A method for preparing friction-resistant graphene film

By adding specific compounds to the polyphosphoric acid solution and performing hot-pressing film formation, combined with in-situ polymerization, the problem of graphene material agglomeration is solved, its wear resistance and mechanical properties are significantly improved, and graphite with excellent friction resistance and mechanical properties is formed. ene film.

CN117801335BActive Publication Date: 2024-10-22SHENZHEN KINGMAG PRECISION TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410001362.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-02
Publication Date
2024-10-22
Estimated Expiration
2044-01-02

AI Technical Summary

Technical Problem

Graphene materials are prone to agglomeration during the preparation process, resulting in limited performance. Existing technologies have failed to effectively improve its wear resistance and mechanical properties.

Method used

Carboxylated graphene, disilane benzoic acid and carboxylated boron nitride are added to the polyphosphoric acid solution, and a graphene composite copolymer solution is formed through a temperature-raising reaction, which is then hot-pressed to form a film on a stainless steel composite plate and combined in situ. Polymerization and organic modification form a graphene film with a three-dimensional network structure.

Benefits of technology

The friction resistance and mechanical properties of the graphene film are significantly improved, and the material's wear resistance and rigid support points are enhanced through the self-healing mechanism and dispersion effect.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present invention relates to the field of graphene technology, and discloses a method for preparing a friction-resistant graphene film. The present invention uses amino groups in amino graphene and 5-hydroxyisophthalic acid and formaldehyde to undergo Mannich reaction to obtain carboxylated graphene. The hydroxyl contained in 3,5-dihydroxybenzoic acid undergoes a substitution reaction with 3-iodopropyltriethoxysilane to obtain disilanebenzoic acid. Hexagonal boron nitride and 3,5-bis-aminomethyl-benzoic acid are alkalized, ball-milled, and neutralized to obtain carboxylated boron nitride. Carboxylated graphene, disilanebenzoic acid, carboxylated boron nitride, and 4,6-bis-aminohydroquinone are added to a polyphosphoric acid solution to obtain a graphene composite copolymer solution by in-situ polymerization, and finally the graphene composite copolymer solution is poured on a stainless steel composite plate, and hot-pressed into a film to obtain a friction-resistant graphene film. The film prepared by the present invention has excellent mechanical properties and wear resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of graphene, and in particular to a method for preparing a friction-resistant graphene film. Background Art

[0002] Graphene is a new type of special two-dimensional carbon material composed of a single layer of carbon atoms tightly bonded in a hexagonal structure. It has good electrical conductivity, thermal conductivity, mechanical properties, and thermal stability, and is widely used in energy, biomedicine, drug delivery, and other fields. However, there is a strong van der Waals force between graphene layers, which leads to the phenomenon of graphene agglomeration when preparing graphene nanocomposites, which seriously affects the performance of the material and limits the application of graphene materials.

[0003] High-performance polymers have the advantages of low density, high strength, flame retardancy and heat resistance, and are widely used in aerospace, electronic communications, weapons and armaments, etc. Among them, poly(p-phenylene benzoxazole) polymers have excellent mechanical properties and flame retardancy. Boron nitride has low dielectric constant, oxidation resistance, wear resistance, and excellent thermal conductivity, and is widely used in thermal conductivity, adsorption, corrosion protection and other fields.

[0004] For example, the patent with authorization announcement number CN111410190B discloses a graphene-boron nitride composite film with insulating and thermally conductive properties and a preparation method thereof. The invention mixes a GO aqueous dispersion with a hexagonal boron nitride aqueous dispersion, applies the film and dries it to obtain a film. The prepared graphene composite film has thermal conductivity and insulating properties, but does not improve wear resistance and mechanical properties. Summary of the invention

[0005] 1. Technical issues to be resolved

[0006] In view of the deficiencies in the prior art, the present invention provides a method for preparing a friction-resistant graphene film. The graphene film prepared by the present invention has excellent friction resistance and mechanical properties.

[0007] (II) Technical solution

[0008] A method for preparing a friction-resistant graphene film, the preparation method being as follows:

[0009] (1) Add carboxylated graphene, disilylbenzoic acid, and carboxylated boron nitride to a 80-90% polyphosphoric acid solution and stir to disperse, then add 4,6-diaminohydroquinone and heat to 120-140° C., stir to react for 10-24 hours, then heat to 160-180° C., and react for 15-30 hours to obtain a graphene composite copolymer solution.

[0010] (2) pouring the graphene composite copolymer solution onto a stainless steel composite plate, placing it in a hot press, hot pressing it into a film for 20-50 minutes, releasing the pressure after the hot pressing, soaking it in deionized water for 2-5 days, and drying it to obtain a friction-resistant graphene film.

[0011] Preferably, in step (1), the mass ratio of carboxylated graphene, disiloxanebenzoic acid, carboxylated boron nitride, and 4,6-diaminohydroquinone is 100:10-20:15-40:60-120.

[0012] Preferably, in step (2), the hot press pressure is 8-12 MPa and the temperature is 160-200°C.

[0013] Preferably, in the step (1), the preparation method of carboxylated graphene is: adding amino graphene, 5-hydroxyisophthalic acid and formaldehyde to a toluene solvent, stirring and dispersing, heating to 100-120° C., reacting for 4-10 hours, washing with deionized water, and drying to obtain carboxylated graphene.

[0014] Preferably, in the steps, the mass ratio of amination graphene, 5-hydroxyisophthalic acid and formaldehyde is 1:15-24:4.5-6.

[0015] Preferably, in the step (1), the preparation method of disiloxane benzoic acid is: adding 3,5-dihydroxybenzoic acid, 3-iodopropyltriethoxysilane and potassium carbonate to tetrahydrofuran solvent, heating to 70-80°C, reacting for 4-8h, and after the reaction is completed, cooling to room temperature, washing with saturated brine, drying, and concentrating by rotary evaporation to obtain disiloxane benzoic acid.

[0016] Preferably, in the step, the mass ratio of 3,5-dihydroxybenzoic acid, 3-iodopropyltriethoxysilane and potassium carbonate is 1:2-3.4:2.5-3.6.

[0017] Preferably, in the step (1), the preparation method of carboxylated boron nitride is: adding hexagonal boron nitride and 3,5-bis-aminomethyl-benzoic acid to a 1-2 mol / L sodium hydroxide solution, then adding zirconium oxide ball milling beads thereto, and ball milling for 5-15 hours. After the reaction is completed, the ball milling beads are sieved out, and then a 0.5-1.5 mol / L hydrochloric acid solution is added thereto, filtered, washed with deionized water, and dried to obtain carboxylated boron nitride.

[0018] Preferably, in the steps, the mass ratio of hexagonal boron nitride to 3,5-bis-aminomethyl-benzoic acid is 1:0.8-1.6.

[0019] (III) Beneficial technical effects

[0020] The present invention utilizes the amino group in the amino graphene to react with 5-hydroxyisophthalic acid and formaldehyde through a Mannich reaction to obtain carboxylated graphene. The hydroxyl group contained in 3,5-dihydroxybenzoic acid is subjected to a substitution reaction with 3-iodopropyltriethoxysilane to obtain disilanebenzoic acid. Hexagonal boron nitride and 3,5-bis-aminomethyl-benzoic acid are alkalized, ball-milled, and neutralized to obtain carboxylated boron nitride. Carboxylated graphene, disilanebenzoic acid, carboxylated boron nitride, and 4,6-di-aminohydroquinone are added to a polyphosphoric acid solution for in-situ polymerization to obtain a graphene composite copolymer solution, and finally the graphene composite copolymer solution is poured onto a stainless steel composite plate and hot-pressed into a film to obtain a friction-resistant graphene film.

[0021] The graphene layers used in the present invention are bonded to each other by van der Waals forces, and are easily plastically deformed by sliding along the crystal plane, thereby exhibiting good friction resistance. However, the graphene itself is very easy to agglomerate. Therefore, the present invention organically modifies the graphene, which has a good dispersing effect and improves the agglomeration phenomenon. Moreover, on this basis, in-situ polymerization is performed to further effectively solve the problem of easy agglomeration of the graphene and better exert its friction resistance.

[0022] The graphene film prepared by the present invention has a benzene ring and a ring structure, wherein the ring structure is obtained through a Mannich reaction. When subjected to external friction, the benzene ring and the five-membered ring can be twisted. After the friction ends, the benzene ring structure and the five-membered ring can self-repair to prevent the material from being damaged, thereby achieving better friction resistance and mechanical properties.

[0023] The graphene film prepared by the present invention has boron nitride. Boron nitride is the same as graphene. Since the surface of boron nitride has a large surface energy, it is very easy to agglomerate. The present invention can improve the dispersion effect and improve the friction resistance and mechanical properties of the material by organically modifying it.

[0024] The graphene film prepared by the present invention has a siloxane structure. The siloxane structure not only contains silicon-oxygen bonds with relatively large bond energy, but also self-crosslinks to form a network structure, which can improve the mechanical properties and friction resistance of the film.

[0025] The graphene film prepared by in-situ polymerization of the present invention has a three-dimensional network structure, and the graphene and boron nitride are uniformly dispersed in the film. When the film is subjected to external force, the graphene and boron nitride can serve as rigid support points and chemical and physical cross-linking points to bear the load, thereby improving the mechanical properties and wear resistance of the material. The film prepared by the present invention has excellent mechanical properties and wear resistance. DETAILED DESCRIPTION

[0026] The present invention is described in detail below through examples to facilitate understanding of the present invention by persons skilled in the art. It is necessary to point out that the examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Non-essential improvements and adjustments made to the present invention by persons skilled in the art based on the above-mentioned invention content should still fall within the scope of protection of the present invention. At the same time, the raw materials mentioned below that are not described in detail are all commercially available products, and the process steps or preparation methods that are not mentioned in detail are all process steps or preparation methods known to those skilled in the art.

[0027] Preparation method of amino graphene: dissolve 50 mL of ethylenediamine in 10 mL of N,N-dimethylformamide solvent, mix evenly, add 200 mg of graphene oxide, 500 mg of N,N-dicyclohexylcarbodiimide and 50 mg of 4-dimethylaminopyridine, stir and disperse, heat to 80°C, reflux for 48 hours, wash with deionized water after the reaction, and dry to obtain amino graphene.

[0028] Preparation method of 3-iodopropyltriethoxysilane: Under nitrogen conditions, 20 g of 3-chlorotriethoxysilane is added to an acetone solvent, and then 14.5 g of potassium iodide is added thereto, the temperature is raised to 55°C, and the reaction is refluxed for 24 hours. After the reaction is completed, it is cooled to room temperature, filtered, and the solvent is removed by rotary evaporation to obtain 3-iodopropyltriethoxysilane.

[0029] Example 1

[0030] (1) 2 g of amino graphene, 30 g of 5-hydroxyisophthalic acid, and 10 g of formaldehyde were added to a toluene solvent, stirred and dispersed, heated to 110° C., reacted for 6 h, washed with deionized water, and dried to obtain carboxylated graphene.

[0031] (2) Add 10 g of 3,5-dihydroxybenzoic acid, 20 g of 3-iodopropyltriethoxysilane, and 30 g of potassium carbonate to tetrahydrofuran solvent, heat to 75° C., react for 8 h, and after the reaction is completed, cool to room temperature, wash with saturated brine, dry, and concentrate by rotary evaporation to obtain disilanebenzoic acid.

[0032] (3) 10 g of hexagonal boron nitride and 8 g of 3,5-bis-aminomethyl-benzoic acid were added to a 1.4 mol / L sodium hydroxide solution, and zirconium oxide ball milling beads were added thereto. The mixture was ball milled for 12 h. After the reaction was completed, the ball milling beads were sieved out, and a 0.8 mol / L hydrochloric acid solution was added thereto. The mixture was filtered, washed with deionized water, and dried to obtain carboxylated boron nitride.

[0033] (4) Add 5 g of carboxylated graphene, 0.5 g of disiloxane benzoic acid, and 0.8 g of carboxylated boron nitride to a 85% polyphosphoric acid solution, stir and disperse, then add 3 g of 4,6-diaminohydroquinone, heat to 140° C., stir and react for 24 h, then heat to 170° C., react for 24 h, and obtain a graphene composite copolymer solution.

[0034] (5) pouring the graphene composite copolymer solution onto a stainless steel composite plate, placing it in a hot press, and hot pressing it at 180° C. and 10 MPa for 30 minutes to form a film. After the hot pressing is completed, the pressure is released, and the plate is immersed in deionized water for 3 days and dried to obtain a friction-resistant graphene film.

[0035] Example 2

[0036] (1) 2 g of amino graphene, 35 g of 5-hydroxyisophthalic acid, and 12 g of formaldehyde were added to a toluene solvent, stirred and dispersed, heated to 100° C., reacted for 10 h, washed with deionized water, and dried to obtain carboxylated graphene.

[0037] (2) Add 10 g of 3,5-dihydroxybenzoic acid, 24 g of 3-iodopropyltriethoxysilane, and 36 g of potassium carbonate to tetrahydrofuran solvent, heat to 80° C., react for 5 h, and after the reaction is completed, cool to room temperature, wash with saturated brine, dry, and concentrate by rotary evaporation to obtain disilanebenzoic acid.

[0038] (3) 10 g of hexagonal boron nitride and 10 g of 3,5-bis-aminomethyl-benzoic acid were added to a 2 mol / L sodium hydroxide solution, and zirconium oxide ball milling beads were added thereto. The reaction was performed for 15 h. After the reaction was completed, the ball milling beads were sieved out, and a 0.5 mol / L hydrochloric acid solution was added thereto. The reaction was filtered, washed with deionized water, and dried to obtain carboxylated boron nitride.

[0039] (4) Add 5 g of carboxylated graphene, 0.6 g of disiloxane benzoic acid, and 1.2 g of carboxylated boron nitride to a 90% polyphosphoric acid solution, stir and disperse, then add 4 g of 4,6-diaminohydroquinone, heat to 140° C., stir and react for 24 h, then heat to 160° C., react for 20 h, and obtain a graphene composite copolymer solution.

[0040] (5) The graphene composite copolymer solution is poured onto a stainless steel composite plate, which is placed in a hot press and hot pressed at 200° C. and 12 MPa for 50 min to form a film. After the hot press is completed, the film is released from the pressure and immersed in deionized water for 2 days and dried to obtain a friction-resistant graphene film.

[0041] Example 3

[0042] (1) 2 g of amino graphene, 40 g of 5-hydroxyisophthalic acid, and 10 g of formaldehyde were added to a toluene solvent, stirred and dispersed, heated to 105° C., reacted for 6 h, washed with deionized water, and dried to obtain carboxylated graphene.

[0043] (2) Add 10 g of 3,5-dihydroxybenzoic acid, 28 g of 3-iodopropyltriethoxysilane, and 34 g of potassium carbonate to tetrahydrofuran solvent, heat to 80° C., react for 7 h, and after the reaction is completed, cool to room temperature, wash with saturated brine, dry, and concentrate by rotary evaporation to obtain disilanebenzoic acid.

[0044] (3) 10 g of hexagonal boron nitride and 12 g of 3,5-bis-aminomethyl-benzoic acid were added to a 2 mol / L sodium hydroxide solution, and zirconium oxide ball milling beads were added thereto. The reaction was performed for 12 h. After the reaction was completed, the ball milling beads were sieved out, and a 1 mol / L hydrochloric acid solution was added thereto. The reaction was filtered, washed with deionized water, and dried to obtain carboxylated boron nitride.

[0045] (4) Add 5 g of carboxylated graphene, 0.7 g of disiloxane benzoic acid, and 1.4 g of carboxylated boron nitride to a 90% polyphosphoric acid solution, stir and disperse, then add 5 g of 4,6-diaminohydroquinone, heat to 140° C., stir and react for 18 h, then heat to 160° C., react for 30 h, and obtain a graphene composite copolymer solution.

[0046] (5) pouring the graphene composite copolymer solution onto a stainless steel composite plate, placing it in a hot press, and hot pressing it at 190° C. and 10 MPa for 40 minutes to form a film. After the hot pressing is completed, the pressure is released, and the plate is immersed in deionized water for 4 days and dried to obtain a friction-resistant graphene film.

[0047] Example 4

[0048] (1) 2 g of amino graphene, 45 g of 5-hydroxyisophthalic acid, and 10 g of formaldehyde were added to a toluene solvent, stirred and dispersed, heated to 110° C., reacted for 6 h, washed with deionized water, and dried to obtain carboxylated graphene.

[0049] (2) Add 10 g of 3,5-dihydroxybenzoic acid, 32 g of 3-iodopropyltriethoxysilane, and 28 g of potassium carbonate to tetrahydrofuran solvent, heat to 75° C., react for 7 h, and after the reaction is completed, cool to room temperature, wash with saturated brine, dry, and concentrate by rotary evaporation to obtain disilanebenzoic acid.

[0050] (3) 10 g of hexagonal boron nitride and 14 g of 3,5-bis-aminomethyl-benzoic acid were added to a 2 mol / L sodium hydroxide solution, and zirconium oxide ball milling beads were added thereto. The mixture was ball milled for 12 h. After the reaction was completed, the ball milling beads were sieved out, and a 1.5 mol / L hydrochloric acid solution was added thereto. The mixture was filtered, washed with deionized water, and dried to obtain carboxylated boron nitride.

[0051] (4) Add 5 g of carboxylated graphene, 0.8 g of disiloxane benzoic acid, and 1.6 g of carboxylated boron nitride to an 85% polyphosphoric acid solution, stir and disperse, then add 5.5 g of 4,6-diaminohydroquinone, heat to 130° C., stir and react for 24 h, then heat to 170° C., react for 24 h, and obtain a graphene composite copolymer solution.

[0052] (5) The graphene composite copolymer solution is poured onto a stainless steel composite plate, which is placed in a hot press and hot pressed at 190° C. and 10 MPa for 30 min to form a film. After the hot press is completed, the pressure is released, and the plate is immersed in deionized water for 4 days and dried to obtain a friction-resistant graphene film.

[0053] Example 5

[0054] (1) 2 g of amino graphene, 48 g of 5-hydroxyisophthalic acid, and 12 g of formaldehyde were added to a toluene solvent, stirred and dispersed, heated to 120° C., reacted for 8 h, washed with deionized water, and dried to obtain carboxylated graphene.

[0055] (2) Add 10 g of 3,5-dihydroxybenzoic acid, 34 g of 3-iodopropyltriethoxysilane, and 35 g of potassium carbonate to tetrahydrofuran solvent, heat to 80° C., react for 5 h, and after the reaction is completed, cool to room temperature, wash with saturated brine, dry, and concentrate by rotary evaporation to obtain disilanebenzoic acid.

[0056] (3) 10 g of hexagonal boron nitride and 16 g of 3,5-bis-aminomethyl-benzoic acid were added to a 2 mol / L sodium hydroxide solution, and zirconium oxide ball milling beads were added thereto. The reaction was performed for 12 h. After the reaction was completed, the ball milling beads were sieved out, and a 1 mol / L hydrochloric acid solution was added thereto. The reaction was filtered, washed with deionized water, and dried to obtain carboxylated boron nitride.

[0057] (4) Add 5 g of carboxylated graphene, 1 g of disiloxane benzoic acid, and 2 g of carboxylated boron nitride to an 85% polyphosphoric acid solution, stir and disperse, then add 6 g of 4,6-diaminohydroquinone, heat to 130° C., stir and react for 18 h, then heat to 170° C., react for 18 h, and obtain a graphene composite copolymer solution.

[0058] (5) The graphene composite copolymer solution is poured onto a stainless steel composite plate, which is placed in a hot press and hot pressed at 170° C. and 10 MPa for 40 min to form a film. After the hot press is completed, the pressure is released, and the plate is immersed in deionized water for 4 days and dried to obtain a friction-resistant graphene film.

[0059] Comparative Example 1

[0060] The difference between this comparative example and Example 1 is that step (4) does not contain disilanebenzoic acid.

[0061] Comparative Example 2

[0062] The difference between this comparative example and Example 1 is that step (4) does not contain stirring and dispersing of carboxylated boron nitride.

[0063] The mechanical properties of the films were tested using an electronic universal testing machine.

[0064] Tensile strength(MPa) Modulus(GPa) Example 1 121.6 5.5 Example 2 134.8 6.8 Example 3 149.2 8.1 Example 4 165.9 9.4 Example 5 160.1 7.2 Comparative Example 1 113.5 4.6 Comparative Example 2 108.0 4.1

[0065] It can be seen from the table that the graphene film prepared by the present invention has relatively excellent mechanical properties.

[0066] The hardness of the film was tested using a microhardness tester.

[0067] The friction resistance of the film was tested using a friction and wear tester.

[0068] Vickers hardness (HV) Friction coefficient Example 1 151.7 2.3 Example 2 169.4 1.6 Example 3 186.0 1.2 Example 4 197.2 0.6 Example 5 188.4 0.8 Comparative Example 1 143.5 2.8 Comparative Example 2 136.9 3.1

[0069] The smaller the friction coefficient, the better the friction resistance, and the harder the material, the better the friction resistance. As can be seen from the table, the graphene film prepared by the present invention has good friction resistance.

[0070] The above describes the specific embodiments of the present invention. It should be understood that the present invention is not limited to the above specific embodiments, and those skilled in the art may make various modifications or variations within the scope of the claims, which do not affect the essence of the present invention.

Claims

1. A method for preparing a friction-resistant graphene film, characterized in that: The preparation method is as follows: (1) adding carboxylated graphene, disilanebenzoic acid, and carboxylated boron nitride to a 80-90% polyphosphoric acid solution, stirring and dispersing, adding 4,6-diaminohydroquinone thereto, heating to 120-140° C., stirring and reacting for 10-24 hours, and then heating to 160-180° C., reacting for 15-30 hours, to obtain a graphene composite copolymer solution, The preparation method of the carboxylated graphene is as follows: adding amino graphene, 5-hydroxyisophthalic acid and formaldehyde into a toluene solvent, stirring and dispersing, heating to 100-120° C., reacting for 4-10 hours, washing with deionized water, and drying to obtain the carboxylated graphene; The preparation method of the disilanebenzoic acid is as follows: 3,5-dihydroxybenzoic acid, 3-iodopropyltriethoxysilane and potassium carbonate are added to a tetrahydrofuran solvent, the temperature is raised to 70-80° C., the reaction is performed for 4-8 hours, and after the reaction is completed, the mixture is cooled to room temperature, washed with saturated brine, dried, and concentrated by rotary evaporation to obtain disilanebenzoic acid; The preparation method of the carboxylated boron nitride is as follows: hexagonal boron nitride and 3,5-bis-aminomethyl-benzoic acid are added to a 1-2 mol / L sodium hydroxide solution, zirconium oxide ball milling beads are added thereto, and ball milling is performed for 5-15 hours. After the reaction is completed, the ball milling beads are sieved out, and a 0.5-1.5 mol / L hydrochloric acid solution is added thereto, filtered, washed with deionized water, and dried to obtain the carboxylated boron nitride; (2) pouring the graphene composite copolymer solution onto a stainless steel composite plate, placing it in a hot press, hot pressing it into a film for 20-50 minutes, releasing the pressure after the hot pressing, soaking it in deionized water for 2-5 days, and drying it to obtain a friction-resistant graphene film.

2. The method for preparing the friction-resistant graphene film according to claim 1, characterized in that: In the step (1), the mass ratio of carboxylated graphene, disilanebenzoic acid, carboxylated boron nitride and 4,6-diaminohydroquinone is 100:10-20:15-40:60-120.

3. The method for preparing the friction-resistant graphene film according to claim 1, characterized in that: In the step (2), the hot press pressure is 8-12 MPa and the temperature is 160-200°C.

4. The method for preparing the friction-resistant graphene film according to claim 1, characterized in that: The mass ratio of the amino graphene, 5-hydroxyisophthalic acid and formaldehyde is 1:15-24:4.5-6.

5. The method for preparing the friction-resistant graphene film according to claim 1, characterized in that: The mass ratio of the 3,5-dihydroxybenzoic acid, 3-iodopropyltriethoxysilane and potassium carbonate is 1:2-3.4:2.5-3.

6.

6. The method for preparing the friction-resistant graphene film according to claim 1, characterized in that: The mass ratio of the hexagonal boron nitride to 3,5-bis-aminomethyl-benzoic acid is 1:0.8-1.6.