High-rate, long-life lithium metal composite anode materials, their preparation methods, and lithium metal batteries
By screening the alloy meso phase and combining it with lithium metal, a lithium metal composite anode material with refined grains was prepared, which solved the problems of lithium dendrite growth and volume expansion, improved the mechanical strength and electrochemical performance of lithium metal batteries, and extended battery life.
Patent Information
- Application Number
- CN202311848205.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-29
- Publication Date
- 2026-11-17
- Estimated Expiration
- 2043-12-29
AI Technical Summary
The commercial application of lithium metal anodes in lithium metal batteries faces challenges such as lithium dendrite growth, volume expansion, poor mechanical strength, and low rate performance, which existing modification methods have failed to effectively address.
A two-dimensional linear mismatch equation was used to screen the alloy mesophase and lithium metal composite. Through high-temperature melting and ultrasonic treatment, a lithium metal composite anode material with refined grains was prepared, which increased the number of grain boundaries and controlled the grain boundary composition, thereby improving the lithium ion migration ability and structural stability.
It significantly improves the mechanical strength, electrochemical rate performance, and cycle performance of lithium metal anodes, alleviates lithium dendrite problems, and enhances battery safety performance.
Smart Images

Figure CN117802334B_ABST
Abstract
Description
Technical Field
[0001] This invention belongs to the field of lithium battery technology, specifically relating to a high-rate, long-life lithium metal composite anode material, its preparation method, and a lithium metal battery. Background Technology
[0002] With the increasing severity of energy shortages and environmental pollution, lithium metal batteries (Li-S, Li-O2, etc.) have been widely studied as a clean energy source. Lithium metal anodes possess extremely high theoretical specific capacity (3860 mAh·g). -1 Its extremely negative potential (-3.040V vs standard hydrogen electrode) is considered the most promising anode material.
[0003] However, the commercial application of lithium metal anodes still faces a series of challenges, including: (1) the high activity of lithium metal makes it easy to react with the electrolyte, which will lead to the continuous consumption of the electrolyte and the lithium metal anode; (2) uneven lithium deposition during electrochemical cycling leads to the growth of lithium dendrites, which eventually causes the separator to be punctured, resulting in battery short circuits and serious safety accidents; (3) the huge volume change of the lithium metal anode during extraction and insertion leads to electrode pulverization, destroys the solid electrolyte interface (SEI), thereby generating dead lithium and promoting the reaction between the electrolyte and lithium metal; (4) poor mechanical strength and low rate performance cannot maintain the material structure stability under high rate discharge, as well as the difficulties in the preparation of ultra-thin lithium strips; the above problems have a crucial impact on the commercial application of lithium metal batteries.
[0004] In recent years, researchers have tried to address these issues of lithium metal anodes from various aspects, including: adjusting electrolyte additives, using solid electrolyte membranes, modifying current collectors, coating the lithium metal surface with a protective film, and alloying lithium metal. However, none of these methods have fundamentally solved the problems of dendrite growth and volume expansion in lithium metal anodes.
[0005] CN201811182577.3 discloses a lithium metal alloy electrode material, its preparation method, and its application. It introduces the formation of an alloy between Li and Al, Zn, and Ag to reduce side reactions between the lithium metal anode and the electrolyte, improve coulombic efficiency, and simultaneously achieve the advantages of high safety and long cycle life. CN201910552753.6 describes a method for extracting a purified alkali-containing aqueous phase using a composite extraction organic phase, followed by separation to obtain an alkali-rich metal salt organic phase. The obtained alkali-rich metal salt organic phase is then washed with a washing solution and subsequently electrolyzed to obtain a lithium metal alloy. CN201910329991.0 provides a three-dimensional composite lithium metal anode, its preparation method, and lithium metal batteries and lithium-sulfur batteries. A three-dimensional porous conductive material, such as copper foam, a three-dimensional porous copper-zinc alloy, or a three-dimensional porous copper-silver alloy, is immersed in a lithium metal solution at a temperature of 310–900°C. The immersion time and temperature are controlled, and the material is then removed and cooled to obtain a three-dimensional composite lithium metal anode. This method suppresses the formation of lithium dendrites and the resulting volume changes during battery cycling, which is beneficial for the commercial application of lithium metal anodes. CN109167029A proposes a silicon nitride-modified lithium metal anode material for lithium-sulfur batteries and its preparation method. Silicon nitride nanowires are obtained by high-temperature nitriding after hydrolysis of tetraethyl orthosilicate. Lithium metal is then loaded into the silicon nitride nanowires through carbothermal reduction. The resulting lithium metal anode material has silicon nitride nanowires stacked on the surface of the lithium metal phase to form a three-dimensional network coating layer, reducing irreversible lithium metal loss and damage to the separator. However, these methods are not conducive to industrial implementation and have certain shortcomings in improving the rate performance of the lithium metal material and suppressing side reactions with the electrolyte. Summary of the Invention
[0006] To overcome the problems of existing technologies, this invention utilizes a two-dimensional linear mismatch equation to screen alloy materials that meet the mismatch requirements and heterogeneous nucleation conditions with lithium metal. Then, by adjusting the proportions and employing a high-temperature melting method, these alloy materials are composited with pure lithium metal. The size of the lithium metal grains and the composition of the grain boundaries are controlled during the crystallization process, thereby achieving a fine-grained lithium metal alloy anode material. This further increases the number of grain boundaries, inducing the formation of more active sites, thus improving lithium-ion migration capability and enhancing rate performance. Simultaneously, controlling the composition at the grain boundaries passivates the originally more active grain boundaries with the electrolyte, improving structural stability during charge and discharge, and further enhancing the electrochemical cycle stability of the lithium metal anode. Furthermore, due to the significantly refined grains, the dislocations between the lithium metal anode materials are increased, resulting in a significant improvement in its mechanical strength. The lithium metal composite anode material prepared by this method significantly improves the mechanical strength, electrochemical rate performance, and cycle performance of the lithium metal anode, and significantly improves the lithium dendrite problem, leading to a substantial improvement in battery safety.
[0007] This invention first provides a method for preparing a high-rate, long-life lithium metal composite anode material, which includes the following steps:
[0008] A. Under an inert atmosphere, the alloy reactor is heated to 300–1200°C. Metallic lithium is added to the reactor and fully melted. The temperature is then raised to 800–1200°C, and an alloy intermediate phase is added while continuously stirring. In step A, the amount of the alloy intermediate phase added is 0.1–20% of the mass of metallic lithium. In step A, the alloy intermediate phase is at least one of Al2Y, AlB2, or Al2Yb.
[0009] B. After the lithium metal and the alloy intermediate phase are thoroughly mixed at high temperature, ultrasonic treatment is performed to ensure that the materials are mixed evenly.
[0010] C. Under ultrasonic treatment conditions, casting is carried out to obtain alloy ingots. Then, stepwise cooling is adopted. The cooling rate is controlled at 3-5℃ / min before 300℃, and then the cooling rate is controlled at 15-20℃ / min. After cooling, the surface oxide layer is removed. Then, the temperature is raised to 60-150℃ and held for a period of time before cooling to room temperature to obtain lithium alloy ingots.
[0011] D. The lithium alloy ingot obtained in step C is extruded, and the extrusion thickness is controlled between 100 and 300 micrometers. Then, the lithium alloy strip is rolled in multiple passes to obtain a lithium metal composite anode material with a thickness of 10 to 50 micrometers.
[0012] In the above preparation method, in step A, the amount of the alloy intermediate phase added is 0.5 to 10% of the mass of lithium metal.
[0013] In the above preparation method, in step A, the temperature is kept at 300-1200℃ for 0.5-2 hours to fully melt the lithium metal.
[0014] In the above preparation method, in step A, the continuous stirring time is 0.5 to 4 hours.
[0015] In the above preparation method, in step B, the ultrasonic treatment time is 0.2 to 2 hours.
[0016] In the above preparation method, step C involves maintaining the temperature at 60–150°C for 1–6 hours.
[0017] In the above preparation method, steps A to C are all carried out under an inert atmosphere.
[0018] In the above preparation method, in step D, the multi-pass rolling is: the number of rolling passes is controlled to be 2 to 5, and the reduction amount of each rolling is controlled to be 20 to 50%.
[0019] The present invention also provides a high-rate, long-life lithium metal composite anode material, which is prepared by the above method.
[0020] The present invention also provides a lithium metal battery, which uses the above-mentioned lithium metal composite anode material as the anode.
[0021] The beneficial effects of this invention are:
[0022] This invention utilizes a two-dimensional linear mismatch equation to screen alloy materials that meet the mismatch requirements and heterogeneous nucleation conditions with lithium metal. The Al2Y, AlB2, and Al2Yb alloy mesophases form heterogeneous nuclei with lithium metal, preferentially crystallizing to provide directional nucleation sites for molten lithium metal and refining the lithium metal grain size. The activity (lithium ion insertion / extraction activity and reactivity) is highest at the lithium metal grain boundaries. The increased number of grain boundaries after grain refinement enhances the ion migration ability of lithium metal during charge and discharge, further improving the electrochemical rate performance of the lithium metal anode. The heterogeneous nucleation of lithium metal around the Al2Y, AlB2, and Al2Yb alloy mesophases... The nucleus and crystal growth allow the Al2Y, AlB2, and Al2Yb alloy mesophases to fill the grain boundaries. Due to the higher stability of these mesophases, they suppress side reactions between the lithium metal phase and the electrolyte, improving the material's structural stability. Simultaneously, Al2Y, AlB2, and Al2Yb have higher adsorption energies for lithium ions, anchoring the lithium metal deposition process and thus enhancing the cycle stability of the lithium metal anode. The significantly refined grains increase the number of dislocations on the lithium metal material surface, strengthening the mechanical strength of the lithium anode and facilitating the fabrication of ultrathin lithium strips, while reducing the risk of strip breakage during rolling.
[0023] Lithium metal is alloyed with a small amount of Al2Y, AlB2, and Al2Yb alloy intermediate phases. While ensuring that the capacity requirements are met, the rate performance, cycle stability, mechanical properties, and corrosion resistance of the lithium metal composite anode material are enhanced. Furthermore, the lithium-ion intercalation and deintercalation process is optimized, which is beneficial for the application of lithium metal anode materials in primary and secondary batteries. Attached Figure Description
[0024] Figure 1 This is a comparison diagram of the grain size and distribution of pure lithium metal anode and modified composite anode.
[0025] Figure 2 This is a comparison chart of the cycle performance of pure lithium metal anode and modified composite anode.
[0026] Figure 3 This is a comparison chart of the rate performance of pure lithium metal anode and modified composite anode.
[0027] Figure 4 This is a comparison chart of the mechanical strength of pure lithium metal anodes and modified composite anodes. Detailed Implementation
[0028] Specifically, a method for preparing a high-rate, long-life lithium metal composite anode material includes the following steps:
[0029] A. Under an inert atmosphere, the alloy reactor is heated to 300–1200°C. Metallic lithium is added to the reactor and fully melted. The temperature is then raised to 800–1200°C, and an alloy intermediate phase is added while continuously stirring. In step A, the amount of the alloy intermediate phase added is 0.1–20% of the mass of metallic lithium. In step A, the alloy intermediate phase is at least one of Al2Y, AlB2, or Al2Yb.
[0030] B. After the lithium metal and the alloy intermediate phase are thoroughly mixed at high temperature, ultrasonic treatment is performed to ensure that the materials are mixed evenly.
[0031] C. Under ultrasonic treatment conditions, casting is carried out to obtain alloy ingots. Then, stepwise cooling is adopted. The cooling rate is controlled at 3-5℃ / min before 300℃, and then the cooling rate is controlled at 15-20℃ / min. After cooling, the surface oxide layer is removed. Then, the temperature is raised to 60-150℃ and held for a period of time before cooling to room temperature to obtain lithium alloy ingots.
[0032] D. The lithium alloy ingot obtained in step C is extruded (usually in an extruder), and the extrusion thickness is controlled to be 100-300 micrometers. Then, the lithium metal alloy strip is rolled through multiple passes to obtain a lithium metal composite anode material with a thickness of 10-50 micrometers.
[0033] In step A of this invention, because lithium metal has high reactivity, the reactor is generally dried in a vacuum environment at 60-120°C (generally for 2-10 hours) to remove water in advance, so as to avoid water reacting with lithium metal at high temperature in the later stage and producing impurities.
[0034] In step A of this invention, the alloy reactor is heated to 300–1200°C and held at that temperature for 0.5–2 hours to ensure that the lithium metal added to the reactor is fully melted. If the temperature at which the lithium metal is melted is too low, the temperature needs to be raised to 800–1200°C before adding the alloy intermediate phase; if the temperature at which the lithium metal is melted is 800–1200°C, further heating is not necessary.
[0035] Through screening, this invention has obtained alloy materials that can meet the mismatch requirements and heterogeneous nucleation conditions with metallic lithium. The intermediate phases of Al2Y, AlB2, and Al2Yb alloys can form heterogeneous nucleation with metallic lithium; however, alloys such as Al2Ca and AlMg2 are not applicable.
[0036] In step A of this invention, it is necessary to control the amount of the alloy mesophase. Preferably, the amount of alloy mesophase added is controlled to be 0.5-10% of the mass of lithium metal, resulting in a negative electrode material with superior performance.
[0037] In step A of this invention, after adding the alloy meso phase, the stirring time is controlled to be 0.5 to 4 hours, so that the lithium metal and the alloy meso phase are melted and alloyed.
[0038] In step B of this invention, although high-temperature stirring ensures thorough mixing of the materials, the inventors discovered that direct casting easily leads to segregation and sedimentation. Therefore, to ensure uniform mixing of the molten lithium alloy throughout the reactor during casting, ultrasonic treatment using equipment such as a ring-shaped ultrasonic transducer is necessary. In step B, the ultrasonic treatment time is 0.2–2 hours.
[0039] In step C of this invention, ultrasonication is only used to ensure that the alloy lithium liquid entering the casting port is uniformly mixed before the mixed alloy material is poured. During the casting process, the casting mold is not ultrasonicated.
[0040] In step C of this invention, the cooling process is controlled as follows: before 300℃ (i.e., 300~1200℃), a cooling rate of 5℃ / min is used to ensure that the alloy mesophase is evenly distributed throughout the entire lithium metal melt during the preferential nucleation process in the early stage (the melting point of the alloy mesophase is higher than that of lithium metal), and to avoid clustering together to form a concentrated area of alloy mesophase; when cooling down to room temperature below 300℃, a cooling rate of 20℃ / min is used because at this time the alloy mesophase has been completely nucleated and distributed throughout the entire melt, and rapid cooling will ensure that the lithium metal phase undergoes heterogeneous nucleation and growth along the grains of the alloy mesophase, thereby achieving the purpose of grain refinement.
[0041] In step C of this invention, after casting, the purpose of heating again to 60–150°C and holding at that temperature is to perform a secondary annealing treatment on the lithium alloy ingot, further improving the crystallinity of the lithium phase and releasing the internal stress of the material. In step C, the temperature is held at 60–150°C for 1–6 hours.
[0042] In this invention, steps A through C are all carried out under an inert atmosphere; step D is generally carried out in a drying room, with the dew point controlled at -45°C to -60°C.
[0043] In step D of this invention, a lithium alloy ingot is placed in an extruder for extrusion. The extrusion die is controlled to control the extrusion thickness to be between 100 and 300 micrometers. The lithium metal alloy strip is then rolled through multiple passes, with the number of rolling passes controlled to be between 2 and 5. The reduction amount in each rolling pass is controlled to be between 20 and 50%, and finally a thickness of 10 to 50 micrometers is obtained. The strip is then sliced to obtain the lithium metal composite anode.
[0044] The present invention also provides a high-rate, long-life lithium metal composite anode material, which is prepared by the above method.
[0045] The present invention also provides a lithium metal battery, which uses the above-mentioned lithium metal composite anode material as the anode.
[0046] The present invention will be further described in detail below through embodiments, but the scope of protection of the present invention is not limited to the embodiments described herein.
[0047] Example 1
[0048] The alloy reactor was dried in a vacuum environment at 80℃ for 5 hours, then heated to 800℃ and held for 2 hours in an argon atmosphere. Lithium metal was added to the reactor and fully melted, followed by the addition of 2 wt.% Al₂B and continuous stirring for 1 hour. After the metals were fully mixed, the melting reactor was placed in a ring-shaped ultrasonic instrument and ultrasonically treated for 30 minutes to ensure uniform mixing. Under ultrasonic treatment, the mixture was cast to obtain a lithium alloy ingot. The ingot was then cooled in stages (the cooling rate was controlled at 5℃ / min before 300℃, and 20℃ / min thereafter), and the surface oxide layer was removed after cooling. The resulting lithium alloy ingot was then heated to 110℃ and held for 4 hours before being cooled to room temperature. The ingot was then extruded using an extruder, with the extrusion die controlled to maintain an extrusion thickness of 200 micrometers. The lithium alloy strip was then rolled in multiple passes, with each roll reduction controlled at 50%, resulting in a final thickness of 25 micrometers. Finally, the strip was sliced using a slicing machine to obtain a composite lithium metal anode suitable for battery assembly.
[0049] In an inert atmosphere glove box, a 2032 coin cell was assembled with an S positive electrode, using 1.0M LiTFSI as the lithium salt and DME:DOL = 1:1 as the electrolyte, and then electrochemical performance was tested.
[0050] Example 2
[0051] The alloy reactor was dried in a vacuum environment at 80℃ for 5 hours, then heated to 1000℃ and held for 2 hours in an argon atmosphere. Metallic lithium was added to the reactor and fully melted, followed by the addition of 2 wt.% AlB2 and 1 wt.% Al2Y, and stirring was continued for 1 hour. After the metals were fully mixed, the smelting reactor was placed in a ring-shaped ultrasonic instrument and ultrasonically treated for 30 minutes to ensure uniform mixing. Under ultrasonic treatment conditions, casting was performed to obtain lithium alloy ingots, with stepped cooling (controlled cooling before 300℃). The heating rate was 5℃ / min, followed by a cooling rate of 20℃ / min. After cooling, the surface oxide layer was removed. The resulting lithium alloy ingot was then heated to 110℃ and held for 4 hours before being cooled to room temperature. The lithium alloy ingot was then extruded using an extruder, with the extrusion die controlled to maintain an extrusion thickness of 200 micrometers. The lithium alloy strip was then rolled in multiple passes, with each rolling pass having a reduction of 50%, resulting in a final thickness of 25 micrometers. Finally, the strip was sliced using a slicing machine to obtain a composite lithium metal anode suitable for battery assembly.
[0052] In an inert atmosphere glove box, a 2032 coin cell was assembled with an S positive electrode, using 1.0M LiTFSI as the lithium salt and DME:DOL = 1:1 as the electrolyte, and then electrochemical performance was tested.
[0053] Example 3
[0054] The alloy reactor was dried in a vacuum environment at 80℃ for 5 hours, then heated to 1000℃ and held for 2 hours in an argon atmosphere. Lithium metal was added to the reactor and fully melted, followed by the addition of 2 wt.% Al2Yb and continuous stirring for 1 hour. After the metals were fully mixed, the melting reactor was placed in a ring-shaped ultrasonic instrument and ultrasonically treated for 30 minutes to ensure uniform mixing. Under ultrasonic treatment, the mixture was cast to obtain a lithium alloy ingot. The ingot was then cooled in stages (the cooling rate was controlled at 5℃ / min before 300℃, and then at 20℃ / min thereafter). After cooling, the surface oxide layer was removed. The resulting lithium alloy ingot was then heated to 110℃ and held for 4 hours before being cooled to room temperature. The lithium alloy ingot was then extruded using an extruder, with the extrusion die controlled to maintain an extrusion thickness of 200 micrometers. The lithium alloy strip was then rolled in multiple passes, with each rolling pass having a reduction of 50%, resulting in a final thickness of 25 micrometers. Finally, the strip was sliced using a slicing machine to obtain a composite lithium metal anode suitable for battery assembly.
[0055] In an inert atmosphere glove box, a 2032 coin cell was assembled with an S positive electrode, using 1.0M LiTFSI as the lithium salt and DME:DOL = 1:1 as the electrolyte, and then electrochemical performance was tested.
[0056] Example 4
[0057] The alloy reactor was dried in a vacuum environment at 80℃ for 5 hours, then heated to 1100℃ and held for 2 hours in an argon atmosphere. Metallic lithium was added to the reactor and fully melted, followed by the addition of 2 wt.% Al₂Yb and 1 wt.% Al₂Y, and stirring was continued for 1 hour. After the metals were fully mixed, the smelting reactor was placed in a ring-shaped ultrasonic instrument and ultrasonically treated for 30 minutes to ensure uniform mixing. Under ultrasonic treatment conditions, casting was performed to obtain lithium alloy ingots, with stepped cooling (controlled cooling before 300℃). The heating rate was 5℃ / min, followed by a cooling rate of 20℃ / min. After cooling, the surface oxide layer was removed. The resulting lithium alloy ingot was then heated to 110℃ and held for 4 hours before being cooled to room temperature. The lithium alloy ingot was then extruded using an extruder, with the extrusion die controlled to maintain an extrusion thickness of 200 micrometers. The lithium alloy strip was then rolled in multiple passes, with each rolling pass having a reduction of 50%, resulting in a final thickness of 25 micrometers. Finally, the strip was sliced using a slicing machine to obtain a composite lithium metal anode suitable for battery assembly.
[0058] In an inert atmosphere glove box, a 2032 coin cell was assembled with an S positive electrode, using 1.0M LiTFSI as the lithium salt and DME:DOL = 1:1 as the electrolyte, and then electrochemical performance was tested.
[0059] Example 5
[0060] The alloy reactor was dried in a vacuum environment at 80℃ for 5 hours, then heated to 1200℃ and held for 2 hours in an argon atmosphere. Metallic lithium was added to the reactor and fully melted, followed by the addition of 2 wt.% Al₂Yb and 2 wt.% Al₂Y, and stirring was continued for 1 hour. After the metals were fully mixed, the smelting reactor was placed in a ring-shaped ultrasonic instrument and ultrasonically treated for 30 minutes to ensure uniform mixing. Under ultrasonic treatment conditions, casting was performed to obtain lithium alloy ingots, with stepped cooling (controlled cooling before 300℃). The heating rate was 5℃ / min, followed by a cooling rate of 20℃ / min. After cooling, the surface oxide layer was removed. The resulting lithium alloy ingot was then heated to 120℃ and held for 4 hours before being cooled to room temperature. The lithium alloy ingot was then extruded using an extruder, with the extrusion die controlled to maintain an extrusion thickness of 200 micrometers. The lithium alloy strip was then rolled in multiple passes, with each rolling pass having a reduction of 50%, resulting in a final thickness of 25 micrometers. Finally, the strip was sliced using a slicing machine to obtain a composite lithium metal anode suitable for battery assembly.
[0061] In an inert atmosphere glove box, a 2032 coin cell was assembled with an S positive electrode, using 1.0M LiTFSI as the lithium salt and DME:DOL = 1:1 as the electrolyte, and then electrochemical performance was tested.
[0062] Example 6
[0063] The alloy reactor was dried in a vacuum environment at 80℃ for 5 hours, then heated to 1200℃ and held for 2 hours in an argon atmosphere. Lithium metal was added to the reactor and fully melted, followed by the addition of 0.5 wt.% Al2Y, and stirring was continued for 1 hour. After the metals were fully mixed, the melting reactor was placed in a ring-shaped ultrasonic instrument for 30 minutes to ensure uniform mixing. Under ultrasonic treatment, the mixture was cast to obtain a lithium alloy ingot. The ingot was then cooled in stages (the cooling rate was controlled at 5℃ / min before 300℃, and 20℃ / min thereafter), and the surface oxide layer was removed after cooling. The resulting lithium alloy ingot was then heated to 120℃ and held for 4 hours before being cooled to room temperature. The ingot was then extruded using an extruder, with the extrusion die controlled to maintain an extrusion thickness of 200 micrometers. The lithium alloy strip was then rolled in multiple passes, with each roll reduction controlled at 50%, resulting in a final thickness of 25 micrometers. Finally, the strip was sliced using a slicing machine to obtain a composite lithium metal anode suitable for battery assembly.
[0064] In an inert atmosphere glove box, a 2032 coin cell was assembled with an S positive electrode, using 1.0M LiTFSI as the lithium salt and DME:DOL = 1:1 as the electrolyte, and then electrochemical performance was tested.
[0065] Example 7
[0066] The alloy reactor was dried in a vacuum environment at 80℃ for 5 hours, then heated to 1200℃ and held for 2 hours in an argon atmosphere. Metallic lithium was added to the reactor and fully melted, followed by the addition of 5 wt.% Al₂Yb and 5 wt.% Al₂Y, and stirring was continued for 1 hour. After the metals were fully mixed, the smelting reactor was placed in a ring-shaped ultrasonic instrument for 30 minutes to ensure uniform mixing. Under ultrasonic treatment conditions, casting was performed to obtain lithium alloy ingots, with stepped cooling (temperature controlled before 300℃). The heating rate was 5℃ / min, followed by a cooling rate of 20℃ / min. After cooling, the surface oxide layer was removed. The resulting lithium alloy ingot was then heated to 120℃ and held for 4 hours before being cooled to room temperature. The lithium alloy ingot was then extruded using an extruder, with the extrusion die controlled to maintain an extrusion thickness of 200 micrometers. The lithium alloy strip was then rolled in multiple passes, with each rolling pass having a reduction of 50%, resulting in a final thickness of 25 micrometers. Finally, the strip was sliced using a slicing machine to obtain a composite lithium metal anode suitable for battery assembly.
[0067] In an inert atmosphere glove box, a 2032 coin cell was assembled with an S positive electrode, using 1.0M LiTFSI as the lithium salt and DME:DOL = 1:1 as the electrolyte, and then electrochemical performance was tested.
[0068] Comparative Example 1
[0069] In an inert atmosphere glove box, pure metallic lithium sheets were used as the negative electrode material, along with S positive electrode sheets, 1.0M LiTFSI as the lithium salt, and DME:DOL = 1:1 as the electrolyte, to assemble a 2032 coin cell, and then electrochemical performance was tested.
[0070] Comparative Example 2
[0071] The alloy reactor was dried in a vacuum environment at 80℃ for 5 hours, then heated to 800℃ and held for 2 hours in an argon atmosphere. Lithium metal was added to the reactor and fully melted, followed by the addition of 2 wt.% Al₂Ca and continuous stirring for 1 hour. After the metals were fully mixed, the melting reactor was placed in a ring-shaped ultrasonic instrument and ultrasonically treated for 30 minutes to ensure uniform mixing. Under ultrasonic treatment, the mixture was cast to obtain a lithium alloy ingot. The ingot was then cooled in stages (the cooling rate was controlled at 5℃ / min before 300℃, and 20℃ / min thereafter), and the surface oxide layer was removed after cooling. The resulting lithium alloy ingot was then heated to 120℃ and held for 4 hours before being cooled to room temperature. The ingot was then extruded using an extruder, with the extrusion die controlled to maintain an extrusion thickness of 200 micrometers. The lithium alloy strip was then rolled in multiple passes, with each roll reduction controlled at 50%, resulting in a final thickness of 25 micrometers. Finally, the strip was sliced using a slicing machine to obtain a composite lithium metal anode suitable for battery assembly.
[0072] In an inert atmosphere glove box, a 2032 coin cell was assembled with an S positive electrode, using 1.0M LiTFSI as the lithium salt and DME:DOL = 1:1 as the electrolyte, and then electrochemical performance was tested.
[0073] Comparative Example 3
[0074] The alloy reactor was dried in a vacuum environment at 80℃ for 5 hours, then heated to 800℃ and held for 2 hours in an argon atmosphere. Lithium metal was added to the reactor and fully melted, followed by the addition of 2 wt.% AlMg2, and stirring was continued for 1 hour. After the metals were fully mixed, the melting reactor was placed in a ring-shaped ultrasonic instrument for 30 minutes to ensure uniform mixing. Under ultrasonic treatment, the mixture was cast to obtain a lithium alloy ingot. The ingot was then cooled in stages (the cooling rate was controlled at 5℃ / min before 300℃, and 20℃ / min thereafter), and the surface oxide layer was removed after cooling. The resulting lithium alloy ingot was then heated to 120℃ and held for 4 hours before being cooled to room temperature. The ingot was then extruded using an extruder, with the extrusion die controlled to maintain an extrusion thickness of 200 micrometers. The lithium alloy strip was then rolled in multiple passes, with each roll reduction controlled at 50%, resulting in a final thickness of 25 micrometers. Finally, the strip was sliced using a slicing machine to obtain a composite lithium metal anode suitable for battery assembly.
[0075] In an inert atmosphere glove box, a 2032 coin cell was assembled with an S positive electrode, using 1.0M LiTFSI as the lithium salt and DME:DOL = 1:1 as the electrolyte, and then electrochemical performance was tested.
[0076] Table 1 Electrochemical Cyclic Performance Data
[0077] sample magnification Number of cycles Capacity retention Comparative Example 1 0.5C 100 75% Comparative Example 2 0.5C 100 73% Comparative Example 3 0.5C 100 67% Example 3 0.5C 100 92% Example 4 0.5C 100 84%
[0078] Figure 1 This image shows a comparison of grain size and distribution between pure lithium metal anodes and modified composite anodes. Figure 1 The scanning electron microscope images show that the grain size of Li-Al2Yb is significantly smaller than that of pure lithium metal, resulting in a significant increase in the number of grain boundaries. This confirms that the addition of the intermediate phase in this alloy achieves the effect of heterogeneous nucleation and reduces the grain size.
[0079] exist Figure 2 , Figure 3 and Figure 4 The electrochemical cycle stability, rate performance, and mechanical strength of pure lithium metal electrodes and lithium metal composite anodes were compared. Figure 2 It is evident that alloying treatment improves the side reactions between the lithium metal anode and the electrolyte to a certain extent, enhances the material structure stability during charging and discharging, thereby improving the cycle stability of the battery and giving it a longer cycle life. Figure 3 This demonstrates a significant improvement in electrochemical rate performance of lithium metal composite anode materials. Meanwhile, Figure 4 The differences in mechanical strength resulting from refining lithium metal anode grains were compared. The alloy intermediates selected using a two-dimensional linear mismatch equation had a significant impact on lithium metal growth and nucleation, leading to a substantial reduction in lithium metal anode grain size and an increase in surface dislocations, thus achieving high mechanical strength. Therefore, the composite alloy anode prepared through this alloying method is an effective approach to extend battery cycle life, enhance rate performance, and improve mechanical strength.
Claims
1. A method for preparing high-rate, long-life lithium metal composite anode material, characterized in that: Includes the following steps: A. Under an inert atmosphere, the alloy reactor is heated to 300~1200℃. After the metallic lithium is fully melted in the reactor, the temperature is raised to 800~1200℃, an alloy mesophase is added, and stirring is continued. In step A, the amount of the alloy mesophase added is 0.1~20% of the mass of the metallic lithium. In step A, the alloy mesophase is Al2Y and AlB2, or Al2Y and Al2Yb. B. After the lithium metal and the alloy intermediate phase are thoroughly mixed at high temperature, ultrasonic treatment is performed to ensure that the materials are mixed evenly. C. Under ultrasonic treatment conditions, casting is carried out to obtain alloy ingots. Then, stepwise cooling is adopted. The cooling rate is controlled at 3~5℃ / min before 300℃, and then the cooling rate is controlled at 15~20℃ / min. After cooling, the surface oxide layer is removed. Then, the temperature is raised to 60~150℃ and held for a period of time before cooling to room temperature to obtain lithium alloy ingots. D. The lithium alloy ingot obtained in step C is extruded, and the extrusion thickness is controlled at 100~300 micrometers. Then, the lithium metal alloy strip is rolled through multiple passes to obtain a lithium metal composite anode material with a thickness of 10~50 micrometers. In step A, the temperature is maintained at 300~1200℃ for 0.5~2h to allow the metallic lithium to fully melt; In step A, the continuous stirring time is 0.5~4h; In step B, the ultrasonic treatment time is 0.2~2 hours; In step C, maintain the temperature at 60~150℃ for 1~6 hours; Steps A through C were all performed under an inert atmosphere; In step D, the multi-pass rolling is as follows: the number of rolling passes is controlled to be 2 to 5, and the reduction amount of each rolling pass is controlled to be 20 to 50%.
2. The method for preparing the high-rate, long-life lithium metal composite anode material according to claim 1, characterized in that: In step A, the amount of the alloy intermediate phase added is 0.5 to 10% of the mass of lithium metal.
3. The high-rate, long-life lithium metal composite anode material prepared by the method described in claim 1.
4. A lithium metal battery, characterized in that: The lithium metal composite anode material as described in claim 3 is used as the anode.
Citation Information
Patent Citations
A metal lithium anode material modified with silicon nitride for lithium-sulfur battery and a preparation method thereof
CN109167029A
Three-dimensional composite metal lithium negative electrode, preparation method thereof, lithium metal battery and lithium-sulfur battery
CN110112367A
Metal lithium alloy as well as preparation method and application thereof
CN110564965A
Metal lithium alloy electrode material, preparation method thereof and metal lithium secondary battery
CN111048744A
0.008-0.016 mm H18 specification lithium battery current collector aluminum foil and production process thereof
CN116043071A