A method for evaluating the performance of gel foam systems
By establishing a stacking index model and a Herschel-Bulkley rheological model, the stacking performance of gel foam was evaluated, which solved the problems of insufficient stability and plugging ability of gel foam in fractured-vuggy reservoirs, and achieved effective plugging and improved recovery in high-temperature and high-salinity reservoirs.
Patent Information
- Application Number
- CN202211115187.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2022-09-14
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2042-09-14
AI Technical Summary
In fractured-vuggy reservoirs, the stability and plugging ability of gel foam are insufficient, resulting in poor performance of foam flooding technology in high-temperature and high-salt environments, making it difficult to effectively plug large fractures and large cavities.
By establishing a packing index model and using the Herschel-Bulkley rheological model and shear stress analysis, the packing performance of gel foam was evaluated, and a gel foam system suitable for fractured-vuggy reservoirs was selected.
The ability of gel foam to plug in fractured-vuggy reservoirs was evaluated, guiding the field application of foam flooding technology in high-temperature, high-pressure, and high-salinity reservoirs and improving oil recovery.
Smart Images

Figure CN117740616B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of gel foam technology, and specifically to a method for evaluating the performance of gel foam systems. Background Technology
[0002] As oilfield development progresses, the remaining usable resources in conventional oil reservoirs are dwindling. To find alternative resources, oilfield workers have turned their attention to unconventional reservoirs. Fractured-vuggy carbonate oil and gas reservoirs, with their large scale and high reserves, have become a type of reservoir attracting significant attention worldwide. However, the discontinuous distribution of fractured-vuggy reservoirs, the large differences in the effective reservoir space scale between fractures and cavities, the complex internal structure and fracture-vuggy contact relationships, and the significant differences in oil-water distribution among different reservoir units all increase the difficulty of reservoir development. Early development relied on elastic and water-drive methods, but the displacement medium flowed along high-permeability channels, leading to severe formation energy depletion, a rapid increase in the water-oil ratio, and poor development results. Later gas injection development, while achieving some success, suffered from severe gas-liquid gravity separation and prominent gas channeling problems during gas injection, severely restricting the effective application of gas drive technology.
[0003] Foam is a compressible non-Newtonian fluid characterized by low leakage, low density, strong sand-carrying capacity, and minimal damage to oil-bearing reservoirs. In formations, it can both plug high-permeability layers and improve the sweep efficiency of low-permeability layers, and effectively seal water-bearing layers. In the exploration of enhanced oil recovery, foam flooding has attracted widespread attention from oilfield workers due to its unique seepage and oil displacement properties, making it a promising tertiary oil recovery method. However, foam systems exhibit poor stability under reservoir conditions. The presence of crude oil in the reservoir causes foam to easily collapse, resulting in weak sealing strength when used as a modifier. To address the problems existing in foam modifier flooding, there is an urgent need to develop a new technology that can both stably inject foam and effectively seal it.
[0004] Gel foam is a dispersion system in which gas is uniformly dispersed in a gel. It not only reduces the drainage rate of the liquid film but also, through the synergistic effect of the foaming agent, increases the impact resistance of the liquid film, thereby enhancing the stability of the foam. Before gelation, gel foam exists in foam form, preferentially entering the high-permeability layer and the aqueous layer; the Jamin effect can effectively block the aqueous layer. After gelation, it exists as gel foam, with the gel acting as the external phase, enhancing the foam's stability.
[0005] The Tarim River fractured-vuggy reservoir is characterized by high reservoir temperature and high formation water salinity, along with a complex reservoir structure containing numerous fractures and karst formations. Applying gel foam to this reservoir requires not only exceptional stability against high temperatures and salinity but also the ability to seal large fractures and karst formations. Therefore, the stability of the selected gel foam in this type of reservoir needs to be considered to determine its sealing capability within the formation. In other words, the performance of the selected gel foam during the sealing process must be taken into account to select a suitable gel foam for the complex formation environment. Summary of the Invention
[0006] The technical problem to be solved by the present invention is to consider the stability of the gel foam used in fractured-vuggy reservoirs, and thus to determine the sealing ability of the gel foam in the formation.
[0007] The technical solution adopted by this invention to solve its technical problem is:
[0008] A method for evaluating the performance of gel foam systems includes the following steps:
[0009] Step 1: Establish the packing index model, where the packing index is denoted as A. This packing index is the ratio of the height h of a unit mass of foam to the equivalent diameter d of the bottom surface under ideal conical foam packing conditions. The packing index is used to characterize the packing performance of gel foam. In this ideal state, half of the apex angle of the cone cross-section formed by the foam packing is θ. The method for obtaining the packing index A is as follows:
[0010] Based on the foam separation experiment, a time-considered model is established, and the relationship between the separation mass and the model is expressed by the following formula:
[0011]
[0012] Where m d (r) represents the cumulative mass (g) of the precipitate at time t, m max The value represents the maximum mass of the separated liquid (g), and t represents the separation time (s). denoted as 1 / 2 precipitation time (s), and b represents a parameter of the precipitation process;
[0013] When the gel foam is in equilibrium, the external forces acting on it in the longitudinal direction are gravity and the supporting force from the bottom surface. When the gel foam is at rest, the gravity acting on the entire gel foam is:
[0014] G=(m0-m d (t))g (2)
[0015] Where m0 is the total weight of the foam in its initial state before separation;
[0016] At this point, the gel foam is in equilibrium. The lateral component of the gravity acting on the gel foam at that point is equal to the static friction force on the bottom surface of the gel foam, and numerically replaced by the lateral shear stress on the gel foam at the shear rate measured in the laboratory:
[0017]
[0018] τ is the transverse shear stress (N);
[0019] Define the instantaneous average foaming ratio E(t) as:
[0020]
[0021] Where m s (t) refers to the mass (g) of foam liquid of the same volume as the foam at time t; m f (0) refers to the initial mass (g) of the foam;
[0022] The expression for the structural damage coefficient λ of the foam is as follows:
[0023]
[0024] Where E(0) is the initial foaming ratio;
[0025] Using the mass of the precipitate as an intermediate variable and assuming a constant shear rate, the relationship between the apparent viscosity of the foam and time was established as follows:
[0026] μ app (γ, t) = μ app (γ,0)Exp(1-(λ(t)) m (6)
[0027] Apparent viscosity is the ratio of transverse shear stress to shear rate. Using the Herschel-Bulkley rheological model, it is transformed into an apparent viscosity expression. Substituting this expression into formula (6), a time-corrected Herschel-Bulkley rheological model is derived, revealing the change in transverse shear stress at a given moment:
[0028] τ(γ, t)=(τ y +Kγ n )Exp(1-(λ(t)) m (7)
[0029] Where γ is the shear rate (s) -1 );τ y K, m, and n are all parameters that can be measured experimentally;
[0030] The centroid of the cone is located at 1 / 4 of its height along the central axis, and under ideal stacking conditions, θ = 30°. Based on the forces acting on the gel foam at different times and the law of similar triangles, and using formulas (3) and (7), the following can be obtained:
[0031]
[0032] The accumulation index A is obtained as follows:
[0033]
[0034] The parameter b is obtained as follows:
[0035] The initial mass m0, the final mass of the separated solution, and the half-separation time of the gel foam system. The measured value of the prepared semi-liquid gel and foaming agent mixture was obtained through experiments; this value is m. max After stirring and foaming, the total weight of the initial foam (without precipitate) is measured as m0. After time t, the precipitated liquid reaches half the total liquid volume before foaming; this time is t'. By measuring the mass of the precipitated liquid at different times t and fitting the data using formula (1), the parameter b can be obtained.
[0036] Parameter τ y The methods for deriving K, n, and n are as follows:
[0037] An experiment was conducted to test the change of apparent viscosity over time. Gel foam with a fixed initial foaming volume was selected for the experiment. It was assumed that the test time was short and the volume fraction of the foam liquid did not change. The changes in the size and shape of the foam were ignored, and thus the viscosity changes caused by time were ignored. The transverse shear stress of the gel foam at different shear rates was obtained by fitting the experimental values using the Herschel-Bulkley model. The transverse shear stress at different times and different shear rates was obtained by fitting the values using formula (7). The parameter τ can be obtained by fitting the values. y K, m, n;
[0038] The obtained parameters b and τ y Substituting K, m, and n into formula (9), we obtain the packing index A as a function of the shear rate γ;
[0039] Step 2: Provide the gel foam system to be evaluated;
[0040] Step 3: Based on the shear rate obtained in the experiment, the packing index A is obtained by formula (9). The larger the value of the packing index A, the better the packing performance of the gel foam system to be evaluated.
[0041] Preferably, in step two, the gel foam system to be evaluated is provided by the following method:
[0042] Step 1: Mix α-modified starch and acrylamide in a 1:1 mass ratio and stir evenly in deionized water to prepare polymer mother liquor;
[0043] Step 2: Add N,N-methylenebisacrylamide to the well-stirred solution and continue stirring for 10 minutes to ensure complete dissolution. Slowly add potassium persulfate initiator to a sealed container and place it in a 130°C high-temperature oven. After a period of time, it will form a gel.
[0044] Step 3: Transfer it to a mixer and stir at high speed for 1 minute to change the solid starch gel into a highly viscous semi-liquid state;
[0045] Step 4: Add tap water to the highly viscous semi-liquid and tap water in a volume ratio of 3:7, stir and mix evenly, and then calculate the volume.
[0046] Step 5: Place it in a foaming device, introduce gas to foam it, and place the prepared foam at 20°C to form the gel foam to be evaluated.
[0047] As a preferred option, in step 1:
[0048] Set the stirring speed to 200-300 r / min and the stirring time to 30 min.
[0049] As a preferred option, the following steps are included:
[0050] Mix 3g of α-modified starch and 3g of acrylamide, add deionized water to make 100mL of solution and stir evenly. Set the stirring speed to 200r / min and the stirring time to 30min to prepare polymer mother liquor.
[0051] Add 0.1g of N,N-methylenebisacrylamide to the well-stirred solution and continue stirring for 10 minutes to ensure complete dissolution. Slowly add 0.001g of potassium persulfate initiator to a sealed container and place it in a 130°C high-temperature oven. After a period of time, it will form a gel.
[0052] Transfer it to a mixer and stir at high speed for 1 minute to turn the solid starch gel into a highly viscous semi-liquid state;
[0053] Add the solution and tap water in a volume ratio of 3:7, and stir to mix thoroughly.
[0054] Place it in a foaming device, introduce gas to foam it, and then place the prepared foam at a certain temperature to form a foam gel.
[0055] As a preferred option, the stacking index of the prepared gel foam to be evaluated is obtained as follows:
[0056] Weigh 100g of the prepared gel foam to be evaluated, i.e., m max =100g; After stirring the mixed solution to produce foam, the total weight of the foam in its initial state before separation is measured as m0 = 100g; After standing for time t after foaming, the separated liquid reaches half of the total liquid volume before foaming, and the time at this point is t. The mass of the precipitated liquid was measured at different times t and fitted using formula (1), yielding a coefficient b = 2.79. The gel foam has a long half-life of precipitation and a very small amount of precipitated liquid; therefore, the precipitated liquid volume m was used in the calculation. d (t) is approximately zero, and the mass of the gel foam is m0-m d Given a constant value for t, the instantaneous expansion ratio E(t) of the gel foam is determined to be 1; the initial expansion ratio E(0) of the gel foam is experimentally measured to be 4, and the structural damage coefficient λ is determined to be 4. The gel foam is then subjected to constant shear rates (1, 3, 7, 15, 30, 60 and 150 s). -1 Shearing was performed for 900 s, and the corresponding apparent viscosity was measured, yielding m = 0.81. An experiment was conducted with simultaneous changes in shear rate and time to obtain the transverse shear stress variation curve. By fitting the experimental values of transverse shear stress and shear rate, K = 1.19, n = 0.383, and τ... y =1.5; Based on the experimental values, the parameter value is obtained, and the formula for the packing index is:
[0057]
[0058] Preferably, the order of steps one and two is reversed.
[0059] The method for evaluating the performance of gel foam systems provided by this invention has the following technical advantages:
[0060] This invention proposes a method for evaluating the performance of gel foam systems. The resulting packing index effectively characterizes the sealing effect of gel foam on fractured-vuggy reservoirs and the displacement of residual oil. This fills a gap in current methods for evaluating the packing performance of gel foam systems and can effectively screen gel foam systems suitable for fractured-vuggy reservoirs, providing theoretical support for oilfield foam-driven enhanced oil recovery technologies. It also effectively guides well selection for the field application of foam-driven technologies in high-temperature, high-pressure, and high-salinity reservoirs. Furthermore, this method uses the relationship between lateral shear stress, shear rate, and viscosity, based on the Herschel–Bulkley modified time model, to quantitatively analyze the packing index of gel foam based on stress analysis. By establishing the packing index through shear rate, the evaluation of the packing performance of gel foam systems can be completed in the laboratory. Attached Figure Description
[0061] Figure 1 This is a schematic diagram of the stacking height and equivalent diameter of an ideal conical foam stack, where r is half of the equivalent diameter;
[0062] Figure 2 A simplified structural diagram of a gel foam under stress. Detailed Implementation
[0063] The present invention will now be described in further detail.
[0064] The present invention will now be described in more detail with reference to the accompanying drawings, which illustrate preferred embodiments of the invention. It should be understood that those skilled in the art can modify the invention described herein while still achieving the beneficial effects of the invention. Therefore, the following description should be understood as being of broad knowledge to those skilled in the art and is not intended to limit the invention.
[0065] For clarity, not all features of the actual embodiments are described. In the following description, well-known functions and structures are not detailed in detail, as they would confuse the invention with unnecessary detail. It should be understood that in the development of any actual embodiment, numerous implementation details must be made to achieve the developer's specific objectives.
[0066] To make the objectives and features of the present invention more apparent and understandable, the specific embodiments of the present invention will be further described below with reference to the accompanying drawings. It should be noted that the drawings are all in a very simplified form and use non-precise ratios, intended only to facilitate and clearly illustrate the objectives of the embodiments of the present invention.
[0067] This invention provides a method for evaluating the performance of gel foam systems, combined with Figure 1 and Figure 2 It includes the following steps:
[0068] Step 1: Establish the packing index model, where the packing index is denoted as A. This packing index is the ratio of the height h of a unit mass of foam to the equivalent diameter d of the bottom surface under ideal conical foam packing conditions. The packing index is used to characterize the packing performance of gel foam. In this ideal state, half of the apex angle of the cone cross-section formed by the foam packing is θ. The method for obtaining the packing index A is as follows:
[0069] Based on the foam separation experiment, a time-considered model is established, and the relationship between the separation mass and the model is expressed by the following formula:
[0070]
[0071] Where m d(t) represents the cumulative mass (g) of the precipitate at time t, m max The value represents the maximum mass of the separated liquid (g), and t represents the separation time (s). denoted as 1 / 2 precipitation time (s), and b represents a parameter of the precipitation process;
[0072] When the gel foam is in equilibrium, the external forces acting on it in the longitudinal direction are gravity and the supporting force from the bottom surface. When the gel foam is at rest, the gravity acting on the entire gel foam is:
[0073] G=(m0-m d (t))g (2)
[0074] Where m0 is the total weight of the foam in its initial state before separation;
[0075] At this point, the gel foam is in equilibrium. The lateral component of the gravity acting on the gel foam at that point is equal to the static friction force on the bottom surface of the gel foam, and numerically replaced by the lateral shear stress on the gel foam at the shear rate measured in the laboratory:
[0076]
[0077] τ is the transverse shear stress (N);
[0078] Define the instantaneous average foaming ratio E(t) as:
[0079]
[0080] Where m s (t) refers to the mass (g) of foam liquid of the same volume as the foam at time t; m f (0) refers to the initial mass (g) of the foam;
[0081] The expression for the structural damage coefficient λ of the foam is as follows:
[0082]
[0083] Where E(0) is the initial foaming ratio;
[0084] Using the mass of the precipitate as an intermediate variable and assuming a constant shear rate, the relationship between the apparent viscosity of the foam and time was established as follows:
[0085] μ app (γ, t) = μ app (γ,0)Exp(1-(λ(t)) m (6)
[0086] Apparent viscosity is the ratio of transverse shear stress to shear rate. Using the Herschel-Bulkley rheological model, it is transformed into an apparent viscosity expression. Substituting this expression into formula (6), a time-corrected Herschel-Bulkley rheological model is derived, revealing the change in transverse shear stress at a given moment:
[0087] τ(γ, t)=(τ y +Kγ n )Exp(1-(λ(t)) m (7)
[0088] Where γ is the shear rate (s) -1 );τ y K, m, and n are all parameters that can be measured experimentally;
[0089] The centroid of the cone is located at 1 / 4 of its height along the central axis, and under ideal stacking conditions, θ = 30°. Based on the forces acting on the gel foam at different times and the law of similar triangles, and using formulas (3) and (7), the following can be obtained:
[0090]
[0091] The accumulation index A is obtained as follows:
[0092]
[0093] The parameter b is obtained as follows:
[0094] The initial mass m0, the final mass of the separated solution, and the half-separation time of the gel foam system. The measured value of the prepared semi-liquid gel and foaming agent mixture was obtained through experiments; this value is m. max After stirring and foaming, the total weight of the initial foam (without precipitate) is measured as m0. After time t, the precipitated liquid reaches half the total liquid volume before foaming; this time is t'. By measuring the mass of the precipitated liquid at different times t and fitting the data using formula (1), the parameter b can be obtained.
[0095] Parameter τ y The methods for deriving K, n, and n are as follows:
[0096] An experiment was conducted to test the change of apparent viscosity over time. Gel foam with a fixed initial foaming volume was selected for the experiment. It was assumed that the test time was short and the volume fraction of the foam liquid did not change. The changes in the size and shape of the foam were ignored, and thus the viscosity changes caused by time were ignored. The transverse shear stress of the gel foam at different shear rates was obtained by fitting the experimental values using the Herschel–Bulkley model. The transverse shear stress at different times and different shear rates was obtained by fitting the values using formula (7). The parameter τ can be obtained by fitting the values. y K, m, n;
[0097] The obtained parameters b and τ y Substituting K, m, and n into formula (9), we obtain the packing index A as a function of the shear rate γ;
[0098] Step 2: Provide the gel foam system to be evaluated;
[0099] Step 3: Based on the shear rate obtained in the experiment, the packing index A is obtained by formula (9). The larger the value of the packing index A, the better the packing performance of the gel foam system to be evaluated.
[0100] This invention proposes a method for evaluating the performance of gel foam systems. The resulting packing index effectively characterizes the sealing effect of gel foam on fractured-vuggy reservoirs and the displacement of residual oil. This fills a gap in current methods for evaluating the packing performance of gel foam systems and can effectively screen gel foam systems suitable for fractured-vuggy reservoirs, providing theoretical support for oilfield foam-driven enhanced oil recovery technologies. It also effectively guides well selection for the field application of foam-driven technologies in high-temperature, high-pressure, and high-salinity reservoirs. Furthermore, this method uses the relationship between lateral shear stress, shear rate, and viscosity, based on the Herschel–Bulkley modified time model, to quantitatively analyze the packing index of gel foam based on stress analysis. By establishing the packing index through shear rate, the evaluation of the packing performance of gel foam systems can be completed in the laboratory.
[0101] In one specific embodiment, in step two, the gel foam system to be evaluated is provided by the following method:
[0102] Step 1: Mix α-modified starch and acrylamide in a 1:1 mass ratio and stir evenly in deionized water to prepare polymer mother liquor;
[0103] Step 2: Add N,N-methylenebisacrylamide to the well-stirred solution and continue stirring for 10 minutes to ensure complete dissolution. Slowly add potassium persulfate initiator to a sealed container and place it in a 130°C high-temperature oven. After a period of time, it will form a gel.
[0104] Step 3: Transfer it to a mixer and stir at high speed for 1 minute to change the solid starch gel into a highly viscous semi-liquid state;
[0105] Step 4: Add tap water to the highly viscous semi-liquid and tap water in a volume ratio of 3:7, stir and mix evenly, and then calculate the volume.
[0106] Step 5: Place it in a foaming device, introduce gas to foam it, and place the prepared foam at 20°C to form the gel foam to be evaluated.
[0107] In step 1:
[0108] Set the stirring speed to 200-300 r / min and the stirring time to 30 min.
[0109] One specific implementation includes the following steps:
[0110] Mix 3g of α-modified starch and 3g of acrylamide, add deionized water to make 100mL of solution and stir evenly. Set the stirring speed to 200r / min and the stirring time to 30min to prepare polymer mother liquor.
[0111] Add 0.1g of N,N-methylenebisacrylamide to the well-stirred solution and continue stirring for 10 minutes to ensure complete dissolution. Slowly add 0.001g of potassium persulfate initiator to a sealed container and place it in a 130°C high-temperature oven. After a period of time, it will form a gel.
[0112] Transfer it to a mixer and stir at high speed for 1 minute to turn the solid starch gel into a highly viscous semi-liquid state;
[0113] Add the solution and tap water in a volume ratio of 3:7, and stir to mix thoroughly.
[0114] Place it in a foaming device, introduce gas to foam it, and then place the prepared foam at a certain temperature to form a foam gel.
[0115] The stacking index of the prepared gel foam to be evaluated was obtained as follows:
[0116] Weigh 100g of the prepared gel foam to be evaluated, i.e., m max =100g; After stirring the mixed solution to produce foam, the total weight of the foam in its initial state before separation is measured as m0 = 100g; After standing for time t after foaming, the separated liquid reaches half of the total liquid volume before foaming, and the time at this point is t. The mass of the precipitated liquid was measured at different times t and fitted using formula (1), yielding a coefficient b = 2.79. The gel foam has a long half-life of precipitation and a very small amount of precipitated liquid; therefore, the precipitated liquid volume m was used in the calculation. d(t) is approximately zero, and the mass of the gel foam is m0-m d Given a constant value for t, the instantaneous expansion ratio E(t) of the gel foam is determined to be 1; the initial expansion ratio E(0) of the gel foam is experimentally measured to be 4, and the structural damage coefficient λ is determined to be 4. The gel foam is then subjected to constant shear rates (1, 3, 7, 15, 30, 60 and 150 s). -1 Shearing was performed for 900 s, and the corresponding apparent viscosity was measured, yielding m = 0.81. An experiment was conducted with simultaneous changes in shear rate and time to obtain the transverse shear stress variation curve. By fitting the experimental values of transverse shear stress and shear rate, K = 1.19, n = 0.383, and τ... y =1.5; Based on the experimental values, the parameter value is obtained, and the formula for the packing index is:
[0117]
[0118] The packing index of the gel foam at different shear rates can be calculated:
[0119] <![CDATA[Shear rate / s -1 > Stacking Index 1 57.96 2 51.09 3 47.07 5 42.09
[0120] This allows for the evaluation of stacking performance.
[0121] In one specific implementation, the order of steps one and two is reversed.
[0122] The foregoing has shown and described the basic principles, main features, and advantages of the present invention; therefore, the above descriptions are merely embodiments of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The embodiments and descriptions in the specification are only principles of the present invention. The present invention also includes various equivalent changes and modifications without departing from its spirit and scope, and all such changes and modifications fall within the scope of the present invention as claimed. The scope of protection of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for evaluating the performance of gel foam systems, characterized in that, Includes the following steps: Step 1: Establish the packing index model, where the packing index is denoted as A. This packing index is the ratio of the height h of a unit mass of foam to the equivalent diameter d of the bottom surface under ideal conical foam packing conditions. The packing index is used to characterize the packing performance of gel foam. In this ideal state, half of the apex angle of the cone cross-section formed by the foam packing is θ. The method for obtaining the packing index A is as follows: Based on the foam separation experiment, a time-considered model is established, and the relationship between the separation mass and the model is expressed by the following formula: in Shown Accumulated mass of the precipitate at any time Indicates the maximum mass of the separated liquid. Indicates the precipitation time Indicates 1 / 2 separation time Dimensionless, representing parameters of the liquid precipitation process; When the gel foam is in equilibrium, the external forces acting on it in the longitudinal direction are gravity and the supporting force from the bottom surface. When the gel foam is at rest, the gravity acting on the entire gel foam is: in, The total weight of the foam in its initial state before separation. The acceleration due to gravity is taken as 9.8 m / s². At this point, the gel foam is in equilibrium. The lateral component of the gravity acting on the gel foam at that point is equal to the static friction force on the bottom surface of the gel foam, and numerically replaced by the lateral shear stress on the gel foam at the shear rate measured in the laboratory: The static friction force experienced by the gel foam on the bottom surface is expressed in units of 1. Transverse shear force (N); Define the instantaneous average foaming ratio E(t) as: in Mass of foam liquid of equal volume to the time and foam The initial mass (g) of the foam. The expression for the structural damage coefficient λ of the foam is as follows: Where E(0) is the initial foaming ratio; Using the mass of the precipitate as an intermediate variable and assuming a constant shear rate, the relationship between the apparent viscosity of the foam and time was established as follows: in, Let be the apparent viscosity at shear rate γ and time t, in Pa·s. The apparent viscosity is the ratio of transverse shear stress to shear rate. Using the Herschel–Bulkley rheological model, the apparent viscosity expression is transformed and substituted into formula (6) to derive the time-corrected Herschel–Bulkley rheological model, thus obtaining the change in transverse shear stress at a certain moment, i.e.: in, Shear rate All of these are parameters that can be measured experimentally. For yield stress, unit The structural damage index is dimensionless. The centroid of the cone is located at 1 / 4 of its height along the central axis, and θ = 30° under ideal stacking conditions. Based on the forces acting on the gel foam at different times and the law of similar triangles, and using formulas (3) and (7), the following can be obtained: The accumulation index A is obtained as follows: Among them, parameters The method is as follows: Initial mass of the gel foam system Final precipitation mass and half precipitation time The measured solution of the prepared semi-liquid gel and foaming agent was obtained through experiments. After stirring and foaming, the total weight of the foam in its initial state (before separation) is measured. After the foam has been left for time t, the precipitated liquid reaches half of the total liquid volume before foaming. This time is called the t-th minute mark. ; Measure at different times The mass of the precipitated liquid is used as the basis for fitting the parameters using formula (1). ; parameter The method is as follows: An experiment was conducted to test the change of apparent viscosity over time. Gel foam with a fixed initial foaming volume was selected for the experiment. It was assumed that the test time was short and the volume fraction of the foam liquid did not change. The changes in the size and shape of the foam were ignored, and thus the viscosity changes caused by time were ignored. The transverse shear stress of the gel foam at different shear rates was used to fit the experimental values using the Herschel–Bulkley model to obtain the transverse shear stress at different times and different shear rates. The parameters were obtained by fitting the values using formula (7). ; The obtained parameters Substituting into formula (9), we obtain the packing index A related to the shear rate. The function; Step 2: Provide the gel foam system to be evaluated; Step 3: Based on the shear rate obtained in the experiment, the packing index A is obtained by formula (9). The larger the value of the packing index A, the better the packing performance of the gel foam system to be evaluated.
2. The method for evaluating the performance of a gel foam system according to claim 1, characterized in that, In step two, the gel foam system to be evaluated is provided using the following method: Step 1: Mix α-modified starch and acrylamide in a 1:1 mass ratio and stir evenly in deionized water to prepare polymer mother liquor; Step 2: Add N,N-methylenebisacrylamide to the well-stirred solution and continue stirring for 10 minutes to ensure complete dissolution. Slowly add potassium persulfate initiator to a sealed container and place it in a 130°C high-temperature oven. After a period of time, it will form a gel. Step 3: Transfer it to a mixer and stir at high speed for 1 minute to change the solid starch gel into a highly viscous semi-liquid state; Step 4: Add tap water to the highly viscous semi-liquid and tap water in a volume ratio of 3:7, stir and mix evenly, and then calculate the volume. Step 5: Place it in a foaming device, introduce gas to foam it, and place the prepared foam at 20°C to form the gel foam to be evaluated.
3. The method for evaluating the performance of a gel foam system according to claim 2, characterized in that, In step 1: Set the stirring speed to 200-300 r / min and the stirring time to 30 min.
4. The method for evaluating the performance of a gel foam system according to claim 3, characterized in that, Includes the following steps: Mix 3g of α-modified starch and 3g of acrylamide, add deionized water to make 100mL of solution and stir evenly. Set the stirring speed to 200r / min and the stirring time to 30min to prepare polymer mother liquor. Add 0.1g of N,N-methylenebisacrylamide to the well-stirred solution and continue stirring for 10 minutes to ensure complete dissolution. Slowly add 0.001g of potassium persulfate initiator to a sealed container and place it in a 130°C high-temperature oven. After a period of time, it will form a gel. Transfer it to a mixer and stir at high speed for 1 minute to turn the solid starch gel into a highly viscous semi-liquid state; Add the solution and tap water in a volume ratio of 3:7, and stir to mix thoroughly. Place it in a foaming device, introduce gas to foam it, and then place the prepared foam at a certain temperature to form a foam gel.
5. The method for evaluating the performance of a gel foam system according to claim 1, characterized in that, The order of steps one and two is reversed.
Citation Information
Patent Citations
Gel foam for coal seam fire control
CN103742186A
Slump and slump flow value estimation method and facility
JP2020071134A