A high thermal conductivity plastic mold steel and its manufacturing method

By optimizing the chemical composition and manufacturing process, a high thermal conductivity plastic mold steel has been developed, which solves the problems of insufficient thermal conductivity and hardenability of existing mold steels, and achieves a highly efficient injection molding cycle, suitable for large molds.

CN117778874BActive Publication Date: 2026-11-17宝武特种冶金有限公司
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202211151995.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-09-21
Publication Date
2026-11-17
Estimated Expiration
2042-09-21

AI Technical Summary

Technical Problem

The thermal conductivity and hardenability of existing plastic mold steels are insufficient, resulting in a long injection molding cycle and making it difficult to meet the needs of high-efficiency production.

Method used

By optimizing the chemical composition and manufacturing process, a high thermal conductivity plastic mold steel is designed, containing specific proportions of elements such as C, Mo, Si, Mn, Cr, Ni, Ti, and B. Combined with special forging, annealing, and tempering treatments, it ensures high thermal conductivity and hardenability.

Benefits of technology

It achieves thermal conductivity of 43.1–44.6 (W/m·K) at 25℃, thermal conductivity of 43.4–45.3 (W/m·K) at 100℃, and room temperature hardness of 31–35 HRC, shortening the injection molding solidification time and improving the production efficiency of injection molded parts.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0003856804210000071
    Figure BDA0003856804210000071
  • Figure BDA0003856804210000081
    Figure BDA0003856804210000081
  • Figure BDA0003856804210000091
    Figure BDA0003856804210000091
Patent Text Reader

Abstract

A high thermal conductivity plastic mold steel and its manufacturing method are disclosed. The plastic mold steel has the following composition by weight percentage: C 0.20-0.40%, Mo 1.20-3.00%, Si≤0.04%, Mn≤0.04%, Cr0.50-1.50%, Ni 0.90-1.50%, Ti 0.025-0.080%, B The content of the alloy is 0.002-0.005%, with the balance including Fe and unavoidable impurities. The percentage content of Ni and Mo is limited to %Ni = 0.5 + (%Mo ÷ 3), and the percentage content of C, Cr, and Ti is limited to %C = (%Cr ÷ 4) + %Ti. The steel is produced by electric arc furnace + refining furnace + vacuum degassing furnace. The cast steel ingots are forged into flat rectangular modules on a high-speed forging machine. After annealing, the modules undergo two-phase quenching and two tempering treatments. The highest thermal conductivity from room temperature to 100℃ reaches 45.3 (W / mK), and the heat treatment hardness reaches 31-35HRC. This achieves a balance between thermal conductivity and hardenability, realizing the goal of high thermal conductivity in large plastic mold steel.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of mold steel, and more particularly to a high thermal conductivity plastic mold steel and its manufacturing method. Background Technology

[0002] Molds, as tools used for forming metal, plastic, and rubber products, have been widely used in the industrial manufacturing field. Among them, injection molding of plastic products is the forming process mode adopted for irregularly shaped plastic products. Injection molding is a process in which granular or powdered plastic is fed from the hopper of an injection molding machine into a barrel equipped with a heating device for heating, melting and plasticizing, making it a viscous melt. Then, under the high pressure of the injection molding machine plunger, it is injected into a closed cavity at a high flow rate through the nozzle at the front end of the barrel. After a period of pressure holding, cooling and shaping, the mold is opened and the plastic part with a certain shape and size can be ejected from the cavity, thus completing a molding cycle.

[0003] The length of the injection molding cycle time for plastic parts determines the efficiency of the process. Factors influencing the cycle time include the temperature of the molten plastic, the water cooling strength of the mold, and the thermal conductivity of the mold. The thermal conductivity of the mold is related to the mold material. Currently, injection molding molds commonly use pre-hardened plastic mold steels such as 2738, 718, and P20, and quenched plastic mold steels such as 1.2343. These plastic mold steels have low thermal conductivity, with a thermal conductivity of 24–32 (W / m·K) from room temperature to 200℃ in the tempered state. Such thermal conductivity limits further reduction of the injection molding cycle time for plastic parts. Therefore, to shorten the injection molding cycle time for plastic parts, mold materials with high thermal conductivity must be selected.

[0004] The thermal conductivity of metallic crystals is due to the collisions between free electrons and metal cations within the crystal. Another metal atom loses its outermost electron and collides with a third metal cation, becoming a neutral atom. If the right end is heated, the neutral atom on the right loses electrons and transfers energy to the metal cations on the left. The metal atoms on the left lose electrons when heated and transfer energy back to the left, thus conducting heat from right to left. The mold material is alloy steel, which is iron-based with added carbon and alloying elements such as C, Si, Mn, Cr, Ni, Mo, V, W, and Nb. The addition of carbon and some alloying elements reduces the number of free electrons, lowering thermal conductivity. Although adding alloying elements reduces thermal conductivity, it increases hardness to meet the high hardness requirements of molds. Therefore, traditional alloy plastic mold steels generally have low thermal conductivity. The thermal conductivity of pre-hardened plastic mold steel grade 2738 in its tempered state from room temperature to 200℃ is 29–30 (W / m·K).

[0005] Existing high thermal conductivity mold steels have a quenched and tempered thermal conductivity of 32–44.2 (W / m·K), which is higher than that of traditional alloy-type plastic mold steels.

[0006] Chinese Patent Publication No. CN102605261A discloses a chemical composition of: C 0.43-0.48%, Si 0.3-0.5%, Mn 0.5-0.8%, Cr 2.3-2.7%, Mo 1.9-2.4%, V 0.7-1.0%, P≤0.03%, S≤0.03%, with the remainder being Fe and unavoidable impurities. The thermal conductivity in the quenched and tempered state is 32 (W / m·K), which is 29.5% higher than that of hot work die steel H13 (24.7 W / m·K at room temperature). However, its thermal conductivity is only slightly improved compared to pre-hardened plastic mold steel of type 2738. Furthermore, the alloy element content is higher than that of 2738, increasing the manufacturing cost of the die steel and reducing its cost-effectiveness.

[0007] Chinese Patent Publication No. CN103334052A discloses a chemical composition of: C 0.45-0.5%, Si < 0.2%, Mn < 0.2%, W 1.0-2.0%, Mo 2.0-3.5%, Cr < 0.3%, with the remainder being Fe and unavoidable impurities. This steel, in its quenched and tempered state, has a thermal conductivity of 44.2 (W / m·K) at 200℃, significantly higher than that of hot work die steel H13 and plastic mold steel 2738. However, its chemical composition contains very low levels of hardenability elements Cr and Mn, resulting in insufficient hardenability. In large molds, ferrite phases easily precipitate during quenching and cooling, reducing the hardness. A drawback of this invention is its unsuitability for heat treatment of large molds.

[0008] Chinese Patent Publication No. CN103334061A discloses a chemical composition of C 0.30–0.45%, Mn 0.20–0.30%, Si 0.10–0.30%, Cr 2.00–3.50%, Ni 2.00–6.00%, W 2.50–4.00%, Mo 1.00–1.50%, V 0.35–0.65%, S≤0.025%, P≤0.025%, with the remainder being Fe. Although this steel composition includes elements such as Cr, Ni, and Mo to improve hardenability, making it suitable for heat treatment of large-section molds, its thermal conductivity is low, with a thermal conductivity of only 35.5 (W / m·K) at 100℃. This thermal conductivity is improved compared to H13 steel, but only slightly improved compared to plastic mold steel 2738. Therefore, it offers no advantage in thermal conductivity. The advantage of this invention is its high hardenability, making it suitable for heat treatment of large-section molds. Its disadvantage is its low thermal conductivity, which offers no advantage compared to plastic mold steel 2738. Summary of the Invention

[0009] The purpose of this invention is to provide a high thermal conductivity plastic mold steel and its manufacturing method, overcoming the shortcomings of low thermal conductivity and low hardenability of existing plastic mold steels. The high thermal conductivity plastic mold steel has a thermal conductivity of 43.1-44.6 (W / m·K) at 25℃, a thermal conductivity of 43.4-45.3 (W / m·K) at 100℃, and a room temperature hardness of 31-35 HRC, thereby shortening the solidification time of plastic mold injection and improving the production efficiency of injection molded parts.

[0010] To achieve the above objectives, the technical solution of the present invention is as follows:

[0011] A high thermal conductivity plastic mold steel has the following chemical composition by weight percentage: C 0.20-0.40%, Mo 1.20-3.00%, Si≤0.04%, Mn≤0.04%, Cr 0.50-1.50%, Ni 0.90-1.50%, Ti 0.025-0.080%, B 0.002-0.005%, with the balance including Fe and other unavoidable impurities, and simultaneously satisfying: %Ni = 0.5 + (%Mo ÷ 3), %C = (%Cr ÷ 4) + %Ti.

[0012] Furthermore, the remainder consists of Fe and other unavoidable impurities.

[0013] The high thermal conductivity plastic mold steel described in this invention has a thermal conductivity of 43.1–44.6 (W / m·K) at 25℃, a thermal conductivity of 43.4–45.3 (W / m·K) at 100℃, and a room temperature hardness of 31–35 HRC.

[0014] In the composition design of the high thermal conductivity plastic mold steel described in this invention:

[0015] Adding 0.20–0.40% C to the Fe matrix improves hardness and hardenability; adding 1.20–3.00% Mo improves thermal conductivity and hardenability, as adding Mo increases the number of free electrons, reducing the decrease in thermal conductivity caused by the addition of carbon and alloying elements to the Fe matrix. Si has a significantly different atomic structure from Fe, reducing thermal conductivity; therefore, the Si content in the steel is controlled to be as low as possible. Mn dissolves into the matrix, causing lattice distortion and reducing thermal conductivity; therefore, the Mn content in the steel is controlled to be as low as possible. Since Si and Mn are added for deoxidation during steelmaking, the steel contains small amounts of Si and Mn. This invention controls the Si and Mn content to ≤0.04% to minimize their impact on thermal conductivity.

[0016] The purpose of adding Cr is to improve hardenability, but excessive Cr content reduces the thermal conductivity of the steel; therefore, 0.50–1.50% Cr is added. Similarly, the purpose of adding Ni is to improve hardenability, but excessive Ni content increases the retained austenite content and reduces hardness; therefore, 0.90–1.50% Ni is added. The purpose of adding B is to improve hardenability, but adding B requires first adding Ti to fix nitrogen, ensuring that the added B effectively improves hardenability; therefore, 0.025–0.080% Ti and 0.002–0.005% B are added. Therefore, the mold steel with the above chemical composition possesses high thermal conductivity, high hardenability, and is suitable for quenching and tempering treatment of large plastic molds.

[0017] The above chemical composition also specifically requires that %Ni = 0.5 + (%Mo ÷ 3). Mo is an alloying element that narrows the temperature range of the austenite phase. Increasing the Mo content means that the temperature range of the austenite phase becomes narrower, which leads to a narrower forging deformation temperature range, an increased quenching temperature, and reduced toughness. Therefore, Ni, an alloying element that expands the temperature range of the austenite phase, is added. The amount of Ni added is related to the amount of Mo added. The addition of Ni and Mo follows %Ni = 0.5 + (%Mo ÷ 3), which can ensure that the lower limit of the single austenite phase temperature range is 900-920℃, the quenching temperature of the two-phase region does not exceed 900℃, and maintain the high toughness of the material.

[0018] It also requires that %C = (%Cr ÷ 4) + %Ti. Cr is a carbide-forming element. Cr exists in steel as carbides, which reduces hardenability. Therefore, to improve hardenability, more Cr needs to exist in the steel in solid solution form during quenching. 23 C6 type carbides have low dissolution temperatures and are easily dissolved during quenching heating, thus allowing Cr to enhance hardenability. Ti is a strong carbide-forming element, forming TiC before Cr, reducing the C content in carbides participating in Cr formation and promoting Cr... 23 The formation of C6 type carbides follows the principle of %C = (%Cr ÷ 4) + %Ti, with the carbides formed being predominantly Cr. 23 Predominantly C6 type carbides, with more Cr added during quenching heating. 23 C6-type carbides dissolve into austenite, increasing the Cr content in austenite and improving hardenability.

[0019] Existing pre-hardened plastic mold steels all contain Si and Mn alloying elements that reduce thermal conductivity, while the content of Mo alloying element that improves thermal conductivity is not high. For example, pre-hardened plastic mold steel with steel grade 2738 contains 1.5% Mn and 0.3% Si, while Mo alloying element is only added at 0.3%. Pre-hardened plastic mold steel with steel grade P20 contains 1.5% Mn and 0.3% Si, while Mo alloying element is only added at 0.2%.

[0020] Compared with existing pre-hardened plastic mold steels, the high thermal conductivity plastic mold steel of this invention has a significantly different composition design. The content of Si and Mn elements is extremely low, both ≤0.04%, while the amount of Mo element added is increased. The decrease in hardenability caused by the reduction of Mn element content is compensated by adding Cr, Ni, and B elements. This allows the high thermal conductivity plastic mold steel of this invention to maintain high hardenability while significantly improving thermal conductivity, thus meeting the hardness requirements of plastic mold steel for large-size modules.

[0021] The manufacturing method of the high thermal conductivity plastic mold steel of the present invention includes the following steps:

[0022] 1) Smelting and casting

[0023] The steel ingots are smelted and cast according to the above composition, and then demolded after cooling in the mold for 14 to 16 hours.

[0024] 2) Forging

[0025] The steel ingot is transferred to the heating furnace of the forging production line for heating at a temperature of 1230-1250℃. After holding at this temperature for 12-18 hours, it is taken out of the furnace for forging. The heated steel ingot is then subjected to six-sided upsetting and drawing deformation 2-3 times using a high-speed forging machine to achieve the finished product size.

[0026] 3) Annealing

[0027] The forged rectangular module is placed into an annealing furnace for annealing. The annealing temperature is 580-620℃, and the module is held at that temperature for 35-50 hours before being removed from the furnace and air-cooled to room temperature.

[0028] 4) Conditioning and tempering

[0029] Quenching treatment: the quenching heating temperature is 830-900℃, and the holding temperature is 12-18 hours. After taking it out of the furnace, oil cooling is used for quenching and cooling is stopped when the module cooling temperature is 25-50℃.

[0030] Tempering treatment: First tempering temperature 520-550℃, holding for 30-40 hours; Second tempering temperature 520-550℃, holding for 18-28 hours.

[0031] Preferably, step 1) uses an EAF electric arc furnace + LF refining furnace + VD vacuum furnace for smelting.

[0032] Preferably, in step 2), a 60MN fast forging machine is used to perform six-sided upsetting and drawing deformation on the heated steel ingot 2 to 3 times to the finished size, and the finished size range is (750~980)×(1200~1350)×(3250~4000)mm.

[0033] Preferably, in step 1), the ingot casting temperature is 1545~1562℃.

[0034] The difference between the preparation method described in this invention and the prior art lies in:

[0035] 1) The present invention extends the mold cooling time of the steel ingot to 14-16 hours after casting, so that the steel ingot undergoes a solid pearlite phase transformation during the solidification process, which refines the solidification structure and prevents the grains of the steel ingot from becoming excessively coarse during forging heating. In contrast, the existing technology requires a mold cooling time of 9-10 hours for the steel ingot, which does not result in a pearlite transformation and produces a coarse solidification structure.

[0036] 2) The forging process of this invention adopts a six-sided upsetting + drawing deformation method to improve the uniformity of the properties of the forged product module in all directions and improve the toughness ratio; the existing technology only performs two-sided upsetting, resulting in a small toughness ratio and obvious toughness anisotropy.

[0037] 3) In this invention, the module is annealed at 580-620℃ after forging, which causes a pearlitic phase transformation, thus achieving both grain refinement and stress relief. In contrast, the existing technology uses annealing at 840-860℃, which does not significantly refine the grains.

[0038] 4) The tempering treatment used in this invention differs from conventional tempering treatment. Conventional tempering treatment uses a single austenite region temperature for quenching, while the tempering treatment in this invention uses a two-phase region temperature of 830-880℃ for quenching. This retains some undissolved carbides, reduces the content of C, Cr, and Mo dissolved in austenite, and lowers the content of residual austenite after quenching. After quenching, tempering treatment is performed. Conventional tempering treatment is performed only once, while the tempering treatment in this invention is performed twice. The purpose of the two tempering treatments is to reduce the content of residual austenite. After two tempering treatments, the content of residual austenite is reduced to 0.5%.

[0039] 5) This invention adds alloying elements Cr, Ni, Mo, and B to improve hardenability. The hardenability is higher than that of existing pre-hardened plastic mold steels 2738, 718, and P20. The hardenability of the material is characterized by the pearlite transformation incubation time in the continuous cooling microstructure transformation curve (CCT curve). The pearlite transformation incubation time of the mold steel within the composition range of this invention is 7365-8213 seconds, and the pearlite transformation incubation time of 2738, 718, and P20 is 300-5685 seconds.

[0040] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0041] The thermal conductivity of the mold steel described in this invention, after quenching and tempering, reaches 43.1–45.3 (W / m·K), which is far higher than the thermal conductivity of existing plastic mold steel (24–32 (W / m·K)). It also has high hardenability, making it suitable for quenching and tempering large molds. It can achieve a hardness of 33 HRC for large-sized modules ((750–980) × (1200–1350) × (3250–4000) mm) after quenching and tempering, meeting the hardness requirements for plastic mold steel. This invention achieves a balance between thermal conductivity and hardenability, realizing the goal of high thermal conductivity in large plastic mold steel.

[0042] The high thermal conductivity mold steel of this invention reduces the injection solidification time of automotive interior and exterior trim molds by 2 to 8 seconds compared to existing mold steels, thereby improving the production efficiency of injection molded parts. Detailed Implementation

[0043] The present invention will be further described below with reference to the embodiments.

[0044] The composition of the steel in the embodiments of the present invention is shown in Table 1, with the remainder including Fe and other unavoidable impurities; Table 2 shows the manufacturing method of the steel in the embodiments of the present invention, and Table 3 shows the performance parameters of the steel in the embodiments of the present invention.

[0045] The manufacturing process of the example is as follows: steelmaking uses a 40-ton EAF electric arc furnace + 40-ton LF furnace + 40-ton VD furnace to smelt and cast into 40-ton steel ingots → the steel ingots are forged and deformed to the finished size on a 60MN fast forging machine → annealing treatment → quenching and tempering treatment.

[0046] As can be seen from Table 3,

[0047]

[0048]

[0049]

Claims

1. A high thermal conductivity plastic mold steel, the chemical composition by weight percentage being: C 0.20~0.40%, Mo 1.20~3.00%, Si≤0.04%, Mn≤0.04%, Cr 0.50~1.50%, Ni 0.90~1.50%, Ti 0.025~0.080%, B 0.002~0.005%, the balance being Fe and other unavoidable impurities, and simultaneously satisfying: %Ni=0.5+(%Mo÷3), %C=(%Cr÷4)+%Ti; the high thermal conductivity plastic mold steel has a thermal conductivity of 43.1~44.6 (W / m·K) at 25℃, a thermal conductivity of 43.4~45.3 (W / m·K) at 100℃, and a room temperature hardness of 31~35HRC.

2. The high thermal conductive plastic mold steel according to claim 1, wherein, The remainder consists of Fe and other unavoidable impurities.

3. The method of manufacturing a high thermal conductive plastic mold steel according to claim 1 or 2, characterized in that, Includes the following steps: 1) Smelting and casting The steel ingot is smelted and cast into steel ingots according to the composition described in claim 1 or 2, and then demolded after cooling in the mold for 14 to 16 hours. 2) Forging The steel ingot is transferred to the heating furnace of the forging production line for heating at a temperature of 1230~1250℃. After holding at this temperature for 12~18 hours, it is taken out of the furnace for forging. The heated steel ingot is then subjected to six-sided upsetting and drawing deformation 2~3 times to the finished size using a high-speed forging machine. 3) Annealing The forged rectangular module is placed into an annealing furnace for annealing. The annealing temperature is 580~620℃, and the module is held at that temperature for 35~50 hours before being removed from the furnace and air-cooled to room temperature. 4) Conditioning and tempering Quenching treatment: the quenching heating temperature is 830~900℃, and the holding temperature is 12~18 hours. After taking it out of the furnace, oil cooling is used for quenching and cooling is stopped when the module cooling temperature is 25~50℃. Tempering treatment: First tempering temperature 520~550℃, holding for 30~40 hours; Second tempering temperature 520~550℃, holding for 18~28 hours.

4. The method of claim 3, wherein the high thermal conductive plastic mold steel is manufactured by the steps of: Step 1) The smelting process uses an EAF electric arc furnace + LF refining furnace + VD vacuum furnace. ​ 5. The method of claim 3, wherein the high thermal conductive plastic mold steel is manufactured by the steps of: preparing a molten steel by melting a predetermined amount of raw materials; pouring the molten steel into a mold; and solidifying the molten steel in the mold. In step 2), the heated steel ingot is subjected to six-sided upsetting and drawing deformation 2-3 times using a 60MN fast forging machine to the finished size, which is (750~980)×(1200~1350)×(3250~4000)mm.

6. The method of claim 3, wherein the high thermal conductive plastic mold steel is manufactured by the steps of: In step 1), the ingot casting temperature is 1545~1562℃. ​

Citation Information

Patent Citations

  • Hot stamping mould steel and method for manufacturing same

    CN102605261A

  • High-thermal conductivity high-abrasion resistance hot stamping die steel and preparation method thereof

    CN103334052A

  • Die-casting die steel with high heat conductivity and large section and preparation and heat treatment method thereof

    CN103334061A

  • Process for setting the thermal conductivity of a steel, tool steel, in particular hot-work steel, and steel object

    CN101512034A

  • Steel with ultra-high thermal conductivity for hot-stamping die and preparation method of steel

    CN102676923A