A solid electrolyte and a method for preparing the same

The flexible nano-BN/PVDF-HFP high ceramic content composite electrolyte prepared by high-energy ball milling and solution casting methods solves the safety hazards of traditional lithium-ion battery liquid electrolytes and the low conductivity problem of pure solid electrolytes, and achieves high ceramic content composite electrolytes. The high performance of the electrolyte extends battery life and improves safety.

CN117790888BActive Publication Date: 2024-10-22GUANGDONG UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410008299.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-04
Publication Date
2024-10-22
Estimated Expiration
2044-01-04

AI Technical Summary

Technical Problem

The liquid electrolyte of traditional lithium-ion batteries has poor thermal stability and is prone to leakage, leading to safety hazards. Pure inorganic or pure polymer solid electrolytes have problems such as large interface impedance, instability, and low ionic conductivity, which limits the application of all-solid-state batteries.

Method used

Amorphous BN nanosheets were prepared using a high-energy ball milling method, and a flexible nano-BN/PVDF-HFP high ceramic content composite electrolyte was designed through solution casting. Combined with two-dimensional BN nanosheets as a matrix, an electrolyte with high ionic conductivity and wide electrochemical window was prepared. , High ceramic content composite solid electrolyte with good thermal stability.

Benefits of technology

It significantly improves the room temperature ionic conductivity, thermal stability and lithium ion migration number of the composite solid electrolyte, extends the service life of the battery, improves the stability of the electrode interface, and reduces the risk of lithium dendrite puncture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117790888B_ABST
    Figure CN117790888B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of all-solid-state lithium batteries, and specifically relates to a solid electrolyte and a preparation method thereof. The present invention first adopts a high-energy ball milling strategy to effectively obtain a large number of high-quality amorphous two-dimensional BN ceramic nanosheets. Two-dimensional amorphous nanosheets have fast ion diffusion channels, larger volume expansion space, rich active sites and surface defects. Then, a flexible amorphous nano BN / PVDF-HFP high-ceramic content composite electrolyte is prepared by a solution casting method. The solid composite electrolyte prepared by the present invention can significantly improve the room temperature ionic conductivity, high thermal stability, high lithium ion migration number, wide electrochemical window and interface stability between the composite solid electrolyte and the electrode, thereby extending the service life of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of all-solid-state lithium batteries, and in particular relates to a solid electrolyte and a preparation method thereof. Background Art

[0002] The electrolyte used in traditional lithium-ion batteries is a liquid electrolyte, which has poor thermal stability, is prone to leakage, and can experience thermal runaway. In severe cases, an internal short circuit in the battery can cause an open flame and explosion. For this reason, the development of solid-state electrolytes is considered to be a fundamental strategy to solve the safety problems of liquid electrolytes. Solid-state electrolytes have the characteristics of high safety, high energy density, high power density, and a wide operating temperature range. Solid-state electrolytes mainly include inorganic solid-state electrolytes and polymer solid-state electrolytes. However, pure inorganic solid-state electrolytes and pure polymer solid-state electrolytes have problems such as large interface impedance, unstable interface, dendrite formation, and low ionic conductivity. In order to overcome these shortcomings, inorganic solid electrolytes are added as fillers to the polymer matrix to form a composite solid-state electrolyte. The ionic conductivity and Li + The ion migration number is higher than that of pure polymer, but it is still low, especially at high temperature, the polymer substrate softens and there is a risk of being pierced by lithium dendrites, which limits its application. The composite electrolyte with high ceramic content not only maintains the hardness of ceramics but also inherits the flexibility of polymers. It also has high lithium ion conductivity, lithium ion migration number, and is not easily pierced by lithium dendrites. Therefore, it is extremely necessary to develop a suitable strategy to prepare composite solid electrolytes with high ceramic content for practical all-solid-state batteries. Summary of the invention

[0003] In order to solve the problem that the room temperature ionic conductivity of composite solid electrolytes is not high, the present invention provides a new solid electrolyte and a preparation method thereof. The prepared solid electrolyte has the advantages of high ionic conductivity, wide electrochemical window, good thermal stability, strong flame retardancy, etc., and has broad application prospects.

[0004] In order to achieve the above object, the technical solution adopted by the present invention is:

[0005] A first aspect of the present invention provides a method for preparing a solid electrolyte, the method comprising the following steps:

[0006] S1. Preparation of amorphous BN nanosheets by high-energy ball milling: Put layered material h-BN and zirconium balls into a zirconium ball tank, heat at 90-110°C for 2-4 hours, evacuate to remove impurities, add alkali metal sheets, seal the zirconium ball tank, and place it in a ball mill for high-energy ball milling. Collect the milled powder, disperse it in water, and then filter and dry it.

[0007] S2. Preparation of amorphous BN nanosheets, flexible nano BN / PVDF-HFP (polyvinylidene fluoride-hexafluoropropylene copolymer) high ceramic content composite electrolyte by solution casting method: dissolve the amorphous BN nanopowder, LITFSI lithium salt and PVDF-HFP in N,N-dimethylformamide to prepare a nano BN / PVDF-HFP solution, heat and stir, and then dry to remove the residual solvent.

[0008] The present invention first prepares amorphous BN nanosheet powder by high-energy ball milling, and then uses two-dimensional BN nanosheets as a matrix to design a flexible nano BN / PVDF-HFP high-ceramic content composite electrolyte that can be easily prepared by a solution casting method. The present invention is simple to operate, has cheap and readily available raw materials, is non-toxic to the environment, and can prepare a high-ceramic content composite solid electrolyte film material with high ion conductivity, wide electrochemical window, good thermal stability, and strong flame retardancy, and is easy to promote on a large scale.

[0009] Preferably, the high-energy ball milling treatment time in S1 is 36-48 hours, and the ball milling pressure is 5-10 bar.

[0010] Preferably, the heating temperature in S1 is 90-110° C. and the heating time is 2-4 h.

[0011] Preferably, the mass ratio of the layered material h-BN and the zirconium balls in S1 is 1-3g:90-150g.

[0012] Preferably, in S1, 10-12 pieces of alkali metal are added to every 1g of layered material h-BN, and each piece of alkali metal is cut into 6-10 strips on average and then added into the zirconium spherical tank.

[0013] Preferably, the mass ratio of the amorphous BN nanopowder, LITFSI lithium salt and PVDF-HFP in S2 is 1:1:0.4-1.4.

[0014] Preferably, the temperature of the heating and stirring in S2 is 50-60°C and the time is 18-30h.

[0015] Preferably, the ball mill in S1 is a Pulverisette 5 planetary ball mill.

[0016] Preferably, the drying in S2 is firstly continuous drying in a vacuum oven at 55-70° C. for 18-30 hours, and then drying at room temperature for 2-4 hours in a transition chamber of a glove box filled with inert gas.

[0017] The second aspect of the present invention provides a solid electrolyte prepared by the preparation method described in the first aspect.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] The present invention provides a method for preparing a novel solid electrolyte. First, a high-energy ball milling strategy is adopted to effectively obtain a large number of high-quality amorphous two-dimensional BN ceramic nanosheets. The two-dimensional amorphous nanosheets have fast ion diffusion channels, larger volume expansion space, rich active sites and surface defects. Then, a flexible amorphous nano BN / PVDF-HFP high-ceramic content composite electrolyte is prepared by a solution casting method. The solid composite electrolyte prepared by the present invention can significantly improve the room temperature ionic conductivity, high thermal stability, high lithium ion migration number, wide electrochemical window and interface stability between the composite solid electrolyte and the electrode, thereby extending the service life of the battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 Optical photograph (a) and SEM photograph (b) of h-BN; optical photograph (c) and SEM photograph (d) of amorphous BN nanosheets; optical photograph (e) and SEM photograph (f) of h-BN / PVDF-HFP (40%); optical photograph (g) and SEM photograph (h) of CSE-40%.

[0021] Figure 2 XRD images of h-BN, amorphous BN nanosheet powder and CSE-40%.

[0022] Figure 3 EIS curves of CSE-40% and h-BN / PVDF-HFP (40%) (a); LSV curves of CSE-40% and h-BN / PVDF-HFP (40%) (b); Steady-state polarization curves and impedance of CSE-40% and h-BN / PVDF-HFP (40%) before and after polarization (c); 0.1 mA cm -2 Lithium deposition / stripping cycle test of Li / CSE-40% / Li and Li / h-BN / PVDF-HFP (40%) / Li symmetric cells (d). DETAILED DESCRIPTION

[0023] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.

[0024] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.

[0025] Example: A method for preparing a composite solid electrolyte with high ceramic content

[0026] The method comprises the following steps:

[0027] (1) Preparation of amorphous BN nanosheets by high-energy ball milling: Weigh 1g of layered material h-BN and 100g of zirconium balls into a zirconium ball jar, place it in an oven and heat and dry it at 100℃ for 2-4 hours, and then evacuate the small chamber of the glove box for 2-4 hours to remove impurities; then weigh 11 pieces of metal lithium, and cut each piece of alkali metal into 8 strips and pour them into the zirconium ball jar to mix with the layered material, apply vacuum silicone grease on the gap of the ball mill jar for sealing, and then put the ball mill jar into a Pulverisette 5 planetary ball mill for high-energy ball milling, and collect the ball milled powder after ball milling for 40 hours (ball milling pressure is about 6 bar). Finally, weigh 40mg of the ball milled powder into a beaker, and pour 200mL of 60℃ deionized water, mix it evenly with a magnetic stirrer to obtain a two-dimensional nanosheet material, and then collect the obtained two-dimensional nanosheet material by vacuum filtration, and dry it at 80℃ to obtain amorphous BN nanopowder.

[0028] (2) Preparation of amorphous BN nanosheets Flexible nano BN / PVDF-HFP (polyvinylidene fluoride-hexafluoropropylene copolymer) high ceramic content composite electrolyte by solution casting: 2.8 g of amorphous BN nanopowder (1 g), LITFSI lithium salt (1 g) and PVDF-HFP (0.8 g) were weighed in a mass ratio of 1:1:40%, and dissolved in 40 mL of N,N-dimethylformamide to prepare a nano BN / PVDF-HFP solution (CSE-40%). After magnetic stirring at 55°C for 24 hours, the obtained CSE-40% sample was placed in a vacuum oven at 60°C for continuous drying for 24 hours, and then dried at room temperature in a transition chamber of a glove box filled with Ar for 2-4 hours to remove the residual solvent, and a high ceramic content composite solid electrolyte (CSE-40%) was obtained.

[0029] Experimental example: Characterization and performance testing of composite solid electrolytes with high ceramic content

[0030] h-BN, amorphous BN nanosheet powder, h-BN / PVDF-HFP (40%) (solid electrolyte prepared from h-BN) and CSE-40% were optically photographed and characterized by SEM and XRD. At the same time, the composite solid electrolytes prepared above were tested for ionic conductivity, ion migration number and electrochemical window. Among them, the ionic conductivity of the composite solid electrolyte was tested by electrochemical impedance spectroscopy (EIS); the Li / composite solid electrolyte / Li symmetric battery was assembled, and the ion migration number was tested by steady-state current method. The electrochemical window test of the composite solid electrolyte was carried out by linear sweep voltammetry (LSV), and the test structure was Li / composite solid electrolyte / stainless steel sheet, the test potential range was 3.5-6V, and the scan rate was 0.01mV / s. The interface stability of CSE to Li metal was determined by constant current cycling of the symmetric battery Li / CSE-40% / Li, and the test current density was set to 0.1mAcm -2 (0.5 hours per plating / stripping).

[0031] Figure 1 (ab) are the optical and SEM images of h-BN, respectively. It can be clearly observed that h-BN is a lamellar structure. Figure 1 (cd) are optical photos and SEM photos of amorphous BN nanosheet powder, showing that the h-BN after ball milling is a nanosheet structure, proving that ball milling can produce nano boron nitride; Figure 1 (ef) are optical and SEM images of h-BN / PVDF-HFP (40%). Figure 1 (gh) are the optical and SEM photos of CSE-40%. It can be seen that the surface structure of the CSE-40% membrane is denser than that of h-BN / PVDF-HFP (40%), and the pores are relatively smaller and smoother.

[0032] Figure 2 The XRD images of h-BN, amorphous BN nanosheet powder and CSE-40% show that h-BN has obvious diffraction peaks at 26.7° and 55.2° (002) and (104) crystal planes, and 41.6° corresponds to the diffraction peak of (100) crystal plane. After milling with P5 zirconium balls, the diffraction peak of h-BN in amorphous nano-BN is not obvious at all, and the peak intensity of CSE-40% composite solid electrolyte is weaker than that of amorphous nano-BN, indicating that CSE-40% has low crystallinity and high ionic conductivity.

[0033] Figure 3 a is the EIS curve of CSE-40%, h-BN / PVDF-HFP (40%) solid electrolyte at room temperature. According to the ionic conductivity formula σ=L / R b *S(where R bThe bulk impedance is obtained by fitting the electrochemical impedance spectrum after testing the steel sheet symmetrical battery. L is the thickness of the solid electrolyte, and S is the area of ​​the solid electrolyte. It can be calculated that the ionic conductivity of CSE-40% and h-BN / PVDF-HFP (40%) are 1.936mS / cm and 0.429mS / cm respectively. From the resistance, it can be seen that the amorphous is smaller. Figure 3 b is the oxidation voltage windows of CSE-40% and h-BN / PVDF-HFP (40%) measured by linear sweep voltammetry (LSV) test, which are 4.8V and 4.7V respectively, indicating that amorphous BN nanosheets have better high temperature resistance than crystalline BN nanosheets. Therefore, this composite electrolyte can meet the practical application needs of lithium batteries, can be used in high-voltage batteries, and increase their energy density; Figure 3 Figure c is the lithium ion migration number measured by the steady-state current method. The ion migration numbers of CSE-40% and h-BN / PVDF-HFP (40%) are 0.47 and 0.4 respectively, proving that amorphous BN nanosheets have faster ion channels; Figure 4d is the lithium deposition / stripping cycle test of the Li-Li symmetric battery assembled by CSE-40% and h-BN / PVDF-HFP (40%). It can be seen that CSE-40% has better cycle stability than the Li-Li symmetric battery assembled by h-BN / PVDF-HFP (40%). The polarization voltage of CSE-40% does not exceed 0.03V (h-BN / PVDF-HFP polarization voltage is 0.047V), the cycle life exceeds 800h, the voltage distribution is stable, and there is no internal short circuit caused by Li dendrite formation during the cycle. The above results show that amorphous BN nanomaterials exhibit better properties than crystalline h-BN.

[0034] In summary, it can be seen that the flexible amorphous nano BN / PVDF-HFP high ceramic content composite electrolyte prepared by the high-energy ball milling method and the solution casting method in the present invention can significantly improve the room temperature ionic conductivity, high thermal stability, high lithium ion migration number, wide electrochemical window and interface stability between the composite solid electrolyte and the electrode, thereby extending the service life of the battery.

[0035] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.

Claims

1. A method for preparing a solid electrolyte, characterized in that: The following steps are involved: S1. Preparation of amorphous BN nanosheets by high-energy ball milling: Put layered material h-BN and zirconium balls into a zirconium ball tank, heat at 90-110°C for 2-4 hours, evacuate to remove impurities, add alkali metal sheets, seal the zirconium ball tank, and place it in a ball mill for high-energy ball milling. Collect the milled powder, disperse it in water, and then filter and dry it. S2. Preparation of amorphous BN nanosheets, flexible nano BN / PVDF-HFP (polyvinylidene fluoride-hexafluoropropylene copolymer) high ceramic content composite electrolyte by solution casting method: dissolving the amorphous BN nanopowder, LITFSI lithium salt and PVDF-HFP in N,N-dimethylformamide to prepare a nano BN / PVDF-HFP solution, heating and stirring, and then drying to remove the residual solvent; The high-energy ball milling treatment time in S1 is 36-48 hours, and the ball milling pressure is 5-10 bar; S1 The mass ratio of the layered material h-BN and the zirconium ball is 1-3g:90-150g; The mass ratio of the amorphous BN nanopowder, LITFSI lithium salt and PVDF-HFP in S2 is 1:1:0.4-1.

4.

2. The method for preparing a solid electrolyte according to claim 1, characterized in that: In S1, 10-12 pieces of alkali metal are added to every 1g of layered material h-BN, and each piece of alkali metal is cut into 6-10 strips on average and then added into the zirconium spherical tank.

3. The method for preparing a solid electrolyte according to claim 1, characterized in that: The temperature of the heating and stirring in S2 is 50-60°C and the time is 18-30h.

4. The method for preparing a solid electrolyte according to claim 1, characterized in that: The ball mill used in S1 was a Pulverisette 5 planetary ball mill.

5. The method for preparing a solid electrolyte according to claim 1, characterized in that: The drying in S2 is firstly carried out in a vacuum oven at 55-70°C for 18-30 hours, and then dried at room temperature for 2-4 hours in a transition chamber of a glove box filled with inert gas.

6. A solid electrolyte prepared by the preparation method according to any one of claims 1 to 5.