is in the on state and the collector voltage is low, that is, when the insulated gate bipolar transistor is in the saturation region, the forward voltage drop from the emitter to the base of the equivalent transistor PNP1 is low, and the first P+ doped layer (the emitter of the equivalent transistor PNP1) becomes a floating region. The N-doped layer can be equivalent to a blocking layer for hole carriers inside the first P+ doped layer at this time; and, at this time, the channel of the insulated gate bipolar transistor is in the on state, and the N+ doped layer injects majority carriers (i.e., electrons) into the silicon carbide layer through the channel located in the P-doped layer, and the majority carriers can be used as the base current of the equivalent transistor PNP2. At this time, the holes injected from the substrate (emitter of the equivalent transistor PNP2) partially recombine with the base current of the equivalent transistor PNP2, and most of the holes have a clustering effect in the first P+ doping layer (i.e., floating P+ injection region) and the silicon carbide layer near the first P+ doping layer, thereby improving the injection enhancement effect of the insulated gate bipolar transistor, reducing the on-state voltage drop of the insulated gate bipolar transistor, and improving the performance of the insulated gate bipolar transistor. In this process, the channel of the equivalent PMOS is not opened, so the equivalent PMOS does not play a role.

[0124] When the insulated gate bipolar transistor is in the amplification region, there is a high voltage drop from the drain to the source of the insulated gate bipolar transistor in this on state. At this time, the voltage of the N-doped layer is further increased, and the PN junction formed by the N-doped layer and the second P+ doped layer is reverse biased. When the depletion region of the N-doped layer contacts the first P+ doped layer, the first P+ doped layer can be clamped by the punch-through effect of the equivalent transistor PNP1, thereby improving the protection of the gate insulating layer in the gate trench and improving the reliability of the insulated gate bipolar transistor; in addition, the equivalent transistor PNP1 at this time has a JFET current limiting effect, which can effectively reduce the saturation current of the insulated gate bipolar transistor.

[0125] When the insulated gate bipolar transistor is in the transient process of switching, due to the aggregation of holes, the voltages of the first P+ doped layer and the N doped layer are relatively high, which is more likely to cause the punch-through of the equivalent transistor PNP1, thereby clamping the first P+ doped layer, thereby reducing the Miller capacitance of the insulated gate bipolar transistor in the transient process of switching, reducing the switching loss of the insulated gate bipolar transistor, and increasing the switching frequency of the insulated gate bipolar transistor.

[0126] In summary, three equivalent elements are parasitic in the insulated gate bipolar transistor. Through the design of the insulated gate bipolar transistor structure, three equivalent elements are parasitic inside the insulated gate bipolar transistor, thereby obtaining different electrical performance improvements under different working conditions; when the insulated gate bipolar transistor is in the reverse withstand voltage state, since the equivalent PMOS clamp is turned on, the first P+ doped layer is equivalently grounded, which improves the reliability of the insulated gate bipolar transistor; when the insulated gate bipolar transistor is in the saturation region, the hole blocking layer formed by the equivalent transistor PNP1 and the base current of the equivalent transistor PNP2 produce a hole aggregation effect, which improves the injection enhancement effect of the insulated gate bipolar transistor, making The conduction voltage drop of the insulated gate bipolar transistor is reduced, and the performance of the insulated gate bipolar transistor is improved; when the insulated gate bipolar transistor is in the amplification region, the equivalent transistor PNP1 clamps the first P+ doped layer due to punch-through, thereby improving the reliability of the insulated gate bipolar transistor, and the first P+ doped layer produces a JFET effect, thereby reducing the saturation current of the insulated gate bipolar transistor; when the insulated gate bipolar transistor is in the transient process of switching, the first P+ doped layer is clamped due to the punch-through of the equivalent transistor PNP1, thereby reducing the Miller capacitance of the insulated gate bipolar transistor in the transient process of switching, reducing the switching loss of the insulated gate bipolar transistor, and improving the switching frequency of the insulated gate bipolar transistor.

[0127] Embodiment 2:

[0128] like Figure 1 As shown, the method for manufacturing the insulated gate bipolar transistor in this embodiment is basically similar to the method for manufacturing the insulated gate bipolar transistor in the first embodiment, and the differences include:

[0129] Modify step S2 in the above embodiment 1 to: Figure 1 As shown, an intrinsic low-doped n-type drift layer (nitrogen doping concentration may be 5×10 15 / cm 3 Up to 1×10 16 / cm 3 ), namely the second silicon carbide layer 11b, is also the breakdown voltage holding layer of the insulated gate bipolar transistor.

[0130] Therefore, the difference between this second embodiment and the aforementioned first embodiment is that an N-doped layer is not provided in this embodiment, so the equivalent PMOS and equivalent transistor PNP1 mentioned in the aforementioned first embodiment do not exist in the insulated gate bipolar transistor, and although the equivalent transistor PNP2 exists in the insulated gate bipolar transistor of this second embodiment, its influence can be ignored.

[0131] Furthermore, for the insulated gate bipolar transistor in Example 2, when the gate voltage exceeds the threshold voltage, an inversion layer will be formed inside the channel, and the electrons in the N+ doped layer will be injected into the second silicon carbide layer and the first silicon carbide layer through the inversion layer; and, the holes in the substrate are injected into the first silicon carbide layer and the second silicon carbide layer through the buffer layer, and a conductivity modulation effect occurs in the silicon carbide layer, thereby reducing the resistance between the source and the drain of the silicon carbide insulated gate bipolar transistor and improving the performance of the insulated gate bipolar transistor.

[0132] It should be understood that the manufacturing method of the insulated gate bipolar transistor in this embodiment is similar to the manufacturing method of the insulated gate bipolar transistor in the aforementioned embodiment 1, and reference can be made to the manufacturing method of the insulated gate bipolar transistor in the aforementioned embodiment 1, and the repeated parts will not be repeated.

[0133] Embodiment three:

[0134] like Figure 2 As shown, the method for manufacturing the insulated gate bipolar transistor in this embodiment is basically similar to the method for manufacturing the insulated gate bipolar transistor in the first embodiment, and the differences include:

[0135] (1) Modify step S2 in the above embodiment 1 to: Figure 2 As shown, an intrinsic low-doped n-type drift layer (nitrogen doping concentration may be 5×10 15 / cm 3 Up to 1×10 16 / cm 3 ), namely the second silicon carbide layer 11b, is also the breakdown voltage holding layer of the insulated gate bipolar transistor.

[0136] (2) Modify step S5 in the above embodiment 1 to: Figure 2 As shown, after the protection groove 9 is formed, the gate insulation layer 6 at the bottom of the protection groove 9 is further etched using a self-alignment process to the upper surface of the first silicon carbide layer 11a (while ensuring that the sidewall oxide of the protection groove 9 maintains protection for the sidewall), and then the resist is removed to form a third P+ doped layer 16.

[0137] Therefore, the difference between the third embodiment and the first embodiment is that in this embodiment, no N-doped layer is provided, and a first through hole is provided in the gate insulating layer at the bottom of the protection trench.

[0138] Furthermore, for the insulated gate bipolar transistor in Example 3, by etching a first through hole in the gate insulation layer at the bottom of the protection groove, the conductive material and the first P+ doped layer are in direct contact, and the grounding of the first P+ doped layer can be effectively achieved through the grounding of the conductive material, thereby providing protection for the gate insulation layer at the bottom of the gate trench, thereby improving the reliability of the insulated gate bipolar transistor.

[0139] It should be understood that the manufacturing method of the insulated gate bipolar transistor in this embodiment is similar to the manufacturing method of the insulated gate bipolar transistor in the aforementioned embodiment 1, and reference can be made to the manufacturing method of the insulated gate bipolar transistor in the aforementioned embodiment 1, and the repeated parts will not be repeated.

[0140] Embodiment 4:

[0141] like Figure 3 As shown, the method for manufacturing the insulated gate bipolar transistor in this embodiment is basically similar to the method for manufacturing the insulated gate bipolar transistor in the first embodiment, and the differences include:

[0142] The step S4 in the above-mentioned embodiment 1 is adjusted to: adopt the etching process in the step S5 in the above-mentioned embodiment 1 to form a gate trench, and the etching depth and the opening remain unchanged.

[0143] Therefore, the difference between this fourth embodiment and the aforementioned first embodiment is that the crystal plane family where the gate trench sidewall is located in this embodiment is changed from the {0-33-8} crystal plane family or the {01-1-4} crystal plane family to the {11-20} crystal plane family, which is specifically reflected in the gate trench morphology changing from "V" type to "U" type.

[0144] Furthermore, at this time, the first sidewall and the second sidewall of the gate trench may correspond to the vertical {11-20} crystal plane family, and the carrier mobility in the channel formed thereby is also relatively high, which can reduce the on-resistance of the insulated gate bipolar transistor and improve the performance of the insulated gate bipolar transistor.

[0145] It should be understood that the manufacturing method of the insulated gate bipolar transistor in this embodiment is similar to the manufacturing method of the insulated gate bipolar transistor in the aforementioned embodiment 1, and reference can be made to the manufacturing method of the insulated gate bipolar transistor in the aforementioned embodiment 1, and the repeated parts will not be repeated.

[0146] Based on the same inventive concept, an embodiment of the present invention further provides an electronic device, the implementation principle of which is similar to the implementation principle of the aforementioned insulated gate bipolar transistor. The specific implementation method of the electronic device can refer to the embodiment of the aforementioned insulated gate bipolar transistor, and the repeated parts will not be repeated.

[0147] Specifically, an electronic device provided by an embodiment of the present invention is Fig.11 As shown, it includes: an insulated gate bipolar transistor 1101 as described in the above embodiment.

[0148] The electronic device may be any device including an insulated gate bipolar transistor, such as but not limited to: an AC motor, a frequency converter, a switching power supply, a lighting circuit, etc.

[0149] Obviously, those skilled in the art can make various changes and modifications to the present invention without departing from the spirit and scope of the present invention. Thus, if these modifications and variations of the present invention fall within the scope of the claims of the present invention and their equivalents, the present invention is also intended to include these modifications and variations.

Claims

1. An insulated gate bipolar transistor, It is characterized in that include: A substrate, and a buffer layer and a silicon carbide layer stacked in sequence on the substrate, wherein the substrate is made of P+ type silicon carbide, the buffer layer is made of P type silicon carbide, and the silicon carbide layer is made of N type silicon carbide; A gate trench is provided in the silicon carbide layer, the gate trench has a sidewall, the sidewall includes a channel region, the sidewall has an inclination angle relative to the substrate surface, and the inclination angle makes the gate trench present a shape that is narrower on a side facing the substrate and wider on a side away from the substrate; Protection grooves are respectively arranged on both sides of the gate groove, and a gate insulating layer and a conductive material are arranged in the protection grooves. A first P+ doping layer is arranged between each protection groove and the substrate, and the bottom of the protection groove is in contact with the corresponding first P+ doping layer; the gate insulating layer covers the side wall and the bottom surface of the protection groove, and the conductive material is located on the side of the gate insulating layer away from the first P+ doping layer.

2. The insulated gate bipolar transistor according to claim 1, It is characterized in that The silicon carbide layer is further provided with: an N-doped layer and a second P+-doped layer stacked in sequence on the first P+-doped layer in a direction from the substrate to the buffer layer; The N-doped layer and the second P+-doped layer are both located on two sides of the protection trench.

3. The insulated gate bipolar transistor according to claim 2, It is characterized in that The conductive material and the N-doped layer, the conductive material and the first P+-doped layer, and the conductive material and the second P+-doped layer are all isolated by the gate insulating layer.

4. The insulated gate bipolar transistor according to claim 2, It is characterized in that The orthographic projections of the N-doped layer and the second P+-doped layer on the substrate are both located within the orthographic projection of the first P+-doped layer on the substrate.

5. The insulated gate bipolar transistor according to claim 1, It is characterized in that The gate insulating layer is provided with a through hole, and the conductive material is connected to the first P+ doped layer through the through hole.

6. The insulated gate bipolar transistor according to claim 1, It is characterized in that There is a gap between the first P+ doped layers corresponding to two adjacent protection trenches.

7. The insulated gate bipolar transistor according to claim 1, It is characterized in that A third P+ doping layer is disposed between the gate trench and the substrate, and the bottom of the gate trench is in contact with the third P+ doping layer.

8. The insulated gate bipolar transistor according to any one of claims 1 to 7, It is characterized in that The side wall includes: a first side wall and a second side wall opposite to each other, the first side wall and the second side wall both belong to the {0-33-8} crystal plane family or the {01-1-4} crystal plane family in the case of a hexagonal crystal system, and an inclination angle of the first side wall relative to the substrate surface is different from an inclination angle of the second side wall relative to the substrate surface.

9. The insulated gate bipolar transistor according to any one of claims 1 to 7, It is characterized in that The sidewall includes a first sidewall and a second sidewall opposite to each other, and the first sidewall or the second sidewall belongs to the {11-20} crystal plane family in the case of a hexagonal system.

10. A method for manufacturing an insulated gate bipolar transistor according to any one of claims 1 to 9, It is characterized in that include: Forming a buffer layer on a substrate, wherein the substrate is made of P+ silicon carbide and the buffer layer is made of P silicon carbide; Forming a silicon carbide layer including a first P+ doped layer on the buffer layer, wherein the silicon carbide layer is made of N-type silicon carbide; Forming a gate trench and protection trenches on both sides of the gate trench on the surface of the silicon carbide layer; The gate trench has a sidewall, the sidewall includes a channel region, and the sidewall has an inclination angle relative to the substrate surface, and the inclination angle makes the gate trench present a shape that is narrower on a side facing the substrate and wider on a side away from the substrate; The first P+ doping layer is located between each of the protection trenches and the substrate, and the bottom of the protection trench is in contact with the corresponding first P+ doping layer.

11. The method according to claim 10, It is characterized in that Forming a silicon carbide layer including a first P+ doped layer on the buffer layer, comprising: forming a first silicon carbide layer on the buffer layer; forming the first P+ doped layer on the surface of the first silicon carbide layer by an ion implantation method; forming a second silicon carbide layer on the first silicon carbide layer having the first P+ doped layer formed thereon; the first silicon carbide layer and the second silicon carbide layer constitute the silicon carbide layer; A gate trench and protection trenches located at both sides of the gate trench are formed on the surface of the silicon carbide layer, including: forming the gate trench and the protection trenches located at both sides of the gate trench on the surface of the second silicon carbide layer.

12. The method according to claim 11, It is characterized in that Forming a second silicon carbide layer on the first silicon carbide layer on which the first P+ doped layer is formed, comprising: forming a first layer on the first silicon carbide layer on which the first P+ doped layer is formed; forming an N-doped layer in the first layer by an ion implantation method, wherein the N-doped layer is located on the first P+ doped layer; forming a second layer on the first layer on which the N-doped layer is formed, wherein the first layer and the second layer constitute the second silicon carbide layer; forming a second P+ doped layer in the second layer by an ion implantation method, wherein the second P+ doped layer is located on the N-doped layer; Forming a protection groove on the surface of the silicon carbide layer includes: etching the second P+ doped layer and the N doped layer to obtain the protection groove that penetrates the second P+ doped layer and the N doped layer.

13. The method according to claim 10, It is characterized in that Also includes: forming a gate insulating layer in the protection trench; Etching the gate insulating layer in the protection trench to form a through hole, wherein the through hole exposes the first P+ doped layer; A conductive material is filled in the protection trench so that the conductive material is connected to the first P+ doped layer through the through hole.

14. The method according to any one of claims 10 to 13, It is characterized in that Also includes: After the gate trench is formed, a third P+ doping layer is formed between the gate trench and the substrate, and the bottom of the gate trench contacts the third P+ doping layer.

15. An electronic device, It is characterized in that include: An insulated gate bipolar transistor as claimed in any one of claims 1 to 9.