Anode materials and their preparation methods, secondary batteries and electrical devices
By combining iron vanadate and carbon materials to control the porosity to 50-60%, and combining it with the sol-gel method to prepare anode materials, the problems of poor conductivity and large volume change of vanadium-based anode materials are solved, thereby improving the cycle performance, first efficiency and rate performance of secondary batteries.
Patent Information
- Application Number
- CN202410016190.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-03
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-01-03
AI Technical Summary
Vanadium-based anode materials exhibit poor conductivity and large volume changes during charge and discharge, resulting in insufficient cycle performance and safety of secondary batteries.
By combining iron vanadate and carbon materials, the porosity of the negative electrode material is controlled to 50-60%, and the negative electrode material is prepared by sol-gel method. In combination with carbon materials such as graphene and carbon nanotubes, the conductivity and structural stability of the material are improved.
It significantly improves the cycle performance and first-charge efficiency of secondary batteries, and also improves rate performance.
Smart Images

Figure BDA0004652722900000051
Abstract
Description
Technical Field
[0001] This application relates to the field of negative electrode material technology, and in particular to a negative electrode material and its preparation method, a secondary battery, and an electrical device. Background Technology
[0002] The rapid development of the electric vehicle industry has led to a growing demand for high-performance rechargeable batteries. Electrode materials, as a key component of rechargeable batteries, play a decisive role in their performance. Currently, the theoretical specific capacity of commercially available graphite anodes is only 372 mAh / g, which significantly limits the large-scale application of rechargeable batteries. Furthermore, the intercalation reaction potential of graphite anodes is similar to that of lithium metal deposition, inevitably leading to the formation of unfavorable lithium dendrites, resulting in internal short circuits and safety issues. Therefore, designing high-performance anode materials with higher safety remains of great importance. Vanadium-based materials are favored by researchers due to their abundant natural resources, low toxicity, and the rich electrons and crystal structures conferred by various oxidation states. Some transition metal vanadates, as rechargeable battery anodes, exhibit significantly higher specific capacity and safety than commercial graphite. However, vanadium-based materials still suffer from large volume changes during charge and discharge, resulting in poor cycle performance, as well as poor conductivity and severe polarization during charge and discharge. Summary of the Invention
[0003] The purpose of this application is to provide a negative electrode material to overcome the problems of poor conductivity and large volume change during charging of vanadium-based negative electrode materials, which in turn lead to poor electrochemical performance of secondary batteries.
[0004] To achieve the above objectives, in a first aspect of this application, a negative electrode material is provided, the negative electrode material comprising iron vanadate and carbon material, the porosity of the negative electrode material being 50% to 60%.
[0005] As an embodiment of this application, the carbon content in the negative electrode material is 0.1wt% to 2wt%.
[0006] As an embodiment of this application, the carbon material includes at least one of graphene, carbon nanotubes, and Ketjen black.
[0007] A second aspect of this application provides a method for preparing the negative electrode material described in the first aspect of this application.
[0008] The method for preparing the negative electrode material according to the second aspect of this application includes the following steps:
[0009] S1. Mix vanadium source, iron source and solvent, dissolve them, add chelating agent, stir to obtain precursor;
[0010] S2. The precursor is calcined and ground to obtain iron vanadate powder material;
[0011] S3. Add the iron vanadate material and the carbon material to anhydrous ethanol, and then stir, dry and grind them in sequence to obtain the negative electrode material.
[0012] As an embodiment of this application, the vanadium source includes ammonium metavanadate and / or vanadium pentoxide.
[0013] As an embodiment of this application, the iron source includes at least one of ferric nitrate, ferric sulfate, ferric chloride, and ferric acetate.
[0014] As an embodiment of this application, the chelating agent includes citric acid and / or glucose.
[0015] As an embodiment of this application, the calcination temperature is 600-900℃ and the calcination time is 2-4 hours.
[0016] As an embodiment of this application, the molar ratio of the iron source to the chelating agent is 1:2 to 3:1.
[0017] A third aspect of this application provides a negative electrode sheet, the negative electrode sheet comprising the negative electrode material described in the first aspect of this application.
[0018] A fourth aspect of this application provides a secondary battery, the secondary battery including the negative electrode sheet described in the third aspect of this application.
[0019] A fifth aspect of this application provides an electrical device comprising the secondary battery described in the fourth aspect of this application.
[0020] Compared with the prior art, the beneficial effects of this application are:
[0021] This application provides a negative electrode material comprising iron vanadate and carbon material, wherein the porosity of the negative electrode material is 50%–60%. By combining iron vanadate and carbon material and controlling the porosity of the negative electrode material within a certain range, the cycle performance, first-efficiency, and rate performance of the secondary battery are improved. Detailed Implementation
[0022] To better illustrate the purpose, technical solution, and advantages of this application, specific embodiments will be used to further describe this application below. However, these embodiments do not limit this application in any way. Unless otherwise specified, the reagents, methods, and equipment used in this application are conventional reagents, methods, and equipment in this technical field. Unless otherwise specified, all reagents and materials used in this application are commercially available.
[0023] An embodiment of this application provides a negative electrode material comprising iron vanadate and carbon material, wherein the porosity of the negative electrode material is 50% to 60%.
[0024] The porosity of the negative electrode material described in this application is 50% to 60%. Specifically, the porosity of the negative electrode material can be 50%, 52%, 55%, 58%, 60%, or any two of these values.
[0025] In some embodiments, the carbon content in the negative electrode material is 0.1 wt% to 2 wt%. For example, the carbon content in the negative electrode material can be 0.1 wt%, 0.5 wt%, 1 wt%, 1.5 wt%, 2 wt%, or any two of these values. Controlling the carbon content within the above range can further optimize the electrochemical performance of the secondary battery.
[0026] In some embodiments, the carbon material includes at least one of graphene, carbon nanotubes, and Ketjen black.
[0027] The embodiments of this application provide a method for preparing a negative electrode material.
[0028] The method for preparing the negative electrode material described in this application includes the following steps:
[0029] S1. Mix vanadium source, iron source and solvent, dissolve them, add chelating agent, stir to obtain precursor;
[0030] S2. The precursor is calcined and ground to obtain iron vanadate powder material;
[0031] S3. Add the iron vanadate material and the carbon material to anhydrous ethanol, and then stir, dry and grind them in sequence to obtain the negative electrode material.
[0032] The method for preparing the negative electrode material described in this application is the sol-gel method. Compared with the high-temperature hydrothermal method, the precursor reaction temperature is lower, the equipment requirements are lower, and the corresponding cost is lower. Furthermore, this method is also applicable to the preparation of other iron vanadates.
[0033] In some embodiments, the vanadium source includes ammonium metavanadate and / or vanadium pentoxide.
[0034] In some embodiments, the iron source includes at least one of ferric nitrate, ferric sulfate, ferric chloride, and ferric acetate.
[0035] In some embodiments, the chelating agent includes citric acid and / or glucose.
[0036] In some embodiments, the solvent includes deionized water and / or ethanol.
[0037] In some embodiments, the calcination temperature is 600–900°C, and the calcination time is 2–4 hours. For example, the calcination temperature can be 600°C, 650°C, 700°C, 750°C, 800°C, 850°C, 900°C, or any two of these values. The calcination time can be 2 hours, 2.5 hours, 3 hours, 3.5 hours, 4 hours, or any two of these values.
[0038] In some embodiments, the molar ratio of the iron source to the chelating agent is 1:2 to 3:1.
[0039] This application also protects negative electrode sheets containing the aforementioned negative electrode material.
[0040] This application also protects secondary batteries containing the aforementioned negative electrode plate.
[0041] This application also protects electrical devices that include the aforementioned secondary batteries.
[0042] The following are specific embodiments of this application, and the technical solutions of this application are further described in conjunction with the embodiments. However, this application is not limited to these embodiments. Unless otherwise specified, the reagents, methods, and equipment used in this application are all conventional reagents, methods, and equipment in this technical field.
[0043] Example 1
[0044] Example 1 provides a negative electrode material, and the preparation method of the negative electrode material is as follows:
[0045] 4.04 g of ferric nitrate and 2.64 g of ammonium metavanadate were added to deionized water and stirred at 70 °C until fully dissolved. Then, 3 g of citric acid monohydrate was added and stirred continuously until the water was completely evaporated to obtain the precursor. The obtained precursor was calcined in air at 800 °C for 3 hours. After grinding, porous iron vanadate powder was obtained. The porous iron vanadate powder and 0.026 g of graphene powder were added to an appropriate amount of anhydrous ethanol and stirred continuously. After the anhydrous ethanol evaporated completely, the mixture was dried in a 100 °C oven and ground to obtain the negative electrode material.
[0046] Examples 2-3
[0047] The difference between Examples 2 and 3 and Example 1 is that the amount of citric acid monohydrate used is different, which is 1g and 5g respectively.
[0048] Examples 4-5
[0049] The difference between Examples 4 and 5 and Example 1 is that the amount of graphene powder used is different, at 0.0026g and 0.052g respectively.
[0050] Comparative Example 1
[0051] Comparative Example 1 provides a negative electrode material, the preparation method of which is as follows:
[0052] 4.04 g of ferric nitrate and 2.64 g of ammonium metavanadate were added to deionized water and stirred at 70 °C until the water was completely evaporated to obtain the precursor. The obtained precursor was calcined in air at 800 °C for 3 h. After grinding, iron vanadate powder material was obtained.
[0053] Comparative Example 2
[0054] 4.04 g of ferric nitrate and 2.64 g of ammonium metavanadate were added to deionized water and stirred at 70 °C until fully dissolved. Then, 3 g of citric acid monohydrate was added and stirred continuously until the water was completely evaporated to obtain the precursor. The obtained precursor was calcined in air at 800 °C for 3 h. After grinding, porous iron vanadate powder material was obtained.
[0055] Comparative Example 3
[0056] 4.04 g of ferric nitrate and 2.64 g of ammonium metavanadate were added to deionized water and stirred at 70 °C until the water was completely evaporated to obtain a precursor. The obtained precursor was calcined in air at 800 °C for 3 h. After grinding, iron vanadate powder material was obtained. The iron vanadate powder and 0.0026 g of graphene powder were added to an appropriate amount of anhydrous ethanol and stirred continuously. After the anhydrous ethanol was completely evaporated, the mixture was placed in a 100 °C oven to dry and then ground to obtain carbon composite porous iron vanadate material.
[0057] test
[0058] The electrochemical performance of the materials prepared in Examples 1-5 and Comparative Examples 1-3 was tested using CR2032 coin cells. One electrode consisted of the prepared vanadium-based anode material, acetylene black, and sodium alginate (mass ratio 70:15:15), while the other electrode was a lithium metal sheet. The electrolyte was 1 mol / L LiPF6 dissolved in an EC / DMC / EMC solvent (volume ratio 1:1:1). The constant current charge / discharge voltage range was 0.01–3 V.
[0059] 1) First reversible specific capacity and first coulombic efficiency test:
[0060] After the button cell is assembled, ① discharge: discharge at a constant current of 2A / g to 0.01V, and the discharge specific capacity is recorded as Q1; ② charge: charge at a constant current of 2A / g to 3V, and the charging specific capacity is recorded as Q2; the initial coulombic efficiency is abbreviated as ICE, ICE = Q2 / Q1.
[0061] 2) Cyclic performance test:
[0062] ① Discharge: Discharge at a constant current of 2A / g to 0.01V, with a 10-minute interval; ② Charge: Charge at a constant current of 2A / g to 3V, with a 10-minute interval; ③ Repeat steps ① and ② for 500 cycles. The discharge capacity at the 500th cycle is Q500.
[0063] 3) Ratio performance test:
[0064] After stabilizing for 300 cycles according to step 2), the rate performance test is performed: ① Discharge to 0.01V with a constant current of 0.1A / g, and charge to 3V with a constant current of 0.1A / g after a 10-minute interval; ② Repeat step ① for 10 cycles; ③ Increase the current density in steps ① and ② to 0.5, 1, and 2A / g, where the discharge capacities corresponding to 0.1, 0.5, 1, and 2A / g are Q310, Q320, Q330, and Q340, respectively.
[0065] Table 1. Carbon content, porosity, and performance of the negative electrode materials described in the examples and comparative examples.
[0066]
[0067] The results above show that:
[0068] As can be seen from the above embodiments and comparative examples, this application improves the cycle performance, first-time efficiency, and rate performance of secondary batteries by combining iron vanadate and carbon materials and controlling the porosity of the negative electrode material within a certain range.
[0069] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of this application and are not intended to limit the scope of protection of this application. Although this application has been described in detail with reference to preferred embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of this application without departing from the substance and scope of the technical solutions of this application.
Claims
1. A negative electrode material, characterized in that, The negative electrode material comprises porous iron vanadate and carbon material, wherein the carbon material content in the negative electrode material is 0.1wt%~2wt%, and the carbon material includes at least one of graphene, carbon nanotubes, and Ketjen black; the porosity of the negative electrode material is 50%~60%. The negative electrode material is prepared according to a preparation method including the following steps: S1. Mix vanadium source, iron source and solvent, dissolve them, add chelating agent, stir to obtain precursor; S2. The precursor is calcined and ground to obtain iron vanadate powder material; S3. Add the iron vanadate material and the carbon material to anhydrous ethanol, and then stir, dry and grind them in sequence to obtain the negative electrode material.
2. The method for preparing the negative electrode material according to claim 1, characterized in that, Includes the following steps: S1. Mix vanadium source, iron source and solvent, dissolve them, add chelating agent, stir to obtain precursor; The vanadium source includes ammonium metavanadate and / or vanadium pentoxide; the iron source includes at least one of ferric nitrate, ferric sulfate, ferric chloride, and ferric acetate; the chelating agent includes citric acid and / or glucose. The molar ratio of the iron source to the chelating agent is 1:2 to 3:1; S2. The precursor is calcined at 600~900°C for 2~4h, and then ground to obtain iron vanadate powder material; S3. Add the iron vanadate material and the carbon material to anhydrous ethanol, and then stir, dry and grind them in sequence to obtain the negative electrode material.
3. A negative electrode sheet, characterized in that, The negative electrode material includes the negative electrode material according to claim 1 or the negative electrode material prepared by the preparation method of the negative electrode material according to claim 2.
4. A secondary battery, characterized in that, Includes the negative electrode sheet as described in claim 3.
5. An electrical device, characterized in that, Includes the secondary battery as described in claim 4.
Citation Information
Patent Citations
Fe2VO4 / ordered mesoporous carbon composite material and application thereof
CN111900389A
Ferrovanadate material as well as preparation method and application thereof
CN114538523A