A dry-process membrane, its preparation method and application

By coating the dry-process separator with an anti-tear slurry containing hydroxyl groups, the problem of easy tearing of the dry-process separator in the TD lateral direction is solved, thereby improving the safety and electrochemical performance of lithium batteries.

CN117748053BActive Publication Date: 2026-11-17EVE POWER CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311755283.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-19
Publication Date
2026-11-17
Estimated Expiration
2043-12-19

AI Technical Summary

Technical Problem

Dry-process separators are prone to tearing in the lateral direction of TD, resulting in insufficient safety performance of lithium batteries, especially when the cell is unexpectedly deformed, which can easily lead to the risk of short circuit between the positive and negative electrodes.

Method used

A tear-resistant slurry is coated on the porous substrate surface of the dry-process diaphragm. The tear-resistant slurry is composed of inorganic substances containing hydroxyl groups and binders. It enhances intermolecular forces through hydrogen bonding and forms a three-dimensional network structure, thereby improving the tear resistance and flexibility of the diaphragm.

Benefits of technology

It enhances the tear resistance of dry-process separators in the TD lateral direction, improves the safety and electrochemical performance of lithium batteries, and reduces the risk of cell rupture under impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004617590710000121
    Figure BDA0004617590710000121
Patent Text Reader

Abstract

This application specifically discloses a dry-process separator, its preparation method, and its application. The dry-process separator comprises a porous substrate layer and a tear-resistant coating coated on at least one surface of the porous substrate layer; the tear-resistant coating comprises a tear-resistant slurry, which includes a polymer, an inorganic material, a binder, and a solvent; wherein the inorganic material contains hydroxyl groups, and the binder contains hydroxyl groups; the inorganic material includes at least one of a tubular structure and a sheet structure; when the inorganic material is a tubular structure, the aspect ratio of the inorganic material is 5:1-10:1; when the inorganic material is a sheet structure, the thickness of the inorganic material is 0.6-1 μm. This application has the advantages of improving the tear resistance of dry-process separators and improving the safety performance of lithium batteries.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of lithium-ion battery technology, and in particular to a dry-process separator, its preparation method, and its application. Background Technology

[0002] Lithium-ion batteries mainly consist of a positive electrode, a negative electrode, a separator, and an electrolyte. The separator plays a crucial role, significantly determining the battery's chemical performance, safety performance, and cost. With increasing demands for higher energy density in various industries, separators are becoming increasingly thinner. However, this thinning of the separator also presents challenges to battery safety. Currently, separators used in the industry are classified according to their manufacturing process into dry-process separators and wet-process separators.

[0003] Wet-process membranes are prepared using a wet process. This process involves mixing liquid hydrocarbons or small-molecule substances with polyolefins, heating and melting the mixture to form a homogeneous mixture, then cooling and separating the phases to obtain a membrane containing white oil. The membrane is then heated to near its melting point and subjected to biaxial stretching for molecular orientation. Finally, extraction is performed, followed by holding at the temperature for a certain period, resulting in a microporous polyethylene film material. In contrast, dry-process membranes are prepared using a dry process. This process involves producing a low-crystallinity, highly oriented polypropylene film using a method similar to that used to produce rigid elastic fibers. This film is first stretched at a low temperature to create microdefects, and then stretched at a high temperature to form micropores, resulting in a microporous membrane with a specific orientation.

[0004] Due to the difference in the membrane manufacturing process, dry-process membranes exhibit excellent thermal shrinkage properties in the transverse direction of the TD (diode) phase. However, this also brings certain drawbacks. Dry-process membranes are prone to tearing along the longitudinal direction of the MD (membrane) phase. Furthermore, the strength of dry-process membranes in the transverse direction of the TD phase is much lower than that of wet-process membranes. Moreover, because dry-process membranes are easily torn, when applied to battery cells, if the cell is accidentally deformed, the membrane will not be able to resist the transverse tearing force and will rupture. This can cause a short circuit between the positive and negative electrodes in the battery cell, leading to a serious safety accident.

[0005] In the research on conventional dry-process separators, it has been found that cells using dry-process separators fail the heavy object impact safety test; therefore, there is an urgent need to propose a dry-process separator with excellent tear resistance, which can improve the safety performance of lithium batteries when applied to cells. Summary of the Invention

[0006] In order to improve the tear resistance of dry-process separators and thus improve the safety performance of lithium batteries, this application provides a dry-process separator, its preparation method, and its application.

[0007] In a first aspect, this application provides a dry-process separator, which adopts the following technical solution:

[0008] A dry-process separator, the dry-process separator comprising a porous substrate layer and a tear-resistant coating applied to at least one surface of the porous substrate layer;

[0009] The tear-resistant coating includes a tear-resistant slurry, which comprises a polymer, an inorganic substance, a binder, and a solvent; wherein the inorganic substance contains hydroxyl groups, and the binder contains hydroxyl groups.

[0010] The inorganic material includes at least one of tubular structure and sheet structure; when the inorganic material is tubular, the aspect ratio of the inorganic material is 5:1-10:1; when the inorganic material is sheet structure, the thickness of the inorganic material is 0.6-1μm.

[0011] Since both inorganic materials and binders contain a certain number of hydroxyl groups, during the preparation of the tear-resistant slurry, the hydroxyl groups in the inorganic materials can react with the hydroxyl groups in the binder to generate a large number of hydrogen bonds, enhancing the intermolecular forces in the tear-resistant slurry. On the one hand, this can improve the adhesion of the tear-resistant slurry to the surface of the porous substrate, allowing the tear-resistant coating formed on the surface of the porous substrate to a certain extent improve the membrane's elongation. On the other hand, this interaction between the binder and the inorganic materials can also allow the inorganic materials to better fill into the polymer, working together with the polymer to form a network structure, increasing the membrane's flexibility and improving the membrane's elongation at break in the transverse direction of the tear diaphragm (TD). This avoids the tearing that often occurs in the transverse direction of the TD during the application of dry-process membranes, thereby improving the membrane's tear resistance and significantly increasing the membrane's thermal shrinkage rate.

[0012] Furthermore, when the inorganic material is tubular and meets the aforementioned aspect ratio limit, it is easier for the inorganic material to overlap and form a three-dimensional network structure in the tear-resistant slurry. At this time, the inorganic material has a larger specific surface area, which can better bind the binder and allow the inorganic material to be filled into the polymer chain segments in a staggered manner, further promoting the formation of the three-dimensional network structure in the tear-resistant coating and improving the tear resistance of the separator. When the inorganic material is sheet-like and meets the aforementioned thickness limit, it has a larger specific surface area, which not only allows it to better bind the binder, but also makes the accumulation of the inorganic material in the tear-resistant coating more loose and dispersed, thereby enhancing the wettability of the dry-process separator. When applied to the battery cell, it can further improve the electrochemical performance of the battery cell.

[0013] Preferably, the inorganic material includes at least one of boehmite, nanocellulose, and halloysite tubes.

[0014] Preferably, the adhesive comprises at least one of polyacrylic acid, polyacrylate, polyacrylonitrile, and terpolymer adhesive.

[0015] The binder used in this application has a certain degree of flexibility, which is beneficial to further improve the tear resistance of dry-process diaphragms.

[0016] Preferably, the polymer includes at least one of polyarylamide, polyimide, polymethyl methacrylate, and polyvinylidene fluoride.

[0017] Preferably, the polymer has a molecular weight of 200,000-1,000,000 Da.

[0018] By adjusting the molecular weight of the polymer, the entanglement between polymer molecular chains becomes tighter, resulting in a more compact three-dimensional network structure formed when inorganic substances fill the spaces between polymer molecules. This leads to a corresponding increase in the density of the tear-resistant coating, thereby enhancing the tear resistance and toughness of the diaphragm.

[0019] Preferably, the solid content of the tear-resistant slurry is 28%-32%, the viscosity of the tear-resistant slurry is <80cp, the pH of the tear-resistant slurry is 7.5-9.0, and the average particle size D50 of the tear-resistant slurry is <1μm.

[0020] By controlling the viscosity and solid content of the tear-resistant slurry, it can be easily coated onto the surface of the porous substrate. The slurry is thin, and the tear-resistant coating formed on the surface of the porous substrate can better bond with the porous substrate while maintaining its thinness. This is conducive to the development of thinner and lighter diaphragms and makes the diaphragms exhibit good tear resistance.

[0021] Preferably, the thickness of the dry membrane is 10-18 μm, and the thickness ratio of the porous substrate layer to the tear-resistant coating is 5-8:1.

[0022] Secondly, this application provides a method for preparing a dry-process separator, employing the following technical solution:

[0023] A method for preparing a dry-process membrane includes the following steps:

[0024] S1: The polymer, the inorganic material, the binder, and the solvent are mixed under stirring to obtain the tear-resistant slurry; wherein the tear-resistant slurry further includes a dispersant comprising 0.5wt%-3wt% of the mass of the tear-resistant slurry;

[0025] S2: The tear-resistant slurry is coated on at least one surface of the porous substrate, and then the solvent is removed and dried to obtain the dry membrane.

[0026] Preferably, the solvent is an aqueous solvent.

[0027] Preferably, the dispersant includes at least one of nonionic dispersants.

[0028] Preferably, the dispersant includes at least one of polyvinyl alcohol, polyvinyl ether, sodium dodecylbenzenesulfonate, and polyvinylpyrrolidone.

[0029] Preferably, the stirring speed is 800-1000 rpm, the stirring process lasts for 25-35 min, the drying temperature is 55-65℃, and the drying process lasts for 15-25 min.

[0030] The dry-process diaphragm in this application has a certain cost advantage, and introduces less or no solvent in the production process, thus improving the environmental performance of the diaphragm.

[0031] Preferably, in the tear-resistant slurry, the mass ratio of the polymer, the inorganic material and the binder is 10-70:40-80:0.1-10.

[0032] Thirdly, this application provides a lithium-ion battery, which adopts the following technical solution:

[0033] A lithium-ion battery, the lithium-ion battery comprising a positive electrode, a negative electrode, and a dry-process separator as described above. Attached Figure Description Detailed Implementation

[0034] To better understand and implement this invention, the technical solution of the present invention will be clearly and completely described below in conjunction with embodiments. Obviously, the described embodiments are only some embodiments of the present invention, and not all embodiments.

[0035] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention pertains. The terminology used herein in the description of the invention is for the purpose of describing particular embodiments only and is not intended to be limiting of the invention.

[0036] Unless otherwise stated, all numerical values ​​for the amounts of expressed components, reaction conditions, etc., used in the specification and claims are to be understood as being modified by the term "about". Therefore, unless otherwise indicated, the numerical parameters set forth herein are approximate values ​​that can be varied to obtain the desired performance.

[0037] The word “and / or” as used in this article refers to one or all of the elements mentioned.

[0038] The terms "include" and "contain" as used in this article cover both cases where only the mentioned elements exist and cases where other unmentioned elements exist in addition to the mentioned elements.

[0039] All percentages in this invention are weight percentages, unless otherwise stated.

[0040] Unless otherwise stated, the terms “a,” “an,” “an,” and “the” as used in this specification are intended to include “at least one” or “one or more.” For example, “a component” refers to one or more components, and therefore more than one component may be considered and may be employed or used in the implementation of the described embodiments.

[0041] Example

[0042] Example 1

[0043] 1. Preparation of dry-process membranes

[0044] The tear-resistant slurry comprises the following raw materials in parts by weight:

[0045] 13 parts of polyvinylidene fluoride with a molecular weight of 200,000-1,000,000 Da.

[0046] 70 parts of boehmite and 7 parts of halloysite tubes with a length-to-diameter ratio of 5:1.

[0047] 8 parts polyacrylic acid

[0048] 2 parts polyvinyl alcohol,

[0049] 300 parts of deionized water;

[0050] Polyvinylidene fluoride, boehmite, halloysite tube, polyacrylic acid, polyvinyl alcohol, and deionized water were stirred at 1000 rpm for 25 minutes to obtain a tear-resistant slurry with a solid content of 30%, a pH of 7.5, a viscosity of 60 cp, and an average particle size of 0.8 μm.

[0051] The above-mentioned tear-resistant slurry was coated on one side of a polypropylene membrane and dried at 60°C for 20 minutes to generate a tear-resistant coating on the surface of the polypropylene membrane, resulting in a dry membrane with a thickness of 18 μm; wherein, the thickness of the polypropylene membrane to the thickness of the tear-resistant coating in the dry membrane is 9:1.

[0052] 2. Cell fabrication

[0053] 2.1. Preparation of the positive electrode sheet

[0054] The positive electrode slurry was prepared as follows: LFP positive electrode active material: conductive agent acetylene black: binder PVDF = 97.9:0.9:1.2 by mass and added to a vacuum mixer for mixing. Then, solvent NMP was added to the mixed slurry and stirred until homogeneous under the action of a vacuum mixer, thereby obtaining the positive electrode slurry of this embodiment.

[0055] The above-mentioned positive electrode slurry is uniformly coated on both surfaces of the positive electrode current collector aluminum foil. After drying at room temperature, it is transferred to an oven for further drying. After drying in the oven, a positive electrode semi-finished product is obtained. Then, the positive electrode semi-finished product is cold-pressed and cut to obtain the positive electrode sheet to be assembled.

[0056] 2.2. Preparation of negative electrode sheet

[0057] The negative electrode slurry was prepared as follows: artificial graphite, conductive agent acetylene black, thickener CMC, and binder SBR were mixed in a vacuum mixer at a mass ratio of 96.4:1:1.2:1.4. Then, deionized water was added to the resulting mixture, and the mixture was stirred in a vacuum mixer until it became homogeneous, thus obtaining the negative electrode slurry of this embodiment.

[0058] The above-mentioned negative electrode slurry is uniformly coated on both surfaces of the negative electrode current collector copper foil. After drying at room temperature, it is transferred to an oven for further drying. After drying in the oven, a negative electrode semi-finished product is obtained. Then, the negative electrode semi-finished product is cold-pressed and cut to obtain the negative electrode sheet to be assembled.

[0059] 2.3 Cell Assembly

[0060] The above-mentioned positive electrode sheet, negative electrode sheet and dry separator are wound together to obtain a bare cell.

[0061] 3. Preparation of lithium batteries

[0062] The bare cells were packaged, injected with electrolyte, allowed to stand, formed, and tested for capacity to produce a pouch cell. The electrolyte used was a commercially available electrolyte.

[0063] Example 2

[0064] 1. Preparation of dry-process membranes

[0065] The tear-resistant slurry comprises the following raw materials in parts by weight:

[0066] 11 parts of polymethyl methacrylate with a molecular weight of 200,000-1,000,000 Da.

[0067] 65 parts boehmite, 12 parts nanocellulose

[0068] 10 parts polyacrylic acid

[0069] Two parts of polyvinyl ether,

[0070] 330 portions of deionized water;

[0071] Polymethyl methacrylate, boehmite, nanocellulose, polyacrylic acid, polyethylene ether, and deionized water were mixed at 800 rpm and stirred for 35 min to obtain a tear-resistant slurry with a solid content of 28%, a pH of 8.0, a viscosity of 70 cp, and an average particle size of 0.5 μm.

[0072] The above-mentioned tear-resistant slurry was coated on one side of a polyethylene diaphragm and dried at 55°C for 25 minutes to generate a tear-resistant coating on the surface of the polyethylene diaphragm, resulting in a dry-process diaphragm with a thickness of 12 μm; wherein, the thickness of the polyethylene diaphragm and the thickness of the tear-resistant coating in the dry-process diaphragm are 5:1.

[0073] 2. Cell fabrication

[0074] 2.1. Preparation of the positive electrode sheet

[0075] The positive electrode slurry was prepared as follows: LFP positive electrode active material: conductive agent acetylene black: binder PVDF = 97.9:0.9:1.2 by mass and added to a vacuum mixer for mixing. Then, solvent NMP was added to the mixed slurry and stirred until homogeneous under the action of a vacuum mixer, thereby obtaining the positive electrode slurry of this embodiment.

[0076] The above-mentioned positive electrode slurry is uniformly coated on both surfaces of the positive electrode current collector aluminum foil. After drying at room temperature, it is transferred to an oven for further drying. After drying in the oven, a positive electrode semi-finished product is obtained. Then, the positive electrode semi-finished product is cold-pressed and cut to obtain the positive electrode sheet to be assembled.

[0077] 2.2. Preparation of negative electrode sheet

[0078] The negative electrode slurry was prepared as follows: artificial graphite, conductive agent acetylene black, thickener CMC, and binder SBR were mixed in a vacuum mixer at a mass ratio of 96.4:1:1.2:1.4. Then, deionized water was added to the resulting mixture, and the mixture was stirred in a vacuum mixer until it became homogeneous, thus obtaining the negative electrode slurry of this embodiment.

[0079] The above-mentioned negative electrode slurry is uniformly coated on both surfaces of the negative electrode current collector copper foil. After drying at room temperature, it is transferred to an oven for further drying. After drying in the oven, a negative electrode semi-finished product is obtained. Then, the negative electrode semi-finished product is cold-pressed and cut to obtain the negative electrode sheet to be assembled.

[0080] 2.3 Cell Assembly

[0081] The above-mentioned positive electrode sheet, negative electrode sheet and dry separator are wound together to obtain a bare cell.

[0082] 3. Preparation of lithium batteries

[0083] The bare cells were packaged, injected with electrolyte, allowed to stand, formed, and tested for capacity to produce a pouch cell. The electrolyte used was a commercially available electrolyte.

[0084] Example 3

[0085] 1. Preparation of dry-process membranes

[0086] The tear-resistant slurry comprises the following raw materials in parts by weight:

[0087] 11 parts of polyarylamide with a molecular weight of 200,000-1,000,000 Da.

[0088] 65 parts boehmite, 12 parts nanocellulose

[0089] 10 parts polyacrylate,

[0090] 2 parts polyvinyl alcohol,

[0091] 280 parts of N-methylpyrrolidone

[0092] Polyarylamide, boehmite, nanocellulose, polyacrylate, polyvinyl alcohol, and N-methylpyrrolidone were mixed under stirring at 900 rpm for 30 min to obtain a tear-resistant slurry with a solid content of 32%, a pH of 9.0, a viscosity of 50 cp, and an average particle size of 0.3 μm.

[0093] The above-mentioned tear-resistant slurry was coated on one side of a polypropylene membrane, and then excess solvent N-methylpyrrolidone was removed by water bath. The membrane was then dried at 65°C for 15 min to generate a tear-resistant coating on the surface of the polypropylene membrane, resulting in a dry membrane with a thickness of 16 μm. The ratio of the thickness of the polypropylene membrane to the thickness of the tear-resistant coating in the dry membrane was 7:1.

[0094] 2. Cell fabrication

[0095] 2.1. Preparation of the positive electrode sheet

[0096] The positive electrode slurry was prepared as follows: LFP positive electrode active material: conductive agent acetylene black: binder PVDF = 97.9:0.9:1.2 by mass and added to a vacuum mixer for mixing. Then, solvent NMP was added to the mixed slurry and stirred until homogeneous under the action of a vacuum mixer, thereby obtaining the positive electrode slurry of this embodiment.

[0097] The above-mentioned positive electrode slurry is uniformly coated on both surfaces of the positive electrode current collector aluminum foil. After drying at room temperature, it is transferred to an oven for further drying. After drying in the oven, a positive electrode semi-finished product is obtained. Then, the positive electrode semi-finished product is cold-pressed and cut to obtain the positive electrode sheet to be assembled.

[0098] 2.2. Preparation of negative electrode sheet

[0099] The negative electrode slurry was prepared as follows: artificial graphite, conductive agent acetylene black, thickener CMC, and binder SBR were mixed in a vacuum mixer at a mass ratio of 96.4:1:1.2:1.4. Then, deionized water was added to the resulting mixture, and the mixture was stirred in a vacuum mixer until it became homogeneous, thus obtaining the negative electrode slurry of this embodiment.

[0100] The above-mentioned negative electrode slurry is uniformly coated on both surfaces of the negative electrode current collector copper foil. After drying at room temperature, it is transferred to an oven for further drying. After drying in the oven, a negative electrode semi-finished product is obtained. Then, the negative electrode semi-finished product is cold-pressed and cut to obtain the negative electrode sheet to be assembled.

[0101] 2.3 Cell Assembly

[0102] The above-mentioned positive electrode sheet, negative electrode sheet and dry separator are wound together to obtain a bare cell.

[0103] 3. Preparation of lithium batteries

[0104] The bare cells were packaged, injected with electrolyte, allowed to stand, formed, and tested for capacity to produce a pouch cell. The electrolyte used was a commercially available electrolyte.

[0105] Example 4

[0106] 1. Preparation of dry-process membranes

[0107] The tear-resistant slurry comprises the following raw materials in parts by weight:

[0108] 11 parts of a polyamide polymer with a molecular weight of 200,000-1,000,000 Da.

[0109] 65 portions of boehmite and 7 portions of halloysite tubes with a length-to-diameter ratio of 10:1.

[0110] 10 parts polyacrylic acid

[0111] Two parts of polyvinyl ether,

[0112] 300 parts deionized water

[0113] Polyamide polymer, boehmite, halloysite tube, polyacrylic acid, polyethylene ether, and deionized water were mixed at 1000 rpm and stirred for 25 min to obtain a tear-resistant slurry with a solid content of 31%, a pH of 8.5, a viscosity of 50 cp, and an average particle size of 0.7 μm.

[0114] The above-mentioned tear-resistant slurry was coated on both sides of a polyethylene diaphragm and dried at 60°C for 25 minutes to generate a tear-resistant coating on the surface of the polyethylene diaphragm, resulting in a dry-process diaphragm with a thickness of 15 μm; wherein, the thickness of the polyethylene diaphragm and the thickness of the tear-resistant coating in the dry-process diaphragm are 7:1.

[0115] 2. Cell fabrication

[0116] 2.1. Preparation of the positive electrode sheet

[0117] The positive electrode slurry was prepared as follows: LFP positive electrode active material: conductive agent acetylene black: binder PVDF = 97.9:0.9:1.2 by mass and added to a vacuum mixer for mixing. Then, solvent NMP was added to the mixed slurry and stirred until homogeneous under the action of a vacuum mixer, thereby obtaining the positive electrode slurry of this embodiment.

[0118] The above-mentioned positive electrode slurry is uniformly coated on both surfaces of the positive electrode current collector aluminum foil. After drying at room temperature, it is transferred to an oven for further drying. After drying in the oven, a positive electrode semi-finished product is obtained. Then, the positive electrode semi-finished product is cold-pressed and cut to obtain the positive electrode sheet to be assembled.

[0119] 2.2. Preparation of negative electrode sheet

[0120] The negative electrode slurry was prepared as follows: artificial graphite, conductive agent acetylene black, thickener CMC, and binder SBR were mixed in a vacuum mixer at a mass ratio of 96.4:1:1.2:1.4. Then, deionized water was added to the resulting mixture, and the mixture was stirred in a vacuum mixer until it became homogeneous, thus obtaining the negative electrode slurry of this embodiment.

[0121] The above-mentioned negative electrode slurry is uniformly coated on both surfaces of the negative electrode current collector copper foil. After drying at room temperature, it is transferred to an oven for further drying. After drying in the oven, a negative electrode semi-finished product is obtained. Then, the negative electrode semi-finished product is cold-pressed and cut to obtain the negative electrode sheet to be assembled.

[0122] 2.3 Cell Assembly

[0123] The above-mentioned positive electrode sheet, negative electrode sheet and dry separator are wound together to obtain a bare cell.

[0124] 3. Preparation of lithium batteries

[0125] The bare cells were packaged, injected with electrolyte, allowed to stand, formed, and tested for capacity to produce a pouch cell. The electrolyte used was a commercially available electrolyte.

[0126] Example 5

[0127] The difference between this embodiment and Embodiment 1 is that, in the process of preparing the tear-resistant slurry, the molecular weight of polyvinylidene fluoride is 100,000-180,000 Da;

[0128] In this embodiment, the anti-tear slurry has a solid content of 30%, a viscosity of 30 cp, and an average particle size of 0.8 μm; the rest are consistent with those in Example 1.

[0129] Example 6

[0130] The difference between this embodiment and Embodiment 1 is that, in the process of preparing the tear-resistant slurry, the molecular weight of polyvinylidene fluoride is 2,100,000-2,500,000 Da.

[0131] In this embodiment, the anti-tear slurry has a solid content of 30%, a viscosity of 120 cp, and an average particle size of 0.8 μm; the rest are consistent with those in Example 1.

[0132] Comparative Example 1

[0133] The difference between this comparative example and Example 1 is that the dry-process diaphragm in this comparative example does not contain an anti-tear coating, while the rest is consistent with Example 1.

[0134] Comparative Example 2

[0135] The difference between this comparative example and Example 1 is that an equal weight of alumina is used instead of halloysite tubes in Example 1; all other parts are consistent with Example 1.

[0136] Comparative Example 3

[0137] The difference between this comparative example and Example 1 is that the length-to-diameter ratio of the halloysite tube is 2:1 during the preparation of the tear-resistant slurry; the rest is the same as in Example 1.

[0138] Comparative Example 4

[0139] The difference between this comparative example and Example 1 is that the length-to-diameter ratio of the halloysite tube is 15:1 during the preparation of the tear-resistant slurry; the rest is the same as in Example 1.

[0140] Comparative Example 5

[0141] The difference between this comparative example and Example 3 is that, in the process of preparing the tear-resistant slurry, the thickness of the boehmite with a lamellar structure is 0.2 μm; the rest is the same as in Example 3.

[0142] Comparative Example 6

[0143] The difference between this comparative example and Example 3 is that, in the process of preparing the tear-resistant slurry, the thickness of the boehmite with a lamellar structure is 1.5 μm; the rest is the same as in Example 3.

[0144] Test methods

[0145] I. Tensile strength and elongation at break tests

[0146] The dry-process separators in the above embodiments and comparative examples were subjected to tensile strength tests. The specific test methods were in accordance with GB / T36363-2018 "Polyolefin Separators for Lithium-ion Batteries".

[0147] II. Heat Shrinkage Rate Test

[0148] The dry-process diaphragms in the above embodiments and comparative examples were subjected to heat shrinkage rate testing. The specific testing method was as follows: the dry-process diaphragms were stacked into 3 layers, flattened, and the air between the membranes was expelled. A sample board (300×100) was taken out, and the diaphragm sample was cut out. The length A1 and width B1 of the cut sample were measured. The oven temperature was set to 90℃. After the temperature reached 90℃, it was kept at that temperature for 1 hour. The sample was then placed in the oven and kept at that temperature for 2 hours. After the holding time was over, the diaphragm was taken out and cooled for 10 minutes. The length A2 and width B2 of the sample were then measured.

[0149] Transverse thermal shrinkage of the diaphragm (TD) = (A1-A2) / A1×100%

[0150] Longitudinal thermal shrinkage of the diaphragm (MD) = (B1-B2) / B1 × 100%.

[0151] III. Impact Test

[0152] The lithium batteries in the above embodiments and comparative examples were subjected to heavy object impact tests. The specific test method referred to GB31241-2014 "Safety Requirements for Ion Batteries and Battery Packs for Portable Electronic Products". After the lithium batteries were fully charged according to the specified test method, the batteries were placed on the surface of the platform. A metal rod with a diameter of 15.8 mm ± 0.2 mm was placed horizontally on the upper surface of the battery's geometric center. A weight of 9.1 kg ± 0.1 kg was dropped from a height of 610 mm ± 25 mm to impact the surface of the battery with the metal rod placed on it, and the results were observed for 6 hours. For cylindrical batteries, the longitudinal axis should be parallel to the surface of the weight, and the metal rod should be perpendicular to the longitudinal axis of the battery. For prismatic batteries and soft-pack batteries, only the wide side was impacted. For button batteries, the metal rod was placed across the center of the battery surface. Each sample was subjected to only one impact test.

[0153] IV. Overcharge Performance Test

[0154] Overcharge performance tests were conducted on the lithium batteries in the above embodiments and comparative examples. The specific test methods were based on the overcharge test in GB / T36276-2018 "Lithium-ion Batteries for Power Storage".

[0155] Table 1. Diaphragm Performance Test Table

[0156]

[0157] Based on Examples 1-4, Comparative Examples 1-2, and Table 1, it can be seen that by using inorganic substances containing hydroxyl groups in the tear-resistant slurry, hydrogen bonds can be generated by reacting with the binder, thereby regulating the intermolecular forces in the tear-resistant slurry. At the same time, after the inorganic substances react with the binder, they can be distributed more evenly among the polymer molecules to form a structure, which increases the flexibility of the separator and improves the elongation at break of the separator in the TD transverse direction. This solves the tearing problem of dry-process separators. Correspondingly, the lithium battery has strong impact resistance and stable overcharge performance.

[0158] Based on Examples 1, 3-6, and Table 1, it can be seen that when the aspect ratio of the tubular inorganic material is too high or too low, or the thickness of the layered inorganic material is too high or too low, it is not conducive to the bonding of the inorganic material with the tear-resistant slurry and the binder. The dispersion uniformity in the tear-resistant slurry decreases, which is not conducive to the uniform distribution of the inorganic material in the polymer molecular chain segments. This leads to a decrease in the relevant performance of the separator, and consequently, a deterioration in the safety performance and overcharge performance of the lithium battery.

[0159] Based on Examples 1, 5-6 and Table 1, it can be seen that when the molecular weight of the polymer is too high or too low, it is not conducive to the formation of a stable three-dimensional network structure in the tear-resistant slurry, which reduces the relevant performance of the separator. Consequently, the safety performance and overcharge performance of the lithium battery deteriorate.

[0160] Based on Examples 1-4, Comparative Examples 7-8, and Table 1, it can be seen that when the solid content and viscosity of the tear-resistant slurry do not meet the above-mentioned limits, on the one hand, the bonding between the components in the tear-resistant slurry is poor; on the other hand, the coating operation of the tear-resistant slurry on the polypropylene separator becomes more difficult, the bonding between the tear-resistant coating and the polypropylene separator is poor, and the improvement effect on the tensile strength, elongation at break, and thermal shrinkage rate of the separator is not significant, thus reducing the impact resistance and overcharge performance of the lithium battery.

[0161] Based on Examples 1, 9-10, and Table 1, it can be seen that when the thickness ratio of the tear-resistant coating to the porous substrate is too low, the contribution to improving the tensile strength of the dry-process separator is limited. However, when the thickness ratio of the tear-resistant coating to the porous substrate is too high, although the various properties of the dry-process separator can still be maintained at a relatively good level, the wettability of the separator decreases slightly, which is not conducive to improving the electrochemical performance of the lithium battery.

[0162] The above embodiments are only used to illustrate the technical solutions of the present invention and are not intended to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the above embodiments, those skilled in the art should understand that modifications or equivalent substitutions can be made to the technical solutions of the present invention, but such modifications or substitutions are all within the scope of protection of the present invention.

Claims

1. A dry method separator, characterized by: The dry membrane includes a porous substrate layer and a tear-resistant coating applied to at least one surface of the porous substrate layer; The tear-resistant coating includes a tear-resistant slurry, which comprises a polymer, an inorganic substance, a binder, and a solvent; wherein the inorganic substance contains hydroxyl groups, and the binder contains hydroxyl groups. The inorganic material is composed of tubular and sheet-like structures. The tubular structures include halloysite tubes. The aspect ratio of the tubular structures is 5:1-10:

1. The thickness of the sheet-like structures is 0.6-1 μm. The molecular weight of the polymer is 200,000-1,000,000 Da. The polymer includes at least one of polyarylamide, polyimide, polymethyl methacrylate, and polyvinylidene fluoride. The porous substrate layer is prepared by a dry process.

2. The dry-process diaphragm according to claim 1, characterized in that: The inorganic material also includes boehmite.

3. A dry-process diaphragm according to claim 1, characterized in that: The adhesive includes at least one of polyacrylic acid, polyacrylate, polyacrylonitrile, and terpolymer adhesive.

4. A dry-process diaphragm according to claim 1, characterized in that: The anti-tear slurry has a solid content of 28%-32%, a viscosity of <80cp, a pH of 7.5-9.0, and an average particle size D50 of <1μm.

5. A dry-process diaphragm according to claim 1, characterized in that: The thickness of the dry-process diaphragm is 10-18 μm, and the thickness ratio of the porous substrate layer to the tear-resistant coating is 5-20:

1.

6. A method for preparing a dry-process separator according to any one of claims 1-5, characterized in that: Includes the following steps: S1: The polymer, the inorganic substance, the binder, and the solvent are mixed under stirring to obtain the tear-resistant slurry; wherein the tear-resistant slurry further includes a dispersant accounting for 0.5wt%-3wt% of the mass of the tear-resistant slurry; S2: The tear-resistant slurry is coated on at least one surface of the porous substrate, and then the solvent is removed and dried to obtain the dry membrane.

7. The method for preparing a dry-process diaphragm according to claim 6, characterized in that: In the tear-resistant slurry, the mass ratio of the polymer, the inorganic material and the binder is 10-70:40-80:0.1-10.

8. A lithium-ion battery, characterized in that: The lithium-ion battery includes a positive electrode, a negative electrode, and a dry separator as described in any one of claims 1-5.

Citation Information

Patent Citations

  • Inorganic ceramic coated functional lithium ion battery diaphragm, preparation method and lithium ion battery thereof

    CN108963164A

  • Isolating membrane, preparation method thereof, and related secondary battery and electric device

    CN116897461A