Semiconductor devices and their fabrication methods
By setting a germanium-containing layer on the side of the fins of a semiconductor device, the lattice structure of the channel is improved, solving the problem of insufficient electron mobility in the buried gate structure and achieving higher electron mobility and performance improvement.
Patent Information
- Application Number
- CN202311434993.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2021-05-28
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2041-05-28
AI Technical Summary
In existing dynamic random access memory cells, due to manufacturing technology limitations, the channel electron mobility of buried gate structures is insufficient, resulting in current leakage and poor performance.
By depositing a germanium-containing layer on the sidewall of the fins of a semiconductor device, and forming an appropriate stress layer, the lattice structure of the channel can be improved, thereby enhancing electron mobility.
By setting a germanium-containing layer on the side of the fin, the electron mobility of the channel is improved, thereby enhancing the performance and function of the semiconductor device.
Smart Images

Figure CN117712165B_ABST
Abstract
Description
Technical Field
[0001] This invention generally relates to a semiconductor device and a method for forming the same, and more specifically, to a semiconductor memory device and a method for forming the same. Background Technology
[0002] Reducing the size of memory cells to improve integration has been a long-standing trend in the memory and semiconductor industries, thereby increasing the storage capacity of dynamic random-access memory (DRAM) chips. In DRAM cells with buried gates, current leakage caused by capacitors is reduced or avoided due to the relatively long channel beneath the buried gate. Therefore, due to the superior performance of buried gates, an increasing number of DRAM cells are equipped with buried gates instead of traditional planar gate structures. In general, DRAM cells with buried gates include transistor devices and charge storage devices capable of receiving signals from bit lines and word lines during operation. However, due to limitations in manufacturing technology, many defects are formed in DRAM cells with buried gates. Summary of the Invention
[0003] The object of this invention is to provide a semiconductor device and a method for forming the same, wherein a germanium-containing layer, such as germanium, germanium silicon, germanium oxide, or germanium silicon oxide, is formed on the side surface of a fin to provide appropriate stress on the device channel and an improved lattice structure of the device channel. Therefore, the channel of the semiconductor device of this invention can achieve better electron mobility.
[0004] To achieve the above objectives, one embodiment of the present invention provides a semiconductor device including a substrate, a gate line, and a stress layer. The substrate includes a plurality of first-height fins and a plurality of second-height fins projecting away from the substrate, wherein the first-height fins and the second-height fins have different heights; the gate line is located above the second-height fins and connected to a first sidewall of the first-height fins; the stress layer is made of a different material than the first-height fins and covers the second sidewall of the first-height fins; wherein the first sidewall of the first-height fin is disposed on one side adjacent to the second-height fins, and the second sidewall of the first-height fin is disposed on the other side away from the second-height fins.
[0005] To achieve the above objectives, another embodiment of the present invention provides a semiconductor device including a substrate, a stress layer, a gate line, and a capping layer. The substrate includes a plurality of fins separated by shallow trench isolation; the stress layer is made of a different material than the plurality of fins and is disposed between the plurality of fins and the shallow trench isolation; the gate line is located within the active region and includes a gate dielectric layer and a gate electrode layer stacked sequentially; the capping layer is located on the gate line; wherein, in a direction away from the substrate, the top of the stress layer is higher than the top of the gate electrode layer.
[0006] To achieve the above objectives, another embodiment of the present invention provides a method for forming a semiconductor device, comprising the following steps: First, a substrate is provided, and a plurality of first height fins are formed on the substrate. Next, a stress layer is formed on the sidewalls of the first height fins, wherein the material of the stress layer is different from the material of the first height fins. Then, an insulating material is filled to isolate the plurality of first height fins; trenches are formed within the first height fins, the trenches defining second height fins with different heights. Finally, a gate dielectric layer, a gate electrode layer, and a capping layer are sequentially stacked on the second height fins. Wherein, in a vertical direction away from the substrate, the top of the stress layer is higher than the top of the gate electrode layer.
[0007] In general, the semiconductor device of the present invention further includes a germanium-containing layer disposed on the fin side surface and a gate line across the fin, wherein the germanium-containing layer generates appropriate channel stress and a better lattice structure for the semiconductor device, thereby enabling the semiconductor device to achieve improved high electron mobility. The germanium-containing layer includes, for example, germanium, silicon germanium, germanium oxide, or other suitable materials. In this way, the semiconductor device of the present invention achieves superior functionality and performance.
[0008] The objects of the invention will undoubtedly become apparent to those skilled in the art after reading the detailed description of the preferred embodiments shown in the following various figures. Attached Figure Description
[0009] Figure 1-11 A schematic diagram of a method for forming a semiconductor device according to a first preferred embodiment of the present invention is shown, wherein:
[0010] Figure 1 A top view of the semiconductor device after the active region has been formed is shown;
[0011] Figure 2 It shows along Figure 1 The sectional view intercepted by section line A-A' in the diagram;
[0012] Figure 3A cross-sectional view of a semiconductor device after the formation of a stress layer is shown;
[0013] Figure 4 A cross-sectional view of a semiconductor device after shallow trench isolation is formed is shown;
[0014] Figure 5 A top view of the semiconductor device after trenching is shown;
[0015] Figure 6 It shows along Figure 5 The sectional view intercepted by section line A-A' in the diagram;
[0016] Figure 7 It shows along Figure 5 The sectional view taken by section line B-B' in the diagram;
[0017] Figure 8 A cross-sectional view of a semiconductor device after an oxidation fabrication process is shown.
[0018] Figure 9 A top view of the semiconductor device after the gate lines have been formed is shown;
[0019] Figure 10 It shows along Figure 9 The sectional view intercepted by section line A-A' in the diagram;
[0020] Figure 11 It shows along Figure 9 The sectional view taken by section line B-B' in the diagram;
[0021] Figure 12-13 This is a schematic diagram illustrating a method for forming a semiconductor device according to a second preferred embodiment of the present invention, wherein:
[0022] Figure 12 A cross-sectional view of a semiconductor device after shallow trench isolation has been formed is shown;
[0023] Figure 13 A cross-sectional view of a semiconductor device after trenching is shown;
[0024] Figure 14 Another cross-sectional view of the semiconductor device after the trenches have been formed is shown;
[0025] Figure 15 A schematic diagram of a method for forming a semiconductor device according to a third preferred embodiment of the present invention is shown.
[0026] The reference numerals in the attached figures are explained as follows:
[0027] 100 substrate
[0028] 101 Top surface
[0029] 102 Trench
[0030] 105 trench
[0031] 105a Exposed sidewall
[0032] 105b Exposed bottom wall
[0033] 110 fins
[0034] 115 fins
[0035] 130 Stress Layer
[0036] 150 Shallow Trench Isolation
[0037] 150a Shallow Trench Isolation
[0038] 151 First Insulation Layer
[0039] 152 Oxide Layer
[0040] 153 Second Insulation Layer
[0041] 155 Shallow trench isolation
[0042] 155a Shallow trench isolation
[0043] 155b Shallow trench isolation
[0044] 170 oxide layer
[0045] 170a oxide layer
[0046] 171 Oxide Layer
[0047] 171a oxide layer
[0048] 173 Oxide Layer
[0049] 190 gate structure
[0050] 190a gate structure
[0051] 191 Gate dielectric layer
[0052] 193 Gate electrode layer
[0053] 210 Covering layer
[0054] 300 Semiconductor Devices
[0055] 500 Semiconductor Devices
[0056] D1 direction
[0057] D2 direction
[0058] G1 Distance
[0059] G2 Distance
[0060] H1 height
[0061] H2 height
[0062] T1 thickness
[0063] T2 thickness
[0064] T3 thickness
[0065] T4 thickness Detailed Implementation
[0066] To better understand the present invention, preferred embodiments will be described in detail below. Preferred embodiments of the present invention are shown in the accompanying drawings with numbered elements. Furthermore, without departing from the spirit of the invention, technical features in the different embodiments described below may be substituted for, recombine, or combined to form another embodiment.
[0067] Figure 1-11 A method for forming a semiconductor device according to a preferred embodiment of the present invention is shown, wherein... Figure 1 , 5 Figures 9 and 10 show top views of the semiconductor device during its fabrication process, while the other figures show cross-sectional views of the semiconductor device during its fabrication process. Firstly, as shown in Figures 9 and 10,… Figure 1-2 As shown, a substrate 100, such as a silicon substrate or a silicon-containing substrate, is provided, and a plurality of fins 110 are formed on the substrate 100, each fin 110 protruding from the topmost surface 101 of the substrate 100. In other words, although the plurality of fins 110 and the substrate 100 are integrally formed, the topmost surface 101 of the substrate 100 can still be regarded as the interface between the plurality of fins 110 and the substrate 100 (e.g., ...). Figure 1 (The dashed lines shown).
[0068] In one embodiment, multiple fins 110 can be formed using a self-aligned double patterning (SADP) fabrication process or a self-aligned reverse double patterning (SARP) fabrication process. First, multiple mandrels (not shown) are formed on a bulk silicon substrate (not shown) using photolithography and etching processes. Then, spacer walls (not shown) are formed on the sidewalls of each mandrel. The mandrels are removed, and the spacer walls are used as masks to pattern the bulk silicon substrate, thereby forming a fin 110. Figure 2The multiple trenches 102 shown are used to simultaneously define multiple fins 110. Alternatively, the multiple fins 110 can also be formed by first forming a patterned mask (not shown) on the substrate 100 to partially cover the top surface 101 of the substrate 100, and then performing an epitaxial process on the substrate 100 through the patterned mask to form a semiconductor layer (not shown) on the exposed top surface 101 of the substrate 100, wherein the semiconductor layer serves as the respective multiple fins.
[0069] In one embodiment, each fin 110 is preferably parallel to each other and is disposed via, as shown in the figure Figure 1 The top view shown extends in direction D1, where direction D1 is parallel to the x-direction or y-direction (e.g., Figure 1 The direction D2 shown has an included angle θ, but is not limited to this. Furthermore, as... Figure 1-2 As shown, the groove 102 may include different distance ratios G1 / G2 in the direction D2, such that some fins 110 may be spaced apart from each other with a relatively small distance G1, while other fins 110 may be spaced apart from each other with a relatively large distance G2. However, in another embodiment, based on actual product requirements, each fin 110 may also be spaced apart from each other at the same distance (not shown in the figure).
[0070] like Figure 3 As shown, a stress (material) layer 130 is then formed on the surfaces of the plurality of fins 110 and the topmost surface 101 of the substrate 100, for example, by a deposition process or an epitaxial growth process. Preferably, the stress (material) layer 130 comprises a germanium-containing layer that can generate appropriate stress and a better lattice structure, wherein the germanium-containing layer includes, for example, germanium, silicon-germanium, etc., but is not limited thereto. For example, the stress (material) layer 130 may include silicon-germanium or germanium, while the substrate 100 and the plurality of fins 110 comprise silicon, thereby improving the lattice structure of the substrate 100 and the fins 110. However, in other embodiments, the stress (material) layer 130 may include other materials such as carbides, silicon carbide, etc., for generating appropriate stress and improving the lattice structure. Furthermore, the stress (material) layer 130 comprises a relatively small thickness T1 relative to the substrate 100, for example, the thickness T1 may be from about 1 angstrom to 10 nanometers, but is not limited thereto.
[0071] Then, as Figure 4As shown, shallow trench isolation 150 is formed on substrate 100 to cover stress (material) layer 130, wherein shallow trench isolation 150 surrounds each fin 110. In one embodiment, shallow trench isolation 150 can be formed by at least one deposition process and a planarization process, wherein a first insulating material layer (not shown) can be preferentially deposited on substrate 100 to at least fill trench 102 having a relatively small distance G1, a second insulating material layer (not shown) can then be deposited on the first insulating material layer to fill trench 102 having a relatively large distance G2, and an etch-back process or a chemical mechanical polishing / planarization process can be performed to remove the second insulating material layer and the first insulating material layer disposed on the topmost surface of the plurality of fins 110, thereby forming as shown Figure 4 The shallow trench isolation 150 is shown flush with the topmost surface of the fin 110. Those skilled in the art will fully recognize that, depending on actual product requirements, the shallow trench isolation 150 can also be formed by other processes, such as atomic layer deposition (ALD) or in-situ vapor generation (ISSG).
[0072] The first and second insulating material layers comprise dielectric materials such as silicon oxide, silicon nitride, silicon oxynitride, or silicon carbonitride, and the materials of the first and second insulating material layers may optionally be the same as or different from each other. Preferably, the materials of the first and second insulating material layers are different, for example, including but not limited to silicon oxide and silicon nitride, respectively. Therefore, the shallow trench isolation 150 disposed within a trench 102 having a relatively large distance G2 can have a multilayer structure, the multilayer structure comprising a first insulating layer (including silicon oxide) 151 and a second insulating layer (including silicon nitride) 153 stacked from bottom to top, and the shallow trench isolation 150 disposed within a trench 102 having a relatively small distance G1 can have, for example, a first insulating layer (including silicon oxide) 151 and a second insulating layer (including silicon nitride) 153 stacked from bottom to top, and the shallow trench isolation 150 disposed within a trench 102 having a relatively small distance G1 can have, for example, a first insulating layer (including silicon oxide) 151 and a second insulating layer (including silicon nitride) 153 stacked from bottom to top, and the shallow trench isolation 150 disposed within a trench 102 having a relatively small distance G1. Figure 4 The diagram shows a single-layer structure comprising only the first insulating layer 151. However, in another embodiment, the trench 102 may also be filled with the same dielectric material or more different dielectric materials of varying densities to form a shallow trench isolation having a partially multilayer structure and a partially single-layer structure.
[0073] Next, as Figure 5-7 As shown, at least one groove 105 is formed in direction D2 to intersect with the plurality of fins 110. Those skilled in the art will readily understand that the exact number of grooves 105 can vary based on actual product requirements, for example, but not limited to, such as... Figure 5 The five shown. In one embodiment, each groove 105 is parallel to each other in direction D2 to simultaneously penetrate a plurality of fins 110 extending in direction D1, and if from... Figure 5As shown in the top view, each fin 110 can be penetrated by two trenches 105 simultaneously, but is not limited thereto. The trenches 105 can be formed by first providing a mask (not shown) on the substrate 100, the mask having at least one opening (not shown) that partially exposes the plurality of fins 110 and the shallow trench isolation 150, and then performing at least one etching process to partially remove the exposed portions of the plurality of fins 110 and the shallow trench isolation 150, thereby forming the trenches 105. Therefore, each trench 105 can simultaneously penetrate the shallow trench isolation 150 and the plurality of fins 110 to form a plurality of fins 115 and shallow trench isolation 155, both of which have, within the trench 105, a... Figure 5-6 The height reduction shown. (As indicated) Figure 7 As shown, multiple fins 115 are formed by etching portions of multiple fins 110, and the maximum height H1 of fin 115 is significantly smaller than the maximum height H2 of fin 110. The heights H1 and H2 of fin 115 and fin 110 can be regarded as the distances between the top surfaces of fin 115 and fin 110 and the top surface 101 of substrate 100, respectively.
[0074] It is worth noting that during the etching process, because the etching rate will vary based on the materials of the multiple fins 110 and shallow trench isolations 150, different degrees of etching may exist among the multiple fins 110 and shallow trench isolations 150. Therefore, the bottom wall of each trench 105 located in the multiple fins 115 and shallow trench isolations 155 may not be flush, for example, as... Figure 6 As shown, the top surface of the plurality of fins 115 can be relatively higher than the top surface of the shallow trench isolation 155. It should also be noted that the stress (material) layer 130 disposed on the exposed portions of the plurality of fins 110 is also removed during the etching process, thereby forming a stress layer 130 that directly exposes the top surface of each fin 115, as shown. Figure 6 As shown. In other words, after the etching process, as Figure 7 As shown, the stress layer 130 covers the top surface and side surfaces of each fin 110, and as... Figure 6 As shown, the stress layer 130 covers only the side surface of each fin 115, and a portion of each groove 105 within the fin 110 has exposed sidewalls 105a and exposed bottom walls 105b (i.e., the topmost surface of each fin 115).
[0075] Following on, such as Figure 8As shown, an oxidation process, such as an ALD or ISSG process, is performed on all exposed surfaces of the plurality of fins 110 and 115 to form an oxide layer 170. Specifically, the oxide layer 170 is formed by simultaneously consuming the underlying exposed surfaces; therefore, the portion of the oxide layer 171 disposed on the side surface of each fin 115 and in direct contact with the stress layer 130 may include the same elements as the stress layer 130. For example, while the stress layer 130 comprises silicon germanium or germanium, a portion of the oxide layer 171 may comprise silicon germanium oxide (SiGeO). x or germanium oxide (GeO) x However, this is not the only possibility. On the other hand, the oxide layer 173 disposed on the topmost surface of each fin 115 and in direct contact with the plurality of fins 115 may include the same elements as the plurality of fins 115, such as silicon oxide (SiO2). x ), and the multiple fins 115 include, but are not limited to, silicon or silicon-containing materials. Similarly, although Figure 8 Not shown, but an oxide layer 171 is disposed on another portion of the topmost surface of each fin 110. Figure 8 Not shown in the image, but... Figure 11 (As shown in the diagram) may also include the same elements as the underlying stress layer 130, and its material may therefore be silicon germanium oxide or germanium oxide; and another portion of the oxide layer 173 disposed on the exposed sidewall 105a of each trench 105 ( Figure 8 Not shown in the image, but Figure 11 (As shown in the figure) may also include the same elements as the multiple fins 110, so its material may be, but is not limited to, silicon oxide.
[0076] It should be noted that due to material differences between different portions of the oxide layer 170 (i.e., the portion of oxide layer 171 and the other portion of oxide layer 173), the oxide layer 170 between different portions can include different thicknesses. For example, the thickness T2 of a portion of oxide layer 171 (e.g., including germanium oxide or silicon oxide) is greater than the thickness T3 of another portion of oxide layer 173 (e.g., including silicon oxide), but this is not a limitation. Furthermore, after the oxidation process, the underlying stress layer 130 can therefore include different elemental concentrations in different portions. For example, if the stress layer 130 includes silicon germanium or germanium, the various portions of the stress layer 130 can include different germanium concentrations after the oxidation process, wherein the stress layer 130 disposed below the oxide layer 170 (i.e., the portion of oxide layer 171) has a relatively lower germanium concentration than the stress layer 130 disposed below the shallow trench isolation 155.
[0077] After that, as Figure 9-11As shown, at least one gate structure 190 is formed within the trench 105 to fill the bottom of the trench 105, and then a capping layer 210 is formed on the gate structure 190 to fill the remaining portion of the trench 105. Those skilled in the art will readily recognize that the precise number of gate structures 190 can correspond to the actual number of trenches 105, for example, but not limited to, such as... Figure 9 The five shown. (As shown in the image) Figure 10-11 As shown, each gate structure 190 extends in direction D2 across a plurality of fins 115 and shallow trench isolation 155, and also includes a gate dielectric layer 191 and a gate electrode layer 193 stacked from bottom to top within each trench 105. In one embodiment, the gate structure 190 can be formed by conformally forming a dielectric layer (not shown, such as silicon oxide, silicon nitride or other suitable dielectric material) on a substrate 100 to at least cover the surface of each trench 105, followed by forming a conductive layer (not shown) on the dielectric layer to at least fill each trench 105, wherein, if the conductive layer comprises a low-resistance metal such as tungsten, aluminum or copper, an etch-back process is performed to partially remove the conductive layer and dielectric layer filling each trench 105, thereby forming the gate dielectric layer 191 and the gate electrode layer 193, and then forming a capping layer 210 on the gate structure 190 to fill each trench 105.
[0078] Through these processes, a semiconductor device 300 according to a preferred embodiment of the present invention is obtained, which includes multiple gate lines (i.e., gate structure 190) respectively embedded in a plurality of fins 110 and shallow trench isolation 150 to perform as buried gate lines. Furthermore, in obtaining... Figure 9-11 Following the structure shown, multiple wires (not shown) and at least one capacitor (not shown) can be further formed on the top surface of the multiple fins 110. The semiconductor device 300 can thus function as a memory device similar to a dynamic random access memory (DRAM) device, where each gate structure 190 functions similarly to a word line (WL) and each wire functions similarly to a bit line (BL) for receiving and transmitting signals in the DRAM array during operation. However, in another embodiment, other active elements can also be formed on the multiple fins 110 in subsequent processes, allowing the semiconductor device 300 to perform various functions or properties as other semiconductor memory devices.
[0079] Further reference Figure 11 According to a preferred embodiment of the present invention, the semiconductor device 300 includes at least one trench 105 passing through a plurality of fins 110 and a shallow trench isolation 150, and at least one gate line (i.e., gate structure 190) buried in the bottom of the at least one trench 105 to cross the plurality of fins 115 and the shallow trench isolation 155 at a reduced height. Figure 11As shown in the cross-sectional view, multiple fins 110 are disposed on both sides of multiple fins 115, and the multiple fins 110 and 115 are surrounded by shallow trench isolation 150. The maximum height H2 of the multiple fins 110 is greater than the maximum height H1 of the multiple fins 115. More precisely, the at least one gate line includes a gate dielectric layer 191 and a gate electrode layer 193 stacked from bottom to top, wherein the gate dielectric layer 191 is disposed between the multiple fins 115 and the gate electrode layer 193, and the gate dielectric layer 191 may include... Figure 11 The cross-sectional view shows a U-shaped structure. Furthermore, the semiconductor device 300 includes a stress layer 130 disposed on the side surfaces of a plurality of fins 115 and on the top surface 101 of the substrate 100. The stress layer 130 preferably comprises a germanium-containing layer, which can generate appropriate stress and a better lattice structure, and the germanium-containing layer preferably comprises a material different from the substrate 100, such as germanium, silicon-germanium, etc. In this way, the channel of at least one gate line can thus obtain appropriate stress and a better lattice structure, thereby improving the electron mobility and performance of the drive current. Furthermore, as... Figure 11 As shown, stress layer 130 is also provided on the top surface and side surface of the plurality of fins 110, because the formation of stress layer 130 takes precedence over the formation of shallow trench isolation 150, and the germanium concentration in stress layer 130 can vary depending on the distribution portion, for example, having a relatively low concentration in the upper part and a relatively high concentration in the bottom part or no residue.
[0080] Furthermore, the semiconductor device 300 also includes an oxide layer 170, which is formed by simultaneously consuming the exposed surfaces beneath it, such as the stress layer 130 or the exposed surfaces of the plurality of fins 110, 115. Therefore, a portion of the oxide layer 171 may also comprise germanium, and it is disposed on the side surfaces of the plurality of fins 115 and the top surface of the plurality of fins 110 to have, for example, Figure 11 The L-shaped structure is shown. Alternatively, another portion of the oxide layer 173 may also comprise silicon, and it is disposed on the topmost surface of the plurality of fins 115 (also referred to as the bottom wall of the trench 105) and the sidewalls of the trench 105 to form a U-shaped structure between the gate structure 190 and the plurality of fins 110, 115 within each trench 105, as shown. Figure 10-11 As shown. In this way, different portions of the oxide layer 170 (i.e., the portion of oxide layer 171 and the other portion of oxide layer 173) may include different materials and different thicknesses T2, T3. In one embodiment, a portion of oxide layer 171 may include silicon-germanium oxide or germanium oxide, and the other portion of oxide layer 173 may include, but is not limited to, silicon oxide.
[0081] Those skilled in the art will readily recognize that the semiconductor device and its formation method in this invention are not limited to the embodiments described above, and may include other examples or variations. The following specification will describe in detail different embodiments of the semiconductor device and its formation method in this invention. For the sake of simplicity, the following specification will detail the differences between different embodiments, while identical features will not be repeated. To facilitate comparison of the differences between embodiments, identical components in each of the following embodiments are labeled with the same symbols.
[0082] Please refer to Figure 12-13 This illustrates a method for forming a semiconductor device according to a second preferred embodiment of the present invention. The preceding steps of this embodiment are substantially the same as those of the preceding steps of the aforementioned first preferred embodiment, and will not be repeated here. The difference between the aforementioned first preferred embodiment and this embodiment is that, in this embodiment, a portion of the shallow trench isolation 150a includes a three-layer structure, wherein the three-layer structure includes an oxide layer 152, a first isolation layer 151, and a second isolation layer 153. Figure 12 As shown, the oxide layer 152 is formed by an ALD process or an ISSG process, and at least a portion of the elements (e.g., germanium, silicon-germanium) within the stress layer 130 are consumed and oxidized to form the oxide layer 152 (e.g., including germanium, silicon-germanium). Subsequently, trenches 105 are formed by partially removing multiple fins 110 and shallow trench isolation 150a (including oxide layer 152, first isolation layer 151, and second isolation layer 153), thereby forming a structure as shown in the diagram. Figure 13 The diagram shows multiple fins 115 with reduced height and shallow groove isolation 155a. Then, similar to the aforementioned first preferred embodiment... Figure 7-11 An oxide layer 170 and a gate structure 190 can be further formed in subsequent processes to span multiple fins 115. However, in another embodiment, the oxide layer 152 and the isolation layers (including a first isolation layer 151 and a second isolation layer 153) can have different etch degrees when forming the trench 105, thus forming multiple fins 115 and shallow trench isolation 155b, wherein the oxide layer 152 remains on the entire side surface of the multiple fins 155 to allow for... Figure 14 The topmost surface portions of the first isolation layer 151 and the second isolation layer 153 shown protrude. In another embodiment, an oxide layer (not shown) formed in a subsequent oxidation process may be disposed on an oxide layer 152, which protrudes from the topmost surface of the first isolation layer 151 and the second isolation layer 153 and may optionally be bonded to the oxide layer 152.
[0083] Therefore, the semiconductor device formed in this embodiment includes a germanium-containing layer (e.g., stress layer 130, oxide layer 171, or oxide layer 152) disposed on the side surfaces of the plurality of fins 115 to provide appropriate stress and improved lattice structure to the channel. This allows the semiconductor device of this embodiment to achieve greater electron mobility, resulting in better functionality and performance.
[0084] Please refer to Figure 15 This illustrates a method for forming a semiconductor device 500 according to a third preferred embodiment of the present invention. The preceding steps of this embodiment are substantially the same as those of the preceding steps of the aforementioned first preferred embodiment, and will not be repeated here. The difference between the aforementioned first preferred embodiment and this embodiment is that in this embodiment, a portion of the oxide layer 171a is formed by completely consuming and oxidizing the underlying stress layer 130, thereby obtaining a thicker T4. Therefore, as... Figure 15 As shown, the oxide layer 170a in this embodiment includes a first portion (i.e., oxide layer 173) directly disposed on the topmost surface of the plurality of fins 115 and a second portion (i.e., oxide layer 171a) directly disposed on the side surfaces of the plurality of fins 115, wherein the first portion 173 and the second portion 171a respectively comprise different materials and thicknesses T3 and T4. In this embodiment, the first portion 173 includes, for example, silicon oxide, and the second portion 171a includes, for example, germanium oxide or silicon oxide, but is not limited thereto. Subsequently, a gate electrode layer 193 is formed to fill the bottom of the trench 105, and then a capping layer 210 is formed on the gate electrode layer 193 to fill the remaining portion of the trench 105. Then, the gate electrode layer 193 and the oxide layer 170a can be formed together to form the gate structure 190a. In other words, the gate dielectric layer 191 of the aforementioned first preferred embodiment is omitted in this embodiment, and the oxide layer 170a formed in this embodiment is disposed between the gate electrode layer 193 and the plurality of fins 115, and can serve as the gate dielectric layer of the gate structure 190a.
[0085] Therefore, the semiconductor device 500 formed in this embodiment also includes a germanium-containing layer (e.g., oxide layer 171a), which is disposed on the side surfaces of the plurality of fins 115 to provide appropriate stress and improved lattice structure to the channel. This allows the semiconductor device 500 of this embodiment to achieve greater electron mobility and better functionality and performance.
[0086] In general, the semiconductor device of the present invention includes a germanium-containing layer disposed on the side surfaces of a plurality of fins, and a gate line crossing the plurality of fins, wherein the germanium-containing layer provides appropriate stress and a preferred lattice structure to its channel. The germanium-containing layer includes, for example, germanium, silicon germanium, and germanium oxide (GeO). x ), silicon germanium oxide (SiGeO) x(or other suitable materials) thus enable the semiconductor device of the present invention to achieve greater electron mobility, thereby achieving better functionality and performance.
[0087] The above description is merely a preferred embodiment of the present invention and is not intended to limit the invention. Various modifications and variations can be made to the present invention by those skilled in the art. Any modifications, equivalent substitutions, improvements, etc., made within the spirit and principles of the present invention should be included within the scope of protection of the present invention.
Claims
1. A semiconductor device, comprising: The substrate includes a plurality of first height fins and a plurality of second height fins projecting in a direction away from the substrate, wherein the first height fins and the second height fins have different heights; A groove is located within the first height fin, and the bottom of the groove defines the top of the second height fin; A gate line is located above the second height fin and in contact with the first sidewall of the first height fin; A stress layer, the material of which is different from that of the first height fin and covers the second sidewall of the first height fin; wherein the first sidewall of the first height fin is disposed on the side adjacent to the second height fin, and the second sidewall of the first height fin is disposed on the other side away from the second height fin.
2. The semiconductor device of claim 1, further comprising an oxide layer located between the gate line and the plurality of second height fins, wherein the oxide layer comprises a first portion and a second portion, the first portion being disposed on the topmost surface of the plurality of second height fins, and the second portion being disposed on the side surfaces of the plurality of second height fins.
3. The semiconductor device of claim 2, wherein the first portion and the second portion comprise different materials.
4. The semiconductor device of claim 2, wherein a portion of the stress layer covers the side surface of the second height fin and is in direct contact with a second portion of the oxide layer.
5. The semiconductor device of claim 2, wherein the second portion comprises the same elements as the stress layer.
6. The semiconductor device of claim 1, wherein the maximum height of the plurality of first height fins is greater than the maximum height of the plurality of second height fins.
7. The semiconductor device of claim 1, further comprising shallow trench isolation surrounding the plurality of first height fins and the plurality of second height fins.
8. The semiconductor device of claim 1, wherein the stress layer comprises silicon germanium or germanium.
Citation Information
Patent Citations
Preparation for dual layer polycrystalline silicon self aligning grid structure
CN101459133A
Semiconductor device and preparation method thereof, and electronic device
CN106505039A