Design and fabrication method of high-pressure temperature-controlled fusing alloy for hydrogen valve

By preparing tin-based alloy materials, the problems of complex preparation, easy contamination, and low strength of existing safety valve core materials are solved. This provides safe and reliable pressure relief protection for hydrogen storage tanks under high pressure, and achieves simple and easy alloy preparation and high-efficiency safety performance.

CN117737538BActive Publication Date: 2026-11-10ZHEJIANG COLLEGE OF ZHEJIANG UNIV OF TECHOLOGY +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311777248.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-22
Publication Date
2026-11-10
Estimated Expiration
2043-12-22

AI Technical Summary

Technical Problem

Existing safety valves have problems with valve core materials, such as complex manufacturing processes, susceptibility to contamination, low strength, and melting points that do not meet the safety requirements of hydrogen storage tanks, making it difficult to protect the safety of hydrogen storage tanks under 70MPa pressure.

Method used

A high-pressure temperature-controlled fusing alloy for hydrogen valves is prepared using alloy materials of tin, indium, additive elements, antimony, molybdenum, lead, copper, and nickel through vacuum melting, filtration casting, and cooling and forming of hardened brittle materials. This ensures that the alloy has a melting point of 110±5℃ and a compressive strength greater than 70MPa.

Benefits of technology

It achieves safe and reliable pressure relief protection for hydrogen storage tanks under high pressure. The alloy preparation process is simple and pollution-free, making it suitable for widespread application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117737538B_ABST
    Figure CN117737538B_ABST
Patent Text Reader

Abstract

This invention belongs to the field of tin alloy technology, specifically relating to the design and preparation method of a high-pressure temperature-controlled fusing alloy for hydrogen valves, comprising the following raw material components: tin, indium, additive elements, antimony, molybdenum, lead, copper, and nickel; the mass percentages of each raw material component are 44.56%–45.52% tin, 50.44%–51.48% indium, 1%–3% additive elements, 0.5%–0.8% antimony, 0.32%–0.54% molybdenum, 0.2%–0.4% lead, 0.15%–0.29% copper, and 0.3%–0.5% nickel. The hydrogen valve high-pressure temperature-controlled fusing alloy disclosed in this invention has a small melting range. When applied to the valve core of a hydrogen storage tank safety valve, it can melt and release pressure in a timely manner when the external environment is too high, protecting the safety of the hydrogen storage tank. Furthermore, the hydrogen valve high-pressure temperature-controlled fusing alloy has high compressive strength, ensuring that the hydrogen storage tank does not leak under working pressure. The preparation method of the hydrogen valve high-pressure temperature-controlled fusing alloy disclosed in this application is simple and easy to operate, and the preparation process is pollution-free, making it suitable for widespread application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of tin alloy technology, specifically relating to the design and preparation method of a high-pressure temperature-controlled fusion alloy for hydrogen valves. Background Technology

[0002] The safety valve in the hydrogen storage cylinder is one of the key components of the entire on-board high-pressure hydrogen storage system. It plays a crucial role in protecting the hydrogen storage cylinder from overpressure. The safety valve contains a temperature control element, which is usually made of a low-melting-point alloy. The safety requirements of the 70MPa on-board hydrogen storage system place higher demands on the performance of the safety valve. It must be able to melt the valve core when the rated ambient temperature reaches 110±5℃ or break instantly when the pressure exceeds 70MPa (maximum allowable pressure 87.5MPa), allowing the hydrogen storage tank to quickly depressurize and prevent the hydrogen from exploding due to overheating or overpressure.

[0003] The valve core materials in existing safety valves have the following drawbacks: First, the existing low-melting-point alloy materials are complex to prepare, difficult to operate, and prone to contamination during preparation. Second, existing research on low-melting-point alloy materials mainly focuses on lead-based and tin-based solders with a melting point of 140–230℃, while the melting point of tin-indium eutectic alloy is 119℃, which cannot fully meet the safety requirements of hydrogen storage tanks. Third, the existing low-melting-point alloy materials have low strength, generally not exceeding 50MPa, which cannot ensure that the hydrogen storage tank does not leak under working pressure and is therefore ineffective in providing protection.

[0004] Therefore, this invention is proposed. Summary of the Invention

[0005] To address the technical problems existing in the prior art, this invention provides a design and preparation method for a high-pressure temperature-controlled fusion alloy for hydrogen valves.

[0006] To achieve the above objectives, the present invention adopts the following technical solution: a design and preparation method for a high-pressure temperature-controlled fusion alloy for hydrogen valves, comprising the following raw material components: tin, indium, additive elements, antimony, molybdenum, lead, copper, and nickel; the mass percentages of each of the raw material components are 44.56%–45.52% tin, 50.44%–51.48% indium, 1%–3% additive elements, 0.5%–0.8% antimony, 0.32%–0.54% molybdenum, 0.2%–0.4% lead, 0.15%–0.29% copper, and 0.3%–0.5% nickel.

[0007] The added element is either bismuth or zinc.

[0008] The mass percentages of each of the raw material components are 45.52% tin, 51.48% indium, 1% added elements, 0.6% antimony, 0.4% molybdenum, 0.3% lead, 0.2% copper and 0.5% nickel.

[0009] A method for preparing a high-pressure temperature-controlled fusing alloy for a hydrogen valve includes the following steps:

[0010] (1) Prepare materials

[0011] Weigh out the raw material components for preparing the high-pressure temperature control fuse alloy for hydrogen valves according to their respective mass percentages;

[0012] (2) Mixed smelting

[0013] The raw material components weighed in step (1) are placed in a vacuum melting furnace for mixing and melting to form a liquid alloy;

[0014] (3) Filtration and casting

[0015] The liquid alloy in step (2) is filtered and then cast.

[0016] (4) Hardened and brittle materials are cooled and molded.

[0017] During the casting process in step (2), a hardened and brittle material is cooled and shaped to obtain a cylindrical alloy ingot;

[0018] (5) Processing alloy ingots

[0019] The cylindrical alloy ingot obtained in step (4) is processed according to the valve core material dimensions;

[0020] (6) Install valve core material

[0021] The alloy ingot processed in step (5) is loaded into the valve core material.

[0022] In step (1), the raw material components tin and indium are spherical structures with a diameter of 8 to 16 mm, while the other raw material components are blocky structures with a length, width, and height of 10 to 15 mm.

[0023] The purity of all raw material components in step (1) is ≥99.995%.

[0024] The specific steps of step (2) are as follows: the proportioned raw material components are put into a high-frequency vacuum melting furnace. When bismuth is selected as the added element, the vacuum furnace is heated to 300-350°C; when zinc is selected as the added element, the vacuum furnace is heated to 450-500°C. The vacuum degree inside the furnace is 0.1 Pa. After the materials are fully stirred and melted by electromagnetic stirring, the furnace is kept warm for 20-30 minutes. During the furnace cooling process, the electromagnetic stirring is started intermittently, that is, the electromagnetic stirring is started once every 10 minutes, and each stirring lasts for 4 minutes.

[0025] The specific steps of step (3) are as follows: remove the surface slag from the liquid alloy, reduce the temperature to 200°C, filter it with foamed alumina, and then cast the liquid alloy into the mold after filtration.

[0026] The specific steps of step (4) are as follows: several hard and brittle materials are placed into the liquid alloy with a cross section perpendicular to the mold. The hard and brittle materials are used as brittle fracture supports. After cooling to room temperature, the resulting cylindrical alloy ingot is taken out.

[0027] The specific steps of step (5) are as follows: using an angle grinder and machining equipment, the cooled cylindrical alloy ingot is processed according to the shape and size of the valve core material.

[0028] The beneficial effects of this invention are as follows:

[0029] The high-pressure temperature-controlled fusing alloy for hydrogen valves disclosed in this application has a small melting range. When applied to the valve core of a safety valve for a hydrogen storage tank, it can melt and release pressure in a timely manner when the external environment is too hot, protecting the safety of the hydrogen storage tank. Furthermore, the high-pressure temperature-controlled fusing alloy for hydrogen valves has high compressive strength, ensuring that the hydrogen storage tank does not leak under operating pressure. The preparation method of the high-pressure temperature-controlled fusing alloy for hydrogen valves disclosed in this application is simple and easy to operate, and the preparation process is pollution-free, making it suitable for widespread application. Attached Figure Description

[0030] Figure 1 This is a flowchart of the method of the present invention;

[0031] Figure 2 This is a graph showing the alloy melting temperature of the high-pressure temperature-controlled melting alloy in Example 1, obtained from DSC testing.

[0032] Figure 3 This is a graph showing the alloy melting temperature of the high-pressure temperature-controlled melting alloy in Example 2, obtained from DSC testing.

[0033] Figure 4 The compressive stress-strain diagram of the high-pressure temperature control fusible alloy of the hydrogen valve in Example 1 is shown.

[0034] Figure 5 This is a compressive stress-strain diagram of the high-pressure temperature-controlled fusion alloy of the hydrogen valve in Example 2. Detailed Implementation

[0035] The technical solutions of the embodiments of the present invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0036] See Figure 1-5 The present invention proposes the following technical solution:

[0037] Example 1

[0038] A high-pressure temperature-controlled fusing alloy for hydrogen valves comprises the following raw material components: tin, indium, additive elements, antimony, molybdenum, lead, copper, and nickel; the mass percentages of each raw material component are: 45.52% tin, 51.48% indium, 1% additive elements, 0.6% antimony, 0.4% molybdenum, 0.3% lead, 0.2% copper, and 0.5% nickel, with bismuth as the additive element.

[0039] A method for preparing a high-pressure temperature-controlled melting alloy for a hydrogen valve includes the following steps: (1) preparing materials; (2) mixing and melting; (3) filtering and casting; (4) adding hardened and brittle materials and cooling and shaping; (5) processing the alloy ingot; and (6) installing it into a hydrogen valve.

[0040] In step (1) above, the tin and indium in the raw material components are spherical raw materials with a diameter of 8 to 16 mm, and the other raw material components are blocky raw materials with a length, width and height between 10 and 15 mm, and the purity of all raw material components is ≥99.995%.

[0041] In step (2) above, the above raw material components are proportioned and then put into a high-frequency vacuum melting furnace. When bismuth is selected as the added element, the vacuum furnace is heated to 300-350°C; when zinc is selected as the added element, the vacuum furnace is heated to 450-500°C. The vacuum degree inside the furnace is 0.1 Pa. After the materials are fully stirred and melted by electromagnetic stirring, they are kept at the temperature for 20-30 minutes. During the furnace cooling process, electromagnetic stirring is started every 10 minutes, and each stirring lasts for 4 minutes.

[0042] In step (3) above, after removing the surface slag, a liquid alloy is obtained. The temperature is reduced to 200°C, and the liquid alloy is filtered using foamed alumina with a pore size of 80 mesh. After filtration, the liquid alloy is cast into a mold.

[0043] In step (4) above, the hard and brittle material is ceramic material, glass material, ceramic fiber or glass fiber, etc. Among them, the ceramic material can be a ceramic rod with a diameter of 4mm and a height of 80mm. The cross section is placed in the liquid alloy with the cross section perpendicular to the mold. The ceramic rod is used as a brittle fracture support. After cooling to room temperature, the cylindrical alloy ingot is taken out. The diameter of the alloy ingot is 20mm and the height is 100mm.

[0044] In step (5) above, the alloy ingot is processed according to the valve core material (required shape) size. The cooled alloy ingot is cut according to the valve core material, i.e. the shape and size of the hydrogen valve, using an angle grinder and machining. The diameter of the cut valve core alloy is 10mm and the height is 25mm.

[0045] In step (6) above, the processed alloy ingot is loaded into the hydrogen valve.

[0046] Alloy ingot X1: (Sn52In)1Bi was prepared. After removing the zirconium oxide portion, the melting temperature range of alloy ingot X1 was found to be 113.8~115.2℃ by DSC test, and the compressive strength of alloy ingot X1 at brittle fracture was found to be 86.06MPa by WDW test.

[0047] Example 2

[0048] A high-pressure temperature-controlled fusing alloy for hydrogen valves comprises the following raw material components: tin, indium, additive elements, antimony, molybdenum, lead, copper, and nickel. The mass percentages of each raw material component are: 45.04% tin, 50.96% indium, 2% additive elements, 0.5% antimony, 0.32% molybdenum, 0.4% lead, 0.28% copper, and 0.5% nickel. The additive element is zinc. The preparation method is the same as in Example 1. The resulting alloy ingot Y1: (Sn52In)2Zn is obtained. After removing the zirconium oxide portion, the melting temperature range of alloy ingot Y1 is found to be 108.1–109.5 °C by DSC testing. The compressive strength of alloy ingot Y1 at brittle fracture is found to be 87.31 MPa by WDW testing.

[0049] The specific component ratios for each embodiment are shown in the table below:

[0050]

[0051]

[0052] The melting temperature range and brittle fracture compressive strength of the alloys in each embodiment are shown in the table below:

[0053] Example 1 Example 2 X1 Y1 Melting temperature range / °C 113.8~115.2 108.1~109.5 Brittle fracture compressive strength / MPa 86.06 87.31

[0054] Based on the above, the advantages of this invention are as follows: The high-pressure temperature-controlled fusing alloy (tin alloy) prepared by this invention for use in valve core materials has a compressive strength greater than 70 MPa, which can meet the normal use requirements of the safety valve of the hydrogen storage tank. It can be used for a long time under the condition of hydrogen pressure of 70 MPa. Moreover, the melting temperature range of this high-pressure temperature-controlled fusing alloy is within 110±5℃, which is extremely small. Once the external temperature is too high, the material will melt and release pressure in time, resulting in higher safety performance. At the same time, the preparation method is simple, pollution-free, easy to operate, and suitable for widespread promotion and use.

[0055] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No reference numerals in the claims should be construed as limiting the scope of the claims.

Claims

1. A method for preparing a high-pressure temperature-controlled fusing alloy for a hydrogen valve, characterized in that, Includes the following steps: (1) Prepare materials Weigh out the raw material components for preparing the high-pressure temperature control fuse alloy for hydrogen valves according to their respective mass percentages; (2) Mixed smelting The raw material components weighed in step (1) are placed in a vacuum melting furnace for mixing and melting to form a liquid alloy; (3) Filtration and casting The liquid alloy in step (2) is filtered and then cast. (4) Add hard and brittle materials and cool to form During the casting process in step (3), a hardened and brittle material is cooled and shaped to obtain a cylindrical alloy ingot; (5) Processing alloy ingots The cylindrical alloy ingot obtained in step (4) is processed according to the valve core material dimensions; (6) Fill the valve core material The alloy ingot processed in step (5) is loaded into the valve core material; The high-pressure temperature-controlled fusion alloy for the hydrogen valve comprises the following raw material components: tin, indium, additives, antimony, molybdenum, lead, copper, and nickel; the mass percentages of each raw material component are 44.56%–45.52% tin, 50.44%–51.48% indium, 1%–3% additives, 0.5%–0.8% antimony, 0.32%–0.54% molybdenum, 0.2%–0.4% lead, 0.15%–0.29% copper, and 0.3%–0.5% nickel; the additives are either bismuth or zinc.

2. The method for preparing the high-pressure temperature-controlled fusing alloy for hydrogen valves as described in claim 1, characterized in that: The mass percentages of each of the raw material components are 45.52% tin, 51.48% indium, 1% added elements, 0.6% antimony, 0.4% molybdenum, 0.3% lead, 0.2% copper and 0.5% nickel.

3. The method for preparing the high-pressure temperature-controlled fusing alloy for the hydrogen valve as described in claim 1, characterized in that: In step (1), the raw material components tin and indium are spherical structures with a diameter of 8 to 16 mm, while the other raw material components are blocky structures with a length, width and height between 10 and 15 mm.

4. The method for preparing the high-pressure temperature-controlled fusing alloy for hydrogen valves as described in claim 1, characterized in that: The purity of all raw material components in step (1) is ≥99.995%.

5. The method for preparing the high-pressure temperature-controlled fusing alloy for the hydrogen valve as described in claim 1, characterized in that, The specific steps of step (2) are as follows: the proportioned raw material components are put into a high-frequency vacuum melting furnace. When bismuth is selected as the added element, the vacuum furnace is heated to 300-350°C; when zinc is selected as the added element, the vacuum furnace is heated to 450-500°C. The vacuum degree inside the furnace is 0.1 Pa. After the mixture is fully stirred and melted by electromagnetic stirring, it is kept at the temperature for 20-30 minutes. During the furnace cooling process, the electromagnetic stirring is started intermittently.

6. The method for preparing the high-pressure temperature-controlled fusing alloy for the hydrogen valve as described in claim 1, characterized in that, The specific steps of step (3) are as follows: remove the surface slag from the liquid alloy, reduce the temperature to 200°C, then filter it with foamed alumina, and then cast the liquid alloy into the mold after filtration.

7. The method for preparing the high-pressure temperature-controlled fusing alloy for the hydrogen valve as described in claim 1, characterized in that, The specific steps of step (4) are as follows: several hard and brittle materials are placed into the liquid alloy with a cross section perpendicular to the mold. The hard and brittle materials serve as a support for brittle fracture. After cooling to room temperature, the cylindrical alloy ingot is taken out.

8. The method for preparing the high-pressure temperature-controlled fusing alloy for the hydrogen valve as described in claim 1, characterized in that, The specific steps of step (5) are as follows: using an angle grinder and machining equipment, the cooled cylindrical alloy ingot is processed according to the shape and size of the valve core material.

Citation Information

Patent Citations

  • Lead-free low-temperature alloy having melting point of 116+ / -3 DEG C and preparation method for same

    CN103146975A

  • Fusible alloy preparation process suitable for 70MPa hydrogen safety valve

    CN114774735A

  • Alloy type thermal fuse and material for a thermal fuse element

    CN1503294A

  • Temperature fuse element, temperature fuse and battery using the same

    CN1795280A