Silicone gel composition, silicone gel and application thereof
By adding high-pigment carbon black and modified multi-walled carbon nanotubes to the silicone gel, the problem of indentation of the silicone gel during impact is solved, the buffering performance and conductive properties are improved, and a better protection effect is achieved.
Patent Information
- Application Number
- CN202311729263.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-14
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2043-12-14
AI Technical Summary
Existing silicone gel may have indentations when it is impacted, affecting the display effect. When the hardness is increased to improve the indentation problem, the cushioning performance and adhesive force will decrease.
A controlled amount of high-pigment carbon black and modified multi-walled carbon nanotubes are added to the silica gel to improve the buffering properties of the silica gel through the light absorption effect of the high-pigment carbon black and the bridging effect of the modified multi-walled carbon nanotubes. and conductive properties.
It improves the indentation effect without reducing the buffering performance, and gives the silicone gel good conductive properties, improving the overall protective performance.
Smart Images

Figure BDA0004612308940000071 
Figure BDA0004612308940000221 
Figure BDA0004612308940000231
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of silicone gel, and in particular to a silicone gel composition, silicone gel and applications thereof. Background Art
[0002] With the rapid development of science and technology, people's requirements for electronic display devices such as mobile phones and tablets are also increasingly tending towards lightweight, ultra-thin and bendable, which makes the protection components of display modules more stringent. At present, there are two main ways to protect common display modules. One is to use buffer foam tape, attach glue on both sides of the foam, and bond and fix the lower copper foil, aluminum foil and other fixed layers to the upper display module. However, this solution not only has a complicated assembly process and weak buffer protection performance, but also the inherent pore structure of the foam will be reflected on the screen, affecting the display effect; the second is to use silicone gel, which has a one-time molding process, high assembly efficiency, excellent buffering performance and large adjustment space, and gradually becomes a new development direction of the industry. Silicone gel is a viscoelastic body. When electronic products are impacted by external forces, the colloid can be squeezed and deformed to offset and absorb part of the external force, reduce the impact of the external force on the display module, and thus achieve a protective effect. After the impact force ends, the colloid will automatically return to its original state. However, if the silicone gel is subjected to a large impact locally, residual deformation may occur, forming indentations, and these indentations may be reflected on the external screen, affecting the display effect.
[0003] In order to solve the problem of silicone gel being prone to indentation, the existing technology has adopted different solutions to improve it. For example, increasing the hardness of the colloid can improve the indentation problem to a certain extent, but after the hardness of the colloid is increased, the adhesion of the colloid is reduced. In addition, its cushioning performance is also greatly reduced. For example, polyethylene terephthalate (PET) film or thermoplastic polyurethane elastomer (TPU) is introduced into the cushioning colloid, and the film print is controlled by the PET film and TPU elastomer. However, since the PET film and TPU elastomer have low energy absorption when impacted, the cushioning performance will also be reduced.
[0004] Therefore, it is of great significance to develop a silicone gel that can improve both indentation and cushioning effects. Summary of the invention
[0005] The purpose of the present invention is to overcome the above problems existing in the prior art and provide a silicone gel composition, silicone gel and application thereof. By adding a controlled amount of high-pigment carbon black and modified multi-walled carbon nanotubes to the silicone gel, the silicone gel can improve both the indentation and the buffering effect, and also give the silicone gel good conductive properties.
[0006] In order to achieve the above object, the first aspect of the present invention provides a silicone gel composition, which comprises the following components in parts by weight:
[0007] Color paste masterbatch: 1-20 parts;
[0008] Modified multi-walled carbon nanotube slurry: 1-20 parts;
[0009] First vinyl silicone oil: 0-20 parts;
[0010] Olefin polysiloxane: 15-60 parts;
[0011] Methyl MQ resin: 50-100 parts;
[0012] Vinyl MQ resin: 0-20 parts;
[0013] Cross-linking agent: 1-5 parts;
[0014] Inhibitor: 0.1-2 parts;
[0015] Catalyst: 1-5 parts;
[0016] First solvent: 100-500 parts;
[0017] Wherein, the color paste masterbatch contains high-pigment carbon black.
[0018] The inventors of the present invention have found that, on the one hand, by adding a certain amount of high-pigment carbon black to silicone gel to prepare black silicone gel, the light transmittance and brightness of the silicone gel can be reduced, the absorption of light can be enhanced, the reflection of the film printing position can be reduced, and the visual effect of the film printing can be reduced; and when the colloid is deformed by impact, the high-pigment carbon black particles squeeze and slide against each other, the internal friction is enhanced, the internal loss is increased, and the buffering effect can be increased. On the other hand, adding a certain amount of modified multi-walled carbon nanotubes (MWCNTs) to the silicone gel, so that the modified multi-walled carbon nanotubes participate in the cross-linking reaction of the silicone gel, and the multi-walled carbon nanotubes are used to connect more colloidal structures in series, which can improve the overall buffering performance of the silicone gel, and the multi-walled carbon nanotubes involved in cross-linking can improve the strength and toughness of the colloid, and reduce the indentation to a certain extent. Therefore, the silicone gel of the present invention can achieve both improvement of indentation and buffering effect.
[0019] Furthermore, the inventors of the present invention have also discovered that the synergistic combination of high-pigment carbon black and modified multi-walled carbon nanotubes, using MWCNTs and high-pigment carbon black to build a framework structure and open up a conductive path can give silicone gel good conductive properties.
[0020] In the present invention, the primary particle size of the high-pigment carbon black is less than 17nm; the primary particle size of the medium-pigment carbon black is 18-27nm; and the primary particle size of the low-pigment carbon black is greater than 41nm. Generally, the smaller the particle size, the larger the specific surface area, and the higher the blackness. The high-pigment carbon black used in the present invention has a darker blackness and can play a better light absorption role.
[0021] In some embodiments, the high-color carbon black can be selected from ORION FW255 of Orion Corporation, #2350 of Mitsubishi Chemical Corporation, MONARCH 1300 of Cabot Corporation, and the like.
[0022] In some embodiments, based on the total weight of the color paste masterbatch being 100wt%, the color paste masterbatch includes: 5-30wt% of high-pigment carbon black, 67-94.5wt% of the second vinyl silicone oil, and 0.5-3wt% of a dispersing aid. High-pigment carbon black particles have poor direct dispersibility and often exist in the form of agglomerates and coagulations, resulting in a larger particle size. In the present invention, the color masterbatch is prepared by a dispersing aid, vinyl silicone oil, and a grinding process, breaking the original agglomeration and aggregation structure. At the same time, the average particle size of the high-pigment carbon black in the color paste masterbatch is limited to less than 15μm, so that the silicone gel can achieve a better appearance and light absorption performance.
[0023] In some embodiments, based on the total weight of the color paste masterbatch, the content of the high-pigment carbon black is 5-30wt%, for example, 5wt%, 10wt%, 12wt%, 15wt%, 18wt%, 20wt%, 25wt%, 30wt%. When the content of the high-pigment carbon black is within the above range, the high-pigment carbon black can be dispersed more evenly, the color of the silicone gel can be more uniform, and the effect of improving and reducing film printing can be better. The content of the high-pigment carbon black is preferably 15-30wt%.
[0024] In the present invention, the viscosity of the second vinyl silicone oil is 50-1,000cps. In some embodiments, the viscosity of the second vinyl silicone oil is 50cps, 100cps, 300cps, 500cps, 600cps, 700cps, 800cps, 850cps, 900cps, 1,000cps, or any value between the two end values. The second vinyl silicone oil in the present invention adopts low-viscosity silicone oil to facilitate uniform dispersion of high-pigment carbon black.
[0025] In some embodiments, based on the total weight of the color paste masterbatch, the content of the second vinyl silicone oil is 67-94.5wt%, for example, it can be 67wt%, 74wt%, 80wt%, 85wt%, 90wt%, 94.5wt%, or any value between the two end values.
[0026] In some embodiments, the dispersing aid may be selected from BYK-2096, BYK-2022, BYK-2117 and the like of BYK Chemical.
[0027] In some embodiments, based on the total weight of the color paste masterbatch, the content of the dispersing aid is 0.5-3wt%, for example, it can be 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, or any value between the two end values.
[0028] In some embodiments, the modified multi-walled carbon nanotube slurry includes component A and a second solvent. The content of the second solvent is 100-300 parts relative to 100 parts of component A. Taking the total weight of component A as 100wt%, component A includes: 3-16wt% of carboxylated multi-walled carbon nanotubes, 0.5-5wt% of silane coupling agent, and 79-96.5wt% of a third vinyl silicone oil. Since multi-walled carbon nanotubes have a large aspect ratio, they are prone to agglomeration when directly added to silicone gel. Therefore, the silane coupling agent is first used to react with the carboxyl groups on the surface of the carboxylated multi-walled carbon nanotubes for modification. The modified multi-walled carbon nanotubes have better dispersibility and have active groups on the surface, which can participate in the cross-linking reaction of silicone gel and improve the buffering performance of silicone gel.
[0029] Carboxylated multi-walled carbon nanotubes refer to multi-walled carbon nanotubes containing carboxyl groups (-COOH) on the surface. Carboxylated multi-walled carbon nanotubes contain carboxyl active groups, which facilitate subsequent modification reactions with silane coupling agents, thereby ensuring the degree of subsequent participation in cross-linking reactions.
[0030] In some embodiments, the average length of the carboxylated multi-walled carbon nanotubes can be limited to, for example, 3 μm-30 μm, illustratively 3 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, or any value in between.
[0031] In some embodiments, based on the total weight of component A being 100wt%, the content of the carboxylated multi-walled carbon nanotubes is 3-16wt%, for example, 3wt%, 6wt%, 10wt%, 13wt%, 16wt%, or any value between the two end values. When the content of the carboxylated multi-walled carbon nanotubes is within the above range, its dispersion can be better promoted and the buffering effect of the silicone gel can be better improved.
[0032] In the present invention, the silane coupling agent is selected from at least one of a methacrylic acid acyloxy silane coupling agent, a vinyl silane coupling agent, and an epoxy silane coupling agent, such as γ-methacryloxypropyltrimethoxysilane (KH-570), vinyltrimethoxysilane (KH-171), and γ-(2,3-epoxypropoxy)propyltrimethoxysilane (KH-560).
[0033] In some embodiments, based on the total weight of component A as 100wt%, the content of the silane coupling agent accounts for 0.5-5wt%, for example, it can be 0.5wt%, 1wt%, 1.5wt%, 2wt%, 2.5wt%, 3wt%, 3.5wt%, 4wt%, 4.5wt%, 5wt%, or any value between the two end values.
[0034] In some embodiments, the viscosity of the third vinyl silicone oil is 50-1,000cps, illustratively 50cps, 100cps, 150cps, 300cps, 500cps, 800cps, 1,000cps, or any value between the two end values. The viscosity of the third vinyl silicone oil is low viscosity. Since the carboxylated multi-walled carbon nanotubes have a large aspect ratio and are added in large amounts, if the viscosity of the third vinyl silicone oil is too low or too high, it is not conducive to subsequent multi-walled carbon nanotube grinding and dispersion. The present invention limits the viscosity of the third vinyl silicone oil within this range, so that the multi-walled carbon nanotubes can be evenly dispersed.
[0035] In some embodiments, based on the total weight of component A as 100wt%, the content of the third vinyl silicone oil accounts for 79-96.5wt%, exemplarily 79wt%, 83wt%, 85wt%, 88wt%, 90wt%, 96.5wt%, or any value in between.
[0036] In some embodiments, the second solvent may be selected from toluene. Relative to 100 parts of component A, the second solvent content is 100-300 parts, illustratively 100 parts, 150 parts, 200 parts, 250 parts, 300 parts, or any value between the two end values.
[0037] In some embodiments, the viscosity of the first vinyl silicone oil is 500 cps-20,000 cps, illustratively 500 cps, 1,000 cps, 2,000 cps, 5,000 cps, 10,000 cps, 15,000 cps, 20,000 cps, or any value therebetween.
[0038] In some embodiments, the vinyl content of the first vinyl silicone oil is 0.06-0.5%, exemplarily 0.06%, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, or any value in between.
[0039] In some embodiments, the first vinyl silicone oil is a polysiloxane containing a vinyl group, and the vinyl distribution can be only terminal vinyl or terminal and side vinyl. The content and viscosity of the vinyl in the first vinyl silicone oil can be limited to further improve the strength, flexibility and adhesion of the silicone gel.
[0040] In some embodiments, the amount of the first vinyl silicone oil added is 0-20 parts, exemplarily 0 parts, 1 parts, 5 parts, 10 parts, 15 parts, 20 parts, or any value between the two end values. The first vinyl silicone oil may not be added in the present invention. When the first vinyl silicone oil is not added, the colloid strength will decrease. If it is necessary to meet certain application scenarios with higher strength requirements, the first vinyl silicone oil of the limited number of parts of the present invention may be selectively added.
[0041] In some embodiments, the chemical structure of the olefin-based polysiloxane is shown in Formula I below:
[0042]
[0043] Wherein, R1 is an alkane group of 1 to 8 carbon atoms, R2 is an unsaturated olefin group of 1 to 8 carbon atoms, m is any integer between 200 and 8,000, and n is any integer between 0 and 500.
[0044] In some embodiments, the viscosity-average molecular weight of the olefin-based polysiloxane is 600,000-750,000, for example, 600,000, 620,000, 650,000, 700,000, or 750,000; the olefin-based content is 0.03-0.30 mol%, for example, 0.03 mol%, 0.05 mol%, 0.09 mol%, 0.10 mol%, 0.12 mol%, 0.15 mol%, 0.22 mol%, or 0.30 mol%.
[0045] Long-chain olefin-based polysiloxane is the base polymer of silicone gel. When the viscosity-average molecular weight and olefin content of the olefin-based polysiloxane are limited to the above ranges, the cross-linking density can be adjusted to balance the cushioning performance and indentation effect of the silicone gel.
[0046] In some preferred embodiments, the olefin-based polysiloxane is a vinyl polysiloxane, that is, R1 is a methyl group, R2 is a vinyl group, m is any integer between 4,000-7,500, and n is any integer between 0-50.
[0047] Vinyl polysiloxane is further preferred, and the viscosity-average molecular weight and vinyl content of the vinyl polysiloxane are limited to the above ranges, so as to better exert the cross-linking polymerization effect of the vinyl polysiloxane (base polymer) and other components, and further improve the overall performance of the silicone gel.
[0048] In some embodiments, the amount of the olefin-based polysiloxane added is 15-60 parts, illustratively 15 parts, 20 parts, 30 parts, 40 parts, 45 parts, 50 parts, 55 parts, 60 parts, or any value in between.
[0049] In the present invention, MQ resin is composed of monofunctional chain segments (R3SiO 1 / 2 M unit for short) and tetrafunctional chain segment (SiO 4 / 2 The structure ratio of the polysiloxane is a special organic / inorganic hybrid polysiloxane.
[0050] In some embodiments, the molecular formula of methyl MQ resin is (Me3SiO 0.5 ) a (SiO2), wherein a is 0.6 to 0.9 and the hydroxyl content is <1.0%.
[0051] In some embodiments, the methyl MQ resin is 50 to 100 parts, illustratively 50 parts, 60 parts, 75 parts, 80 parts, 90 parts, 100 parts, or any value in between.
[0052] In some embodiments, the molecular formula of the vinyl MQ resin is (Me3SiO 0.5 ) a (ViMe2SiO 0.5 ) b (SiO2), a=0.5~0.9, b=0~0.3, a+b=0.6~0.9, vinyl content is 0.5-3.0%.
[0053] In some embodiments, the vinyl MQ resin is 0 to 20 parts, illustratively 0 parts, 1 parts, 3 parts, 10 parts, 15 parts, 20 parts, or any value in between.
[0054] In the present invention, vinyl MQ resin may not be added. The main function of vinyl MQ resin is to improve the hardness and strength of the colloid. If it is necessary to meet some high-strength colloid application scenarios, the above-mentioned proportion of vinyl MQ resin may be added. The synergistic use of methyl MQ resin and vinyl MQ resin can better improve the adhesion and colloid strength of silicone gel.
[0055] In some embodiments, the crosslinking agent is hydrogen-containing silicone oil. As a crosslinking agent for silicone gel, hydrogen-containing silicone oil determines the type of crosslinking bonds and the crosslinking density, and has a decisive influence on the product performance of silicone gel. Preferably, the hydrogen content of the hydrogen-containing silicone oil is 0.8-1.6%, exemplarily 0.8%, 0.9%, 1.0%, 1.2%, 1.5%, 1.6%. An addition crosslinking reaction can occur between the silicon hydrogen group in the hydrogen-containing silicone oil and the vinyl group in the vinyl silicone oil. Limiting the amount of hydrogen-containing silicone oil added and the hydrogen content can improve the crosslinking degree of silicone gel and enhance the buffering performance. The hydrogen-containing silicone oil can, for example, be SYL-OFF from Dow Chemical Company. TM SL-7028.
[0056] In some embodiments, the amount of the cross-linking agent added is 1 to 5 parts, exemplified by 1 part, 1.37 parts, 2 parts, 2.25 parts, 3.6 parts, 5 parts, or any value in between.
[0057] In some embodiments, the inhibitor is selected from acetylenic alcohol compounds, such as methyl butynol, ethynyl cyclohexanol, 2-phenyl-3-butyn-2-ol, 3,6-dimethyl-1-heptyn-3-ol, 3,5-dimethyl-1-hexyn-3-ol, 3,7,11-trimethyldodecyn-3-ol (TMDO), and the like.
[0058] In some embodiments, the inhibitor is added in an amount of 0.1 to 2 parts, exemplarily 0.1 parts, 0.27 parts, 0.45 parts, 0.68 parts, 1 parts, 1.5 parts, 2 parts, or any value in between.
[0059] In some embodiments, the catalyst is selected from a complex of a transition metal, such as a complex of a transition metal platinum, rhodium, etc., preferably a platinum catalyst, such as SYL-OFF TM 4000Catalyst.
[0060] In some embodiments, the catalyst is added in an amount of 1 to 5 parts, exemplified by 1 part, 1.65 parts, 2 parts, 2.7 parts, 4.2 parts, 5 parts, or any value in between.
[0061] In some embodiments, the first solvent is selected from one or more of toluene, xylene, and ethyl acetate. In the present invention, the first solvent is a mixture of toluene and ethyl acetate. The use of two solvents with different boiling points can have good leveling performance and curing effect, thereby improving the appearance effect of the silicone gel and the uniformity of product performance.
[0062] In some embodiments, the first solvent is added in an amount of 100 to 500 parts, exemplarily 100 parts, 150 parts, 200 parts, 280 parts, 350 parts, 440 parts, 500 parts, or any value between the two end values. The first solvent of the present invention contains 50-250 parts of toluene and 50-250 parts of ethyl acetate.
[0063] The present invention also provides a method for preparing the silicone gel according to the first aspect of the present invention, which comprises the following steps:
[0064] S1: preparing color paste masterbatch;
[0065] S2: preparing modified multi-walled carbon nanotube slurry;
[0066] S3: uniformly mixing and dispersing the color paste masterbatch, the modified multi-walled carbon nanotube slurry, the olefin-based polysiloxane and the first organic solvent to obtain a first mixture;
[0067] S4: adding vinyl silicone oil, methyl MQ resin, vinyl MQ resin and inhibitor to the first mixture and mixing them uniformly to obtain a second mixture;
[0068] S5: adding the cross-linking agent and the catalyst to the second mixture at a certain interval, mixing them evenly, to obtain a third mixture;
[0069] S6: coating the third mixture and curing it at high temperature.
[0070] The order of S1 and S2 can be adjusted, and each step will be explained in detail below.
[0071] Step S1
[0072] The steps of preparing the color paste masterbatch include: weighing high-pigment carbon black, second vinyl silicone oil and a dispersing aid, and then sequentially performing mechanical stirring pre-dispersion and grinding dispersion.
[0073] In some embodiments, based on the total weight of the color paste masterbatch, the content of the high-pigment carbon black is 5-30wt%, the content of the second vinyl silicone oil is 67-94.5wt%, and the content of the dispersing aid is 0.5-3wt%.
[0074] In some embodiments, the steps of preparing a color paste masterbatch include: (1) adding a second vinyl silicone oil, high-pigment carbon black and a dispersing aid into a container, mechanically stirring and pre-dispersing for 30 to 60 minutes to obtain a pre-dispersed liquid; (3) adding the pre-dispersed liquid into a grinding device, grinding it thoroughly to a fineness of less than 15 μm, and obtaining a color paste masterbatch with a high-pigment carbon black content of 5 to 30 wt%.
[0075] The above method for preparing color paste masterbatch can promote high-pigment carbon black to be more evenly dispersed in silicone gel, making the black color of silicone gel more uniform, thereby improving the visual effect of silicone gel in reducing film printing.
[0076] Step S2
[0077] The steps of preparing modified multi-walled carbon nanotube slurry include: mixing carboxylated multi-walled carbon nanotubes, third vinyl silicone oil and second solvent, heating to reflux, dropping silane coupling agent for modification reaction, and vacuum degassing and grinding.
[0078] In some embodiments, the modified multi-walled carbon nanotube slurry includes component A and a second solvent. Relative to 100 parts of component A, the content of the second solvent is 100-300 parts. Taking the total weight of component A as 100wt%, component A includes: 3-16wt% of carboxylated multi-walled carbon nanotubes, 0.5-5wt% of silane coupling agent, and 79-96.5wt% of a third vinyl silicone oil.
[0079] In some embodiments, the method for preparing a modified multi-walled carbon nanotube slurry includes: (1) adding a second solvent, a third vinyl silicone oil, and carboxylated multi-walled carbon nanotubes to a reaction kettle in sequence, heating and reflux under mechanical stirring; (2) adding a silane coupling agent and reacting for 5 to 10 hours; (3) vacuum degassing (to separate the solvent and small molecules) and cooling; (4) adding the above slurry to a dispersing device for further grinding and dispersion to obtain a slurry with a modified multi-walled carbon nanotube content of 3-16wt%.
[0080] The method for preparing modified multi-walled carbon nanotube slurry first uses a silane coupling agent to react with the carboxyl groups on the surface of the carboxylated multi-walled carbon nanotubes for modification. The modified multi-walled carbon nanotubes have better dispersion properties and can participate in the cross-linking reaction of the silicone gel to improve the buffering properties of the silicone gel.
[0081] Step S3
[0082] The prepared color paste masterbatch, modified multi-walled carbon nanotube slurry, olefin-based polysiloxane as a base polymer and the first solvent are mixed and dispersed uniformly in advance to obtain a first mixture. In this way, the high-color carbon black and the modified multi-walled carbon nanotubes can be better dispersed in the base polymer, which is beneficial to obtaining a silicone gel with a more uniform color and to connecting more colloidal structures in series with the modified multi-walled carbon nanotubes, so that the silicone gel can take into account both improving the indentation and enhancing the buffering effect.
[0083] In some embodiments, step S3 includes: adding a color paste masterbatch, a modified multi-walled carbon nanotube slurry, an olefin-based polysiloxane (e.g., vinyl polysiloxane), and an appropriate amount of a first solvent (e.g., toluene, ethyl acetate, or a mixture of the two) in a planetary agitator in sequence, stirring and dispersing for 2-5 hours to obtain a first mixture, and transferring it to a stirring tank for standby use.
[0084] Step S4
[0085] The first vinyl silicone oil, methyl MQ resin, vinyl MQ resin, an appropriate amount of the first solvent and an inhibitor are added to the first mixture and mixed evenly.
[0086] In some embodiments, the first vinyl silicone oil, methyl MQ resin, vinyl MQ resin, an appropriate amount of the first solvent, and an inhibitor are sequentially added to the first mixture, and the mixture is mechanically stirred for 30 to 60 minutes to obtain a second mixture.
[0087] Step S5
[0088] In the second mixture, the crosslinking agent and the catalyst are added in sequence at a certain interval, for example, at an interval of 3-6 minutes, and after sufficient stirring, a third mixture is obtained, that is, a silicone gel coating solution.
[0089] In some embodiments, a crosslinking agent and a catalyst are added to the second mixture at an interval of 3-6 minutes, and stirring is continued for 30-50 minutes. The mixture is filtered with a filter element to obtain a silicone gel coating solution.
[0090] Step S6
[0091] The coating liquid (third mixture) is coated on the surface of a release film or a substrate, and then cured at high temperature to obtain the silicone gel film of the present invention.
[0092] In some embodiments, a scraper or slot die coating head is used to coat the coating liquid on the release surface of the first release film, and then the coating liquid is cured in an oven at a high temperature of 150-165° C., and a second release film is attached to obtain a silicone gel product.
[0093] In some embodiments, the first release film and the second release film may be the same or different. The first release film and the second release film may be independently selected from fluorine release films.
[0094] The method for preparing silicone gel provided by the present invention has a simple material preparation process, and is formed by coating once, without the need for multiple coating, laminating, transferring and other processes, and has high efficiency and yield.
[0095] The second aspect of the present invention provides a silicone gel, which is obtained by combining the silicone gel composition described in the first aspect of the present invention.
[0096] The third aspect of the present invention provides an application. The silicone gel composition provided in the first aspect of the present invention can be applied to display module bonding or protective films or other electronic products, which can solve the problem of indentation and ensure the buffering effect.
[0097] The present invention adopts the above technical solution to achieve the following beneficial effects:
[0098] (1) The silicone gel composition provided by the present invention can reduce the light transmittance and brightness of the silicone gel, increase the degree of absorption of incident light, reduce the reflection of light, reduce the reflection of the film print position, and thus reduce the influence of the film print on the appearance by adding a certain amount of high-pigment carbon black into the silicone gel. On the other hand, when the colloid is impacted, the internal friction is increased through the squeezing and sliding between the high-pigment carbon black particles, thereby improving the internal loss and increasing the cushioning effect.
[0099] (2) The silicone gel composition provided by the present invention contains a certain amount of modified multi-walled carbon nanotubes that can participate in the cross-linking reaction of the silicone gel. The multi-walled carbon nanotubes can be used to connect more colloidal structures in series by means of the bridging effect, thereby improving the overall buffering performance of the silicone gel. The multi-walled carbon nanotubes that participate in the cross-linking can improve the strength and toughness of the colloid, thereby improving the film print to a certain extent and reducing the impact on the appearance.
[0100] (3) The synergistic combination of the silica gel, high-pigment carbon black and modified carbon nanotubes provided by the present invention can give the silica gel good conductive properties.
[0101] The endpoints and any values of the range disclosed in this article are not limited to the precise range or value, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article. Herein, in the absence of special instructions, data ranges include endpoints. DETAILED DESCRIPTION
[0102] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0103] Unless otherwise defined, all scientific and technical terms used in the present invention have the same meanings as commonly understood by one of ordinary skill in the art to which the present invention relates.
[0104] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0105] The materials and reagents used in the following examples, unless otherwise specified, can be obtained from commercial sources. The first vinyl silicone oil, the second vinyl silicone oil and the third vinyl silicone oil in each example of the present invention were purchased from Zhejiang Runhe Silicone New Materials Co., Ltd., the methyl MQ resin and the vinyl MQ resin were purchased from Shandong Dayi Chemical Co., Ltd., and the vinyl polysiloxane was purchased from Dongjue Silicone Group Co., Ltd.
[0106] The present invention is described in detail below in conjunction with specific embodiments, which are used to understand but not to limit the present invention.
[0107] Example 1
[0108] 1. The composition of silicone gel, by weight, includes the following raw material components:
[0109] Color paste masterbatch, 8 parts;
[0110] Modified multi-walled carbon nanotube slurry, 8 parts;
[0111] First vinyl silicone oil, 8 parts, viscosity 10,000 cps, vinyl content 0.1%;
[0112] Vinyl polysiloxane, 45 parts, viscosity average molecular weight 650,000, vinyl content 0.1 mol%;
[0113] Methyl MQ resin, 75 parts, M:Q ratio 0.75:1;
[0114] Vinyl MQ resin, 3 parts, M:Q ratio 0.75:1, vinyl content 1.2%;
[0115] Crosslinking agent: SYL-OFF TM SL 7028, 2.25 parts;
[0116] Inhibitor: methylbutynol, 0.45 parts;
[0117] Catalyst: SYL-OFF TM 4000Catalyst, 2.7 copies;
[0118] First solvent: toluene, 140 parts; ethyl acetate, 140 parts;
[0119] The composition of color paste masterbatch is as follows:
[0120] High color carbon black: MONARCH 1300, 24wt%,
[0121] The second vinyl silicone oil, viscosity 150cps, 74wt%,
[0122] Dispersing agent: BYK-2096, 2wt%;
[0123] The modified multi-walled carbon nanotube slurry is composed of the following:
[0124] Component A: carboxylated multi-walled carbon nanotubes: average length 18 μm, 13 wt%,
[0125] Silane coupling agent: KH-570, 2wt%,
[0126] The third vinyl silicone oil, viscosity 150cps, 85wt%;
[0127] Relative to 100 parts of component A, second solvent: toluene, 200 parts.
[0128] 2. Preparation method of silicone gel:
[0129] (1) Preparation of color paste masterbatch:
[0130] Add the second vinyl silicone oil, high-pigment carbon black and dispersing aid in the above-mentioned mass ratio into a container, pre-disperse for 50 minutes to obtain a pre-dispersed liquid; add the pre-dispersed liquid into a grinding device, grind for 4 to 5 hours, ensure that the fineness is less than 15 μm (the average particle size of the high-pigment carbon black is less than 15 μm), stop dispersing, and obtain a color paste masterbatch.
[0131] (2) Preparation of modified multi-walled carbon nanotube slurry:
[0132] Toluene, third vinyl silicone oil and carboxylated multi-walled carbon nanotubes were added to the reaction kettle in sequence, and the temperature was raised to reflux under mechanical stirring; a silane coupling agent was added dropwise and the reaction was carried out for 6 hours; vacuum degassing was performed and the temperature was lowered; the above slurry was added to a dispersing device for further grinding and dispersion to obtain a modified multi-walled carbon nanotube slurry.
[0133] (3) Preparation of silicone gel
[0134] Add color paste masterbatch, modified multi-walled carbon nanotube slurry, vinyl polysiloxane and half of the toluene in a planetary agitator in turn, disperse at high speed for 3 hours, move to a stirring kettle after sufficient dispersion, then add the remaining toluene, ethyl acetate, the first vinyl silicone oil, methyl MQ resin, vinyl MQ resin and inhibitor in turn, stir mechanically for 60 minutes, add the cross-linking agent and catalyst in turn with an addition interval of 5 minutes, continue stirring for 45 minutes, filter through a filter element to obtain a silicone gel.
[0135] Example 2
[0136] This example is carried out with reference to Example 1, and its preparation method is the same as that of Example 1, but the composition of the silicone gel is different, as follows:
[0137] Color paste masterbatch: 3 parts;
[0138] Modified multi-walled carbon nanotube slurry: 3 parts;
[0139] First vinyl silicone oil: 3 parts, viscosity 500cps, vinyl content 0.06%;
[0140] Vinyl polysiloxane: 35 parts, viscosity average molecular weight is 600,000, vinyl content is 0.08 mol%;
[0141] Methyl MQ resin, 50 parts, M:Q ratio 0.75:1;
[0142] Vinyl MQ resin, 1.5 parts, M:Q ratio 0.75:1, vinyl content 1.2%;
[0143] SYL-OFF TM SL 7028, 1.37 parts;
[0144] Methylbutynol, 0.27 parts;
[0145] SYL-OFF TM 4000Catalyst, 1.65 copies;
[0146] Toluene, 85 parts; ethyl acetate, 85 parts.
[0147] The composition of color paste masterbatch is as follows:
[0148] MONARCH 1300, 8.5wt%,
[0149] Second vinyl silicone oil: viscosity 1,000cps, 91.0wt%,
[0150] BYK-2096, 0.5 wt%;
[0151] The modified multi-walled carbon nanotube slurry is composed of the following:
[0152] Component A: carboxylated multi-walled carbon nanotubes: average length 5 μm, 5 wt%,
[0153] KH-570, 0.5wt%,
[0154] Third vinyl silicone oil: viscosity 1,000cps, 94.5wt%,
[0155] Relative to 100 parts of component A, toluene, 200 parts.
[0156] Example 3
[0157] This example is carried out with reference to Example 1, and its preparation method is the same as that of Example 1, but the composition of the silicone gel is different, as follows:
[0158] Color paste masterbatch, 20 parts;
[0159] Modified multi-walled carbon nanotube slurry, 20 parts;
[0160] First vinyl silicone oil, 20 parts, viscosity 20,000 cps, vinyl content 0.12%;
[0161] Vinyl polysiloxane, 50 parts, viscosity average molecular weight 750,000, vinyl content 0.2 mol%;
[0162] Methyl MQ resin, 100 parts, M:Q ratio 0.75:1;
[0163] Vinyl MQ resin, 20 parts, M:Q ratio 0.75:1, vinyl content 0.5%;
[0164] SYL-OFF TM SL 7028, 3.6 parts;
[0165] Methylbutynol, 0.68 parts;
[0166] SYL-OFF TM 4000Catalyst, 4.2 copies;
[0167] Toluene, 220 parts; ethyl acetate, 220 parts.
[0168] The composition of color paste masterbatch is as follows:
[0169] MONARCH 1300, 30wt%,
[0170] Second vinyl silicone oil, viscosity 80cps, 67wt%,
[0171] BYK-2096, 3 wt%;
[0172] The modified multi-walled carbon nanotube slurry is composed of the following:
[0173] Component A: carboxylated multi-walled carbon nanotubes, average length 30 μm, 16 wt%,
[0174] KH-570, 5wt%,
[0175] The third vinyl silicone oil, viscosity 80cps, 79wt%,
[0176] Relative to 100 parts of component A, toluene, 200 parts.
[0177] Example 4
[0178] This example is carried out with reference to Example 2, wherein the silicone gel component only does not contain the first vinyl silicone oil and the vinyl MQ resin, and the other components, compositions and preparation methods are the same as those in Example 2.
[0179] Comparative Example 1
[0180] This group of comparative examples is made with reference to Example 1, and is used to illustrate the effect of the amount and performance of high-pigment carbon black on the performance of silicone gel. In this comparative example, only the amount and ratio of the color paste masterbatch are changed, and the content of the first solvent is adjusted to make the silicone gel coating concentration consistent. The other components, compositions and preparation methods are the same as those in Example 1, as shown below:
[0181] Comparative Example 1a: 23 parts of color paste masterbatch, 155 parts of toluene, 155 parts of ethyl acetate, the specific ratio in the color paste masterbatch is: 32wt% of MONARCH 1300, 66wt% of the second vinyl silicone oil (viscosity 80cps), 2wt% of BYK-2096;
[0182] Comparative Example 1b: This comparative example does not contain color paste masterbatch, 135 parts of toluene, and 135 parts of ethyl acetate;
[0183] Comparative Example 1c: In the color paste masterbatch in this comparative example, an equal amount of low-pigment carbon black (Cabot M120) is used to replace high-pigment carbon black.
[0184] Comparative Example 2
[0185] This group of comparative examples is carried out with reference to Example 1, and is used to illustrate the effect of the amount of modified multi-walled carbon nanotube slurry added on the performance of silicone gel. In this comparative example, only the amount of modified multi-walled carbon nanotube slurry added is changed, and in order to make the silicone gel coating concentration consistent, the content of the first solvent is adjusted. The other components, compositions and preparation methods are the same as those in Example 1, as shown below:
[0186] Comparative Example 2a: 23 parts of modified multi-walled carbon nanotube slurry, 155 parts of toluene, 155 parts of ethyl acetate, the average length of the carboxylated multi-walled carbon nanotubes in the slurry is 22 μm, the slurry contains 18wt% carboxylated multi-walled carbon nanotubes, 2wt% KH-570, 80wt% of the third vinyl silicone oil (viscosity 80cps), and the amount of toluene in the second solvent remains unchanged;
[0187] Comparative Example 2b: This comparative example does not contain modified multi-walled carbon nanotube slurry, 135 parts of toluene, and 135 parts of ethyl acetate.
[0188] Comparative Example 3
[0189] This comparative example is carried out with reference to Example 1, and the difference from Example 1 is that neither the color paste masterbatch nor the modified multi-walled carbon nanotube slurry is added to the silicone gel at the same time, and the other components, compositions and preparation methods are the same as those in Example 1.
[0190] Comparative Example 4
[0191] This comparative example is carried out with reference to Example 1. The difference from Example 1 is that no color paste masterbatch is added, and the effect on the performance of the silicone gel is evaluated only by increasing the colloid hardness. The preparation method is the same as that of Example 1. The composition of the silicone gel, by weight, includes the following raw material components:
[0192] Modified multi-walled carbon nanotube slurry: 13 parts;
[0193] The first vinyl silicone oil, 10 parts, has a viscosity of 10,000 cps and a vinyl content of 0.35%;
[0194] Vinyl polysiloxane, 30 parts, viscosity average molecular weight 600,000, vinyl content 0.24 mol%;
[0195] Methyl MQ resin, 70 parts, M:Q ratio 0.85:1;
[0196] Vinyl MQ resin, 12 parts, M:Q ratio 0.7:1, vinyl content 2.2%;
[0197] SYL-OFF TM SL 7028, 2.05 parts;
[0198] Methylbutynol, 0.41 parts;
[0199] SYL-OFF TM 4000Catalyst, 2.44 copies;
[0200] Toluene, 125 parts; Ethyl acetate, 125 parts;
[0201] The modified multi-walled carbon nanotube slurry is composed of the following:
[0202] Component A: carboxylated multi-walled carbon nanotubes, average length 25 μm, 15 wt%,
[0203] KH-570, 2wt%,
[0204] The third vinyl silicone oil, viscosity 120cps, 83wt%,
[0205] Relative to 100 parts of component A, toluene, 200 parts.
[0206] Comparative Example 5
[0207] Silicone release films with release forces of 1 to 3 gf / in and 3 to 5 gf / in were used as substrates, respectively. High-viscosity acrylic pressure-sensitive adhesive (AG42A from Jiangsu Crown New Material Technology Co., Ltd.) was coated with a micro-concave coating head. The adhesive films were cured in an oven at 100°C to prepare acrylic adhesive films. The above-mentioned adhesive films were respectively transferred to both sides of the TPU elastomer. After the product was matured, a TPU buffer tape with a total thickness of 150 μm was obtained.
[0208] Test Case
[0209] The silicone gel prepared in the above embodiments and comparative examples is coated on the release surface of the first fluorine release film by a doctor blade or slot die coating head, cured in an oven at a high temperature of 160°C, composited with the second fluorine release film, and rolled up to obtain a finished product. The finished products obtained in each embodiment and comparative example are sampled and tested for the following performances, and the test results are recorded in Table 2.
[0210] (1) 180° peel force test
[0211] The test was conducted in accordance with GB / T 2792-2014 "Test method for peel strength of adhesive tapes". The sample strip was cut to a width of 25 mm. The release film on the composite film surface was torn off and a 50 μm PET original film was applied for reinforcement. The other side was attached to a SUS standard test plate to test the 180° peel strength of the tape.
[0212] (2) Tensile strength
[0213] The sample was made into a 1 mm thick strip, clamped on a universal tensile testing machine, and subjected to a tensile test at a speed of 100 mm / min until it broke, and the strength value corresponding to the maximum force before breaking was recorded.
[0214] (3) Indentation test
[0215] Stick the sample between the copper foil and the PMMA sheet with the copper foil facing upwards. Use a steel probe to press the sample and hold it for 30 seconds. After taking it out, observe the deformation from the PMMA surface. If there is residual deformation, it is unqualified. Adjust the pressing pressure up and down until no indentation appears. Record the corresponding pressure. Among them, pressure <2.5MPa is poor, 2.5-3.5MPa is qualified, and >3.5MPa is excellent.
[0216] (4) Buffer height
[0217] Stick the product between the display module and the copper foil and aluminum foil, then place the display module on a steel impact table with the copper foil facing up and keeping it level. Take a steel ball and hit the display module vertically from different heights. Test 30 points in parallel and record the height at which no bad pixels appear on the display module. The height must be ≥40mm.
[0218] (5) Volume resistivity
[0219] The test method refers to ANSI / ESD STM 11.11-2021 "Measurement of Surface Resistance of Planar Materials". The larger the volume resistivity value, the better the insulation performance of the material, and vice versa. The volume resistivity value exceeds 1.0×10 13 Ω·m means that the material has no conductive properties.
[0220] (6) Brightness
[0221] Take a film sample, tear off the release films on both sides, use a colorimeter to test directly, and record the brightness (L value). Generally, the larger the L value, the lighter the color; conversely, the darker the color.
[0222] (7) Light transmittance
[0223] Take a film sample, tear off the release films on both sides, use a transmittance tester to directly test it, and record the transmittance. The transmittance reflects the light transmittance of the material. The greater the transmittance, the better the light transmittance.
[0224] (8) Appearance
[0225] Take samples to visually inspect the number of surface point defects, appearance and glue overflow at the incision, and grade them according to the levels in Table 1 below, and record the grading results.
[0226] Table 1
[0227]
[0228]
[0229] *Indicates the test area is 1m 2 .
[0230] Table 2
[0231]
[0232] From the comparative examples and test results of the embodiments in Table 2, it can be seen that the silicone gel provided by the present invention has the best comprehensive performance. Compared with the interlayer TPU and hardened silicone gel solutions, the present invention adds a certain amount of high-pigment carbon black and MWCNTS for compounding and synergizing, and the indentation resistance is close to that of the TPU elastomer solution, and the buffer height is significantly improved, and the product has low light transmittance.
[0233] It can be found from Example 1, Comparative Example 1 and Comparative Example 2 that high-pigment carbon black can significantly reduce the L value and light transmittance, reduce the intensity of reflected light, improve the ability to resist indentation, and assist in improving the buffering performance. Only by adding a suitable proportion of pigment carbon black and modified MWCNTS can the material's anti-indentation and buffering performance be significantly improved. Adding too much pigment carbon black and modified MWCNTS will lead to increased agglomeration, limited improvement, and even negative effects such as decreased buffering and deterioration of appearance. Without pigment carbon black and modified MWCNTS, silicone gel cannot effectively absorb light and improve impact resistance, and it is difficult to achieve the desired effect. In addition, under the same addition ratio, high-pigment carbon black has a stronger light absorption ability, and the effect of improving anti-indentation is significantly better than that of low-pigment carbon black. Modified MWCNTS can significantly improve buffering performance through bridging, and at the same time, the performance against indentation is also improved. In addition, the combination of high-pigment carbon black and modified MWCNTS not only has a mutual gain effect on indentation and buffering, but also can significantly improve conductivity. This may be because MWCNTS and carbon black build a conductive framework structure, thereby opening up a conductive path.
[0234] It should be noted that, in this article, the terms "comprise", "include" or any other variant thereof are intended to cover non-exclusive inclusion, so that the process, method, article or device including a series of elements includes not only those elements, but also includes other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the sentence "comprise one..." do not exclude the presence of other identical elements in the process, method, article or device including the element. In addition, it should be pointed out that the scope of the methods and devices in the embodiments of the present application is not limited to performing functions in the order shown or discussed, and may also include performing functions in a substantially simultaneous manner or in reverse order according to the functions involved, for example, the described method may be performed in an order different from that described, and various steps may also be added, omitted, or combined. In addition, the features described with reference to certain examples may be combined in other examples.
[0235] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A silicone gel composition, characterized in that: The silicone gel composition comprises the following components in parts by weight: Color paste masterbatch: 1-20 parts; Based on the total weight of the color paste masterbatch being 100wt%, the color paste masterbatch comprises: 5-30wt% of high-color carbon black, 67-94.5wt% of the second vinyl silicone oil and 0.5-3wt% of a dispersing aid; Modified multi-walled carbon nanotube slurry: 1-20 parts; the modified multi-walled carbon nanotube slurry comprises: component A and a second solvent, with the content of the second solvent being 100-300 parts relative to 100 parts of component A; based on the total weight of component A being 100wt%, component A comprises: 3-16wt% of carboxylated multi-walled carbon nanotubes, 0.5-5wt% of a silane coupling agent, and 79-96.5wt% of a third vinyl silicone oil; First vinyl silicone oil: 0-20 parts; Olefin polysiloxane: 15-60 parts; Methyl MQ resin: 50-100 parts; Vinyl MQ resin: 0-20 parts; Cross-linking agent: 1-5 parts; Inhibitor: 0.1-2 parts; Catalyst: 1-5 parts; First solvent: 100-500 parts.
2. The composition according to claim 1, characterized in that The viscosity of the second vinyl silicone oil is 50-1,000 cps.
3. The composition according to claim 1, characterized in that The viscosity of the third vinyl silicone oil is 50-1,000 cps.
4. The composition according to claim 1, characterized in that The average particle size of the high-pigment carbon black in the color paste masterbatch is less than 15 μm; And / or, the average length of the carboxylated multi-walled carbon nanotubes is 3 μm-30 μm.
5. The composition according to claim 1, characterized in that The viscosity of the first vinyl silicone oil is 500-20,000 cps, and the vinyl content of the first vinyl silicone oil is 0.06-0.5%; And / or, the viscosity average molecular weight of the olefin-based polysiloxane is 600,000-750,000, and the olefin content in the olefin-based polysiloxane is 0.03-0.30 mol%.
6. The composition according to claim 1, characterized in that In the methyl MQ resin, the M:Q ratio is (0.6-0.9):1, and the hydroxyl content is <1.0%; And / or, in the vinyl MQ resin, the M:Q ratio is (0.6-0.9):1, and the vinyl content is 0.5-3.0%.
7. The composition according to any one of claims 1 to 6, characterized in that The cross-linking agent is hydrogen-containing silicone oil; and / or, the inhibitor is selected from alkynol compounds; And / or, the catalyst is selected from transition metal complexes.
8. The composition according to claim 7, characterized in that The hydrogen content of the hydrogen-containing silicone oil is 0.8-1.6%.
9. A silicone gel, characterized in that: Composed of the composition according to any one of claims 1 to 8.
10. A display module adhesive film, characterized in that: The display module adhesive film contains the silicone gel composition according to any one of claims 1 to 8, or the silicone gel according to claim 9.
11. An electronic product, characterized in that: The electronic product contains the silicone gel composition according to any one of claims 1 to 8, or the silicone gel according to claim 9.
Citation Information
Patent Citations
Conductive silicone rubber with high elastic resilience and preparation method thereof
CN103937258A
Double-component pouring silica gel, method for preparing same and pouring method
CN105623593A
Cited By