A method for thinning and cleaning ultra-thin flexible glass
By spraying and ultrasonic cleaning with mixed solutions of hydrofluoric acid, acetic acid and sulfuric acid and mixed solutions of xylene and ethanol during the glass thinning process, the problem of alkali metal salt residue affecting glass performance is solved, and better results are achieved Supports glass cleaning effect and chemical tempering process.
Patent Information
- Application Number
- CN202311795516.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-25
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2043-12-25
AI Technical Summary
During the process of glass thinning, alkali metal salt remains in the glass cracks and affects the glass performance and hinders the progress of the chemical tempering process.
The glass is sprayed and thinned with a mixed solution of hydrofluoric acid, acetic acid and sulfuric acid, followed by spraying and washing with a mixed solution of xylene, ethanol and water. Finally, through ultrasonic cleaning and air-drying steps, the glass is used in solution 2. The benzene ring structure adsorbs metal salt impurities and cleans the glass surface.
It effectively reduces the metal salt residue in the glass surface and cracks, improves the performance of flexible glass, promotes the progress of chemical tempering processes, and avoids warping caused by insufficient thinning thickness.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of glass processing, and in particular to a method for thinning and cleaning ultra-thin flexible glass. Background Art
[0002] Float glass has high flatness, good surface quality and can be mass-produced. It is welcomed by various industries. With the birth of Willow glass in the United States, domestic and foreign countries have also begun to try to use float method to produce flexible glass. Flexible glass refers to glass below 0.1mm, which has the advantages of good flexibility, high hardness, and stable chemical properties. At present, the float method produces flexible glass by chemical thinning of the finished glass, and the thickness of the glass can reach less than 0.1mm. The chemical thinning method uses HF to react with SiO2 to generate SiF4 gas and H2O, which destroys the skeleton of the glass and achieves glass thinning. However, there are tiny cracks on the surface of the glass, and the thickness of chemical thinning is not necessarily greater than the depth of the micro-cracks. The glass generates insoluble sodium and potassium alkali metal salts under the action of etching solution. These products may remain in the cracks of the glass, which will make the pressure on the upper and lower surfaces of the glass different, and will prevent K from being formed during the chemical tempering process. + 、Na + The exchange of ions further increases the pressure difference between the upper and lower surfaces of the glass, causing warping and seriously affecting the performance of the glass. The thinner the glass, the greater the impact of alkali metal salt residue on the performance of the flexible glass, and it is also not conducive to the chemical tempering process of the flexible glass. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a method for thinning and cleaning ultra-thin flexible glass, so as to solve the problem in the related technology of glass thinning that the residual alkali metal salt in the glass cracks affects the glass performance and is not conducive to the chemical tempering process.
[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for thinning and cleaning ultra-thin flexible glass, comprising the following steps:
[0005] Step 1: adding water to hydrofluoric acid, acetic acid and sulfuric acid in a certain proportion to obtain a solution 1, and using the solution 1 to thin the original glass sheet in a top spraying manner to obtain a thinned glass;
[0006] Step 2, mixing xylene, ethanol and water in a certain proportion to obtain solution 2;
[0007] Step 3, spraying the thinned glass with solution 2, and then washing with water;
[0008] Step 4: ultrasonically clean the glass obtained in step 3 and then air-dry it.
[0009] In a preferred solution, in step 1, the thickness of the original glass is 0.35-0.45 mm, and after the original glass is coated and attached to the back plate with tape, the original glass is sprayed with a solution to reduce its thickness.
[0010] In a preferred embodiment, in step one, the components of solution one are mixed by weight: 5 to 10 parts of hydrofluoric acid, 15 to 20 parts of acetic acid, 20 to 28 parts of sulfuric acid, and 40 to 50 parts of water.
[0011] In a preferred embodiment, in step 1, the temperature of solution 1 is 50-60° C., and the thinning time is 0.5-5 h.
[0012] In a preferred embodiment, in step 2, the components of solution 2 are mixed by weight: 1 to 5 parts of xylene, 70 to 80 parts of ethanol, and 20 to 25 parts of water.
[0013] In a preferred embodiment, in step three, the spraying temperature of solution 2 is 30-40° C., and the spraying time is 5-10 min.
[0014] In a preferred embodiment, in step 3, the water washing temperature is 25-30°C and the water washing time is 25-35s.
[0015] In a preferred embodiment, in step 4, the ultrasonic cleaning time is 1 to 5 minutes.
[0016] In a preferred solution, in step 4, the glass after ultrasonic cleaning is blown dry with an air knife, and then the tape is cut with a knife to peel off the back plate.
[0017] The present invention provides a method for thinning and cleaning ultra-thin flexible glass, which has the following beneficial effects:
[0018] 1. This method uses solution 2 for spray cleaning. Since solution 2 contains a benzene ring structure with strong metal adsorption capacity, it can adsorb metal salt impurities left in tiny cracks after thinning, reduce the impact of impurities on the performance of flexible glass, and is beneficial to the chemical tempering process. At the same time, it can further clean the dust on the glass surface.
[0019] 2. It avoids the metal salt impurities remaining in the cracks due to insufficient glass thinning, thus affecting the properties of the flexible glass. DETAILED DESCRIPTION
[0020] Embodiment 1:
[0021] A method for thinning and cleaning ultra-thin flexible glass, comprising the following steps:
[0022] Step 1: Lay a 0.40mm thick glass sheet to be thinned on the back plate with tape. Mix hydrofluoric acid, acetic acid and sulfuric acid with water in a certain proportion to obtain solution 1, and use top spraying to thin the original glass with solution 1 to obtain thinned glass.
[0023] In this embodiment, the components of solution 1 are mixed by weight: 5 parts of hydrofluoric acid, 20 parts of acetic acid, 25 parts of sulfuric acid, and 45 parts of water. The temperature of solution 1 is 50° C., and the thinning time is 0.5 h.
[0024] The original glass is thinned with a solution using a top spray method.
[0025] Step 2: Mix xylene, ethanol and water in a certain proportion to obtain solution 2.
[0026] In this embodiment, the components of solution 2 are mixed by weight: 2 parts of xylene, 75 parts of ethanol, and 23 parts of water.
[0027] Step 3: After spraying the thinned glass with Solution 2, set the spray temperature to 35°C and the spray time to 7 minutes to adsorb the metal salts remaining in the smile cracks and further clean the impurities on the surface of the flexible glass.
[0028] After spraying, wash with water at a temperature of 25°C for 30 seconds until the glass surface is clean and free of residue.
[0029] Step 4: ultrasonically clean the glass obtained in step 3 and then air-dry it.
[0030] The ultrasonic cleaning time is 2 minutes. The glass after ultrasonic cleaning is blown dry with an air knife, and then the tape is cut with a knife to peel off the back plate.
[0031] Embodiment 2:
[0032] Step 1: Lay a 0.40mm thick glass sheet to be thinned on the back plate with tape. Mix hydrofluoric acid, acetic acid and sulfuric acid with water in a certain proportion to obtain solution 1, and use top spraying to thin the original glass with solution 1 to obtain thinned glass.
[0033] In this embodiment, the components of solution 1 are mixed by weight: 5 parts of hydrofluoric acid, 20 parts of acetic acid, 25 parts of sulfuric acid, and 45 parts of water. The temperature of solution 1 is 50° C., and the thinning time is 0.5 h.
[0034] The original glass is thinned with a solution using a top spray method.
[0035] Step 2: Mix xylene, ethanol and water in a certain proportion to obtain solution 2.
[0036] In this embodiment, the components of solution 2 are mixed by weight: 1 part of xylene, 75 parts of ethanol, and 24 parts of water.
[0037] Step 3: After spraying the thinned glass with Solution 2, set the spray temperature to 35°C and the spray time to 7 minutes to adsorb the metal salts remaining in the smile cracks and further clean the impurities on the surface of the flexible glass.
[0038] After spraying, wash with water at a temperature of 25°C for 30 seconds until the glass surface is clean and free of residue.
[0039] Step 4: ultrasonically clean the glass obtained in step 3 and then air-dry it.
[0040] The ultrasonic cleaning time is 2 minutes. The glass after ultrasonic cleaning is blown dry with an air knife, and then the tape is cut with a knife to peel off the back plate.
[0041] Embodiment 3:
[0042] Step 1: Lay a 0.40mm thick glass sheet to be thinned on the back plate with tape. Mix hydrofluoric acid, acetic acid and sulfuric acid with water in a certain proportion to obtain solution 1, and use top spraying to thin the original glass with solution 1 to obtain thinned glass.
[0043] In this embodiment, the components of solution 1 are mixed by weight: 5 parts of hydrofluoric acid, 20 parts of acetic acid, 25 parts of sulfuric acid, and 45 parts of water. The temperature of solution 1 is 50° C., and the thinning time is 0.5 h.
[0044] The original glass is thinned with a solution using a top spray method.
[0045] Step 2: Mix xylene, ethanol and water in a certain proportion to obtain solution 2.
[0046] In this embodiment, the components of solution 2 are mixed by weight: 5 parts of xylene, 75 parts of ethanol, and 20 parts of water.
[0047] Step 3: After spraying the thinned glass with Solution 2, set the spray temperature to 35°C and the spray time to 7 minutes to adsorb the metal salts remaining in the smile cracks and further clean the impurities on the surface of the flexible glass.
[0048] After spraying, wash with water at a temperature of 25°C for 30 seconds until the glass surface is clean and free of residue.
[0049] Step 4: ultrasonically clean the glass obtained in step 3 and then air-dry it.
[0050] The ultrasonic cleaning time is 2 minutes. The glass after ultrasonic cleaning is blown dry with an air knife, and then the tape is cut with a knife to peel off the back plate.
[0051] Comparative Example 1:
[0052] The difference between this comparative example and Example 1 is that xylene and ethanol are not added to Solution 2, and other preparation methods and steps are the same as those in Example 1, which will not be repeated here.
[0053] Comparative Example 2:
[0054] The difference between this comparative example and Example 1 is that xylene is not added to Solution 2, and other preparation methods and steps are the same as those in Example 1, which will not be repeated here.
[0055] After spraying the thinned glass with Solution 2, the sprayed solution was sampled and the concentrations of sodium and potassium in the solution were tested using ICP-OES. The higher the concentrations of sodium and potassium in the tested solution, the better the adsorption effect of Solution 2 on metal residues, and the better the effect of reducing metal residues in glass cracks.
[0056] Ultra-thin flexible glass prepared by different methods was used to test the warping of the glass. The smaller the warping, the better the quality of the prepared glass and the improved the glass performance.
[0057]
[0058] In Table 1, G1 represents the glass prepared in Example 1, G2 represents the glass prepared in Example 2, G3 represents the glass prepared in Example 3, and D1 and D2 represent the glasses prepared in Comparative Example 1 and Comparative Example 2, respectively.
[0059] From the data in Table 1, it can be seen that this method can utilize the adsorption capacity of benzene ring structure for metal ions to reduce glass microcracks and metal residues on the surface. At the same time, ethanol can further clean impurities on the glass surface, greatly improving the performance of flexible glass, which is beneficial to the glass chemical tempering process. The operation is simple and can avoid warping caused by different thinning thicknesses.
Claims
1. A method for thinning and cleaning ultra-thin flexible glass, characterized in that: The steps include: Step 1: adding water to hydrofluoric acid, acetic acid and sulfuric acid in a certain proportion to obtain a solution 1, and using the solution 1 to thin the original glass in a top spraying manner to obtain a thinned glass; Step 2: xylene, ethanol and water are mixed in a certain proportion to obtain solution 2, wherein the components of solution 2 are mixed by weight: 1-5 parts of xylene, 70-80 parts of ethanol, and 20-25 parts of water; Step 3, spraying the thinned glass with solution 2, and then washing with water; Step 4: ultrasonically clean the glass obtained in step 3 and then air-dry it.
2. The method for thinning and cleaning ultra-thin flexible glass according to claim 1, characterized in that: In the step 1, the thickness of the original glass is 0.35-0.45 mm. After the original glass is coated, it is attached to the back plate with a tape, and then the original glass is sprayed with a solution to be thinned.
3. The method for thinning and cleaning ultra-thin flexible glass according to claim 1, characterized in that: In step 1, the components of solution 1 are mixed by weight: 5-10 parts of hydrofluoric acid, 15-20 parts of acetic acid, 20-28 parts of sulfuric acid, and 40-50 parts of water.
4. The method for thinning and cleaning ultra-thin flexible glass according to claim 1, characterized in that: In the step 1, the temperature of solution 1 is 50-60° C., and the thinning time is 0.5-5 h.
5. The method for thinning and cleaning ultra-thin flexible glass according to claim 1, characterized in that: In the step 3, the spraying temperature of solution 2 is 30-40° C., and the spraying time is 5-10 min.
6. The method for thinning and cleaning ultra-thin flexible glass according to claim 1, characterized in that: In the step 3, the water washing temperature is 25-30°C and the water washing time is 25-35s.
7. The method for thinning and cleaning ultra-thin flexible glass according to claim 1, characterized in that: In the step 4, the ultrasonic cleaning time is 1 to 5 minutes.
8. The method for thinning and cleaning ultra-thin flexible glass according to claim 1, characterized in that: In the step 4, the glass after ultrasonic cleaning is blown dry with an air knife, and then the tape is cut with a knife to peel off the back plate.