A high-strength and high-plasticity extrusion casting aluminum alloy and preparation method thereof
By optimizing the composition and process of aluminum alloys, the contradiction between strength and plasticity of extrusion-cast aluminum alloys is solved, and high-strength and high-plasticity aluminum alloys are achieved to meet the needs of lightweight structural parts and improve production efficiency and performance. .
Patent Information
- Application Number
- CN202410024052.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-08
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-01-08
AI Technical Summary
There is a contradiction between strength and plasticity in existing extrusion cast aluminum alloys, which cannot meet the demand for high strength and high plasticity in lightweight development.
By scientifically designing the composition of aluminum alloys, including Si, Mg, Ti, Sr and controlling the content of Fe impurity elements, combined with argon injection refining, bubbling hydrogen removal and solid solution aging treatment, the squeeze casting process is optimized to form a high-quality Aluminum alloy with high strength and plasticity.
It significantly improves the tensile strength, yield strength and elongation after fracture of extrusion cast aluminum alloy, improves the overall performance of aluminum alloy, meets the demand for lightweight structural parts, and shortens production process time and energy consumption.
Smart Images

Figure CN117802364B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of aluminum alloys and preparation thereof, in particular to a high-strength and high-plasticity extrusion casting aluminum alloy and a preparation method thereof. Background Art
[0002] Aluminum alloy has the advantages of low density, high specific strength, good electrical and thermal conductivity, and recyclability. It is widely used in the fields of automobiles, rail transit, mechanical equipment, etc., and is used to manufacture various load-bearing structural parts. With the development of lightweight automobiles, rail transit, and mechanical equipment, higher requirements are also placed on the comprehensive mechanical properties of aluminum alloy parts, such as higher strength and plasticity, to improve safety and service life. Squeeze casting is a technology that solidifies aluminum alloy liquid under the direct action of extrusion force. Squeeze casting technology has a strong shrinkage compensation function and is very suitable for the production of high-strength aluminum alloy parts.
[0003] The invention patent document with publication number CN112375941A describes "An extrusion casting aluminum alloy material and its preparation method". The aluminum alloy material disclosed therein has a tensile strength of 329.85-354.23 MPa, a yield strength of 222.07-224.88 MPa, and an elongation of 2.64-2.8%.
[0004] The invention patent document with publication number CN108251714A describes "A high-strength and toughness aluminum alloy produced by extrusion casting and its extrusion casting method". The aluminum alloy material disclosed therein has a tensile strength of 351.4-395.1 MPa, a yield strength of 303.8-345.2 MPa, and an elongation of 6.2-7.2%.
[0005] The invention patent document with publication number CN108796317A describes "A semi-solid extrusion cast aluminum alloy suitable for new energy vehicles and a preparation method thereof". The aluminum alloy disclosed therein has a tensile strength greater than 420 MPa, a yield strength greater than 380 MPa, and a thermal conductivity greater than 160 W / m·K, but an elongation less than 1%.
[0006] From the production practice and literature retrieval results, there is a contradiction between the strength and plasticity of the current extrusion casting aluminum alloy, that is, the existing extrusion casting aluminum alloy either has high strength and low plasticity, or high plasticity and low strength, so that the strength and plasticity of the existing extrusion casting aluminum alloy cannot meet the requirements of the lightweight development of various load-bearing structural parts for high-strength and high-plasticity extrusion casting aluminum alloys. Therefore, the existing extrusion casting aluminum alloys and their preparation methods still need to be improved and developed. Summary of the invention
[0007] The purpose of the present invention is to provide a high-strength and high-plasticity extrusion cast aluminum alloy and a preparation method thereof in view of the above-mentioned problems. By scientifically designing the component composition and preparation process of the extrusion cast aluminum alloy, the strength and plasticity of the extrusion cast aluminum alloy are improved at the same time, so that the extrusion cast aluminum alloy can meet the demand for high-strength and high-plasticity extrusion cast aluminum alloys for lightweight development of various load-bearing structural parts.
[0008] The technical solution adopted by the present invention is as follows: a high-strength and high-plasticity extrusion casting aluminum alloy, which is composed of the following components in mass percentage: Si (6.5-7.5%), Mg (0.25-0.45%), Ti (0.08-0.12%), Sr (0.01-0.03%), Fe not exceeding 0.15%, and the rest being Al and other inevitable impurities.
[0009] Among them, Si and Mg are the main strengthening elements of the extrusion casting aluminum alloy. Si and Mg can form Mg2Si strengthening phase, which significantly enhances the strength of the extrusion casting aluminum alloy. The higher the content of Si and Mg, the higher the strength of the extrusion casting aluminum alloy. However, if the content of Si and Mg is too high, the plasticity of the extrusion casting aluminum alloy will be reduced. Preferably, the content of Si is 6.5-7.5%, and the content of Mg is 0.25-0.45%.
[0010] Ti exists in the form of aluminum-titanium alloy in extrusion casting aluminum alloy. Its main function is to refine the coarse dendritic α-Al grains, improve the uniformity of the organizational composition of the aluminum alloy, and improve the casting fluidity, strength and plasticity of the aluminum alloy. If the Ti content is too low, the grain refinement effect is not obvious; but if the Ti content is too high, the grain refinement effect will not be significantly improved, but the production cost will increase. Therefore, as a preferred embodiment, the Ti content is 0.08-0.12%.
[0011] Sr exists in the form of aluminum-strontium alloy in the extrusion casting aluminum alloy. Its main function is to refine the modified eutectic Si phase. The eutectic Si phase is usually distributed in the aluminum alloy matrix in the form of coarse flakes. This coarse flake eutectic Si phase will seriously split the aluminum alloy matrix, which is an important reason for the low strength, especially low plasticity, of the extrusion casting aluminum alloy. Adding 0.01-0.03% Sr can change the morphology of eutectic Si in the extrusion casting aluminum alloy from coarse flakes to fine and uniform particles or fibers, which can significantly improve the strength and plasticity of the extrusion casting aluminum alloy.
[0012] Fe is an inevitable impurity element in squeeze casting aluminum alloys. It is usually distributed in the aluminum alloy matrix in the form of coarse needle-shaped Fe-rich phases. The coarse needle-shaped Fe-rich phases will seriously split the aluminum alloy matrix, which is an important reason for the low strength and especially low plasticity of squeeze casting aluminum alloys. Therefore, the content of impurity element Fe must be strictly controlled to make the Fe content ≤0.15%.
[0013] Furthermore, among other impurities, the proportion of a single element does not exceed 0.05%, and the total amount does not exceed 0.15%.
[0014] A method for preparing an aluminum alloy, preparing the high-strength and high-plasticity extrusion casting aluminum alloy, comprising the following steps:
[0015] S1: melting and preparing aluminum alloy liquid according to the composition and mass percentage of the aluminum alloy, and raising the temperature of the aluminum alloy liquid to 700-730°C;
[0016] S2: using argon as a carrier and a current refining agent, the aluminum alloy liquid is subjected to a slag removal treatment by a spray refining method, and then the scum on the surface of the aluminum alloy liquid is removed; specifically, using argon as a carrier, a powdered refining agent is sprayed into the aluminum alloy liquid through a powder spray tank for refining and slag removal;
[0017] S3: introducing a mixed gas consisting of argon and chlorine into the aluminum alloy liquid in a bubbling manner to perform a dehydrogenation treatment;
[0018] S4: forming an aluminum alloy by extrusion casting the aluminum alloy liquid;
[0019] S5: The aluminum alloy is subjected to solid solution and aging treatment to obtain an extrusion casting aluminum alloy with high strength and high plasticity.
[0020] Furthermore, in step S1, the raw materials of corresponding elements can be pure aluminum ingots, pure magnesium ingots, aluminum-silicon alloys, aluminum-titanium alloys and aluminum-strontium alloys. After calculation and weighing, a furnace is selected to melt the raw materials into aluminum alloy liquid, and then the temperature of the aluminum alloy liquid is increased to 700-730°C. This temperature range can not only ensure that the aluminum alloy liquid has high fluidity, but also reduce the oxidation damage of the aluminum alloy liquid due to excessive temperature, thereby achieving the purpose of reducing the oxidation burning of the aluminum alloy liquid.
[0021] It should be noted that the inclusions in the aluminum alloy liquid are mainly oxides, especially aluminum oxide, which mainly come from the oxide film (aluminum oxide film) on the surface of raw materials such as aluminum ingots, magnesium ingots, and alloys, and the oxide (aluminum oxide) produced by the oxidation of the aluminum alloy liquid during the smelting process. Other inclusions also include the combustion products of non-aluminum materials and the slag falling off the furnace lining. If these inclusions are left in the squeeze casting aluminum alloy, they will form looseness, split the aluminum matrix, destroy the continuity of the aluminum alloy's structure, cause local stress concentration, and become the crack source and crack extension direction of the squeeze casting aluminum alloy, ultimately reducing the strength and plasticity of the squeeze casting aluminum alloy. For this reason, the aluminum alloy liquid needs to be refined.
[0022] Furthermore, in step S2, the purity of argon is not less than 99.99% to prevent other gases from reacting with elements in the aluminum alloy liquid to form compounds; that is, in order to obtain a better slag removal effect while not causing the aluminum alloy liquid to absorb hydrogen and oxidize or other chemical reactions, it is necessary to select argon with high purity as the carrier gas. It should be particularly pointed out that, compared with conventional nitrogen, argon will not react with the aluminum alloy liquid, and will not produce aluminum nitride mixed in the aluminum alloy liquid, thereby not producing aluminum slag containing aluminum nitride.
[0023] Further, in step S2, the amount of the refining agent is 0.1-0.2% of the weight of the aluminum alloy liquid, and the blowing refining time is 10-20 minutes, so as to ensure the refining and slag removal effect and reduce the production cost; specifically, the amount of the refining agent should not be too little, the temperature of the aluminum alloy liquid during refining should not be too low, and the refining time should not be too short, otherwise the slag removal effect is not ideal. The amount of the refining agent should not be too much, the temperature of the aluminum alloy liquid during refining should not be too high, and the refining time should not be too long, otherwise it will lead to increased oxidation and hydrogen absorption of the aluminum alloy liquid and increase production costs.
[0024] Furthermore, in step S3, the purity of argon is not less than 99.99%, the purity of chlorine is not less than 99.99%, the volume percentage of chlorine in the mixed gas is 10-15%; the flow rate of the mixed gas is 1-2m 3 / min, and the dehydrogenation time is 10-20min. Specifically, the gas in the aluminum alloy liquid is mainly hydrogen, which mainly comes from the reaction between the aluminum alloy liquid and water vapor during the smelting process, including water vapor contained in the air, moisture brought in by the charge and fuel gas, etc. Before degassing, the hydrogen content of the aluminum alloy liquid is usually 0.3-0.5mL / 100gAl. Hydrogen is mainly distributed in the gaps between aluminum atoms in the aluminum alloy liquid in the form of atoms or ions, and a small amount is suspended in the aluminum alloy liquid in the form of molecular bubbles. The solubility of hydrogen in the aluminum alloy liquid gradually decreases with the decrease of temperature. The solubility of hydrogen in solid aluminum is very low. During the solidification process of the aluminum alloy liquid, a large number of hydrogen atoms gradually enrich, nucleate and grow between the crystals, and finally expand to form hydrogen pores. This step S3 can effectively dehydrogenate the aluminum alloy liquid, so that a large amount of hydrogen is precipitated, hydrogen is prevented from being retained in the extrusion casting aluminum alloy to form hydrogen pores, the density of the extrusion casting aluminum alloy is improved, and hydrogen pores are prevented from splitting the aluminum matrix and destroying the organizational continuity of the aluminum alloy; local stress concentration is avoided, and stress is prevented from becoming the crack source and crack extension direction of the extrusion casting aluminum alloy; and the strength and plasticity of the extrusion casting aluminum alloy are finally improved and guaranteed. In addition, chlorine is added to the mixed gas. Due to the active nature of chlorine, it is easy for hydrogen atoms in the aluminum alloy liquid to combine and take away hydrogen in the aluminum alloy liquid, thereby significantly improving the dehydrogenation effect, and the higher the volume percentage of chlorine in the mixed gas, the better the dehydrogenation effect.
[0025] Further, in step S3, the hydrogen in the aluminum alloy liquid is removed by bubbling. On the one hand, the bubbles have a stirring effect on the aluminum alloy liquid when floating, avoiding the dead corner of hydrogen removal in the aluminum alloy liquid in the furnace, and improving the hydrogen removal efficiency of the aluminum alloy liquid. The structure for realizing bubbling can be to install a plurality of porous air-permeable bricks at the bottom of the furnace, and then pass a mixed gas composed of argon and chlorine into the aluminum alloy liquid in the furnace through the air-permeable bricks. After the mixed gas passes through the porous air-permeable bricks, it is decomposed into small and uniform small bubbles. The small bubbles capture the hydrogen in the aluminum alloy liquid during the floating process, and then float out of the aluminum alloy liquid to play a degassing role. A plurality of porous air-permeable bricks are evenly installed, and the air-permeable bricks decompose the mixed gas into small and uniform small bubbles, so that the bubbles are evenly distributed in the aluminum alloy liquid.
[0026] Further, in step S4, during extrusion casting, the pouring temperature of the aluminum alloy liquid is 690-700°C, the mold temperature is 350-400°C, the extrusion pressure ratio is 100-150MPa, the filling speed is 0.5-0.8m / s, and the holding time is 5-10s. Specifically, the density and filling integrity of the extrusion casting aluminum alloy are closely related to the extrusion casting process. If the extrusion casting process combination is unreasonable, the extrusion casting aluminum alloy with dense structure and complete filling will not be obtained; and the extrusion casting aluminum alloy with high strength and high plasticity cannot be obtained. Through a large number of experimental studies, the present invention has found that under the conditions of the aluminum alloy liquid pouring temperature of 690-700°C, the mold temperature of 350-400°C, the extrusion pressure ratio is 100-150MPa, the filling speed is 0.5-0.8m / s, and the holding time is 5-10s, an extrusion casting aluminum alloy with dense structure and complete filling can be obtained.
[0027] Further, in step S5, the solution treatment is to heat the aluminum alloy in an environment of 540-550°C for 2-3h, and then water cool it to room temperature; the aging treatment is to heat the aluminum alloy after the solution treatment in an environment of 160-170°C for 3-4h, and then cool it to room temperature with the furnace. Specifically, solution treatment and aging are important means to further improve the strength of extrusion casting aluminum alloys. The solution treatment and aging temperatures of traditional extrusion casting aluminum alloys are relatively low, which not only leads to low production efficiency of extrusion casting aluminum alloys, but also causes the strength and plasticity of extrusion casting aluminum alloys to fail to achieve the best combination. The present invention has conducted a lot of exploration and research on the solid solution and aging process. The extrusion casting aluminum alloy is heated at 540-550°C for 2-3 hours for solid solution, then put into water and cooled to room temperature, and then the extrusion casting aluminum alloy is heated at 160-170°C for 3-4 hours for aging, and then cooled to room temperature with the furnace. This can not only greatly improve the strength and plasticity of the extrusion casting aluminum alloy, but also greatly shorten the total heating time, which is not only conducive to reducing the energy consumption and production cost during the solid solution aging of the extrusion casting aluminum alloy, but also greatly improve the production efficiency of the extrusion casting aluminum alloy.
[0028] Furthermore, in step S2, the refining agent used for spray refining is a powder with a particle size not greater than 2 mm, composed of the following components in mass percentage: 45.1% ZnCl2, 25.3% K2CO3, 7.6% NaNO3, 11.5% KF, 6.3% K2SO4, and 4.2% Li2SO4.
[0029] Furthermore, the refining agent can be prepared simultaneously when preparing the high-strength and high-plasticity extrusion casting aluminum alloy, or can be prepared in advance and stored for use when preparing the high-strength and high-plasticity extrusion casting aluminum alloy; the preparation of the refining agent includes the following steps:
[0030] A1: Mix the raw materials according to the composition and mass percentage of the refining agent;
[0031] A2: Heat the raw materials to 1150℃ to melt under argon protection, then cool and solidify into refining agent blocks;
[0032] A3: The refining agent block is crushed into powder to obtain the refining agent.
[0033] Furthermore, the purity of the raw material in step A1 is not less than 99.8%; the purity of the argon in step A2 is not less than 99.99%; and the particle size of the refining agent is not greater than 2 mm.
[0034] It should be noted that the slag removal effect of aluminum alloy liquid is not only related to the refining process, but also closely related to the composition and preparation method of the refining agent. Existing commercially available refining agents are mainly made by directly crushing and mixing raw materials such as sodium salt, fluoride salt, chloride salt, hexachloroethane, etc. The components of the refining agent exist independently of each other, which makes the refining agent not only have a high melting point, but also have a low slag removal efficiency. Even if a large amount of refining agent is used, high-purity aluminum alloy liquid cannot be obtained. In order to improve the refining effect, the present invention obtains the refining agent through a large number of experimental explorations and studies. The refining agent is mainly composed of ZnCl2 and K2CO3, and is further combined with a small amount of NaNO3, KF, K2SO4 and Li2SO4. At the same time, the traditional mechanical mixing preparation method is broken through. The raw materials are first heated and melted at 1150°C under the protection of argon gas, and then cooled, solidified and crushed into a powdery refining agent. The melting point of ZnCl2 is about 290°C, the melting point of NaNO3 is 306.8°C, the melting point of K2CO3 is 891°C, the melting point of KF is 858°C, the melting point of K2SO4 is 1069°C, and the melting point of Li2SO4 is 859°C. Although the melting points of K2CO3, KF, K2SO4 and Li2SO4 are relatively high, through melting and solidification crystallization, K2CO3 and KF form a KF·K2CO3 eutectic with a melting point of only 688°C, and K2SO4 and L i2SO4 forms a K2SO4·Li2SO4 eutectic with a melting point of only 716℃, which greatly reduces the melting point of the refining agent and makes it easier to dissolve in the aluminum alloy liquid. ZnCl2 decomposes Cl2, K2CO3 decomposes CO2, and NaNO3 decomposes N2, CO2 and NO gases. A large number of bubbles capture inclusions in the aluminum alloy liquid during the floating process, which plays an efficient role in slag removal. The K2SO4·Li2SO4 eutectic melts into liquid molten salt, which has a good wetting and spheroidizing effect on inclusions such as alumina, promotes the separation of inclusions from the aluminum alloy liquid, and can further improve the slag removal efficiency. In addition, the refining agent does not contain sodium salt and hexachloroethane, but only contains a small amount of fluoride salt, which is more environmentally friendly to use.
[0035] In summary, due to the adoption of the above technical solution, the beneficial effects of the present invention are:
[0036] The present invention can refine the coarse dendritic α-Al grains and the coarse lamellar eutectic Si phase by scientifically designing the composition and preparation process of the extrusion casting aluminum alloy, thereby improving the purity of the aluminum alloy liquid, eliminating the harm of the coarse dendritic α-Al grains, the coarse lamellar eutectic Si phase, the hydrogen pores and the inclusions to the strength and plasticity of the extrusion casting aluminum alloy, thereby greatly improving the strength and plasticity of the extrusion casting aluminum alloy, making the tensile strength of the extrusion casting aluminum alloy not less than 300MPa, the yield strength not less than 270MPa, and the elongation after fracture not less than 8%. Compared with the same type of A356 and ZL101 extrusion casting aluminum alloys, the strength of the extrusion casting aluminum alloy disclosed by the present invention is improved by more than 10%, and the plasticity is improved by more than 50%. In addition, the present invention also greatly shortens the heating time of the extrusion casting aluminum alloy solid solution and aging, which is conducive to reducing the energy consumption during solid solution aging, reducing the production cost, and improving the production efficiency of the extrusion casting aluminum alloy. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] The present invention will now be described by way of example with reference to the accompanying drawings, in which:
[0038] Figure 1 This is the microstructure diagram of the high-strength and high-plasticity extrusion casting aluminum alloy of Example 1.
[0039] Figure 2 This is the microstructure diagram of the high-strength and high-plasticity extrusion casting aluminum alloy of Example 2.
[0040] Figure 3 This is the microstructure diagram of the high-strength and high-plasticity extrusion casting aluminum alloy of Example 3.
[0041] Figure 4 This is the microstructure diagram of the high-strength and high-plasticity extrusion casting aluminum alloy of Example 4. DETAILED DESCRIPTION
[0042] All features disclosed in this specification, or steps in all methods or processes disclosed, except mutually exclusive features and / or steps, can be combined in any manner.
[0043] Any feature disclosed in this specification, unless otherwise stated, can be replaced by other equivalent or alternative features with similar purposes. That is, unless otherwise stated, each feature is only an example of a series of equivalent or similar features.
[0044] Example 1
[0045] like Figure 1As shown, a high-strength and high-plasticity extrusion casting aluminum alloy is composed of the following components in mass percentage: Si (6.9%), Mg (0.41%), Ti (0.09%), Sr (0.02%), Fe accounts for no more than 0.15%, and the rest is Al and other inevitable impurities. Among other impurities, the proportion of a single element is no more than 0.05%, and the total amount is no more than 0.15%.
[0046] A method for preparing an aluminum alloy, for preparing the high-strength and high-plasticity extrusion casting aluminum alloy disclosed in this embodiment 1, comprises the following steps:
[0047] S1: melting the aluminum alloy into a liquid aluminum alloy in a furnace according to the composition and mass percentage of the aluminum alloy, and raising the temperature of the aluminum alloy liquid to 710° C.;
[0048] S2: using argon gas with a purity of 99.99% as a refining agent with a carrier current accounting for 0.15% of the weight of the aluminum alloy liquid, spraying and refining the aluminum alloy liquid for 16 minutes to remove slag, and then removing the scum on the surface of the aluminum alloy liquid;
[0049] S3: The bottom of the furnace is evenly distributed with air-permeable bricks, and bubbles are blown into the aluminum alloy liquid in the furnace through the air-permeable bricks. A mixed gas consisting of argon with a purity of 99.99% and chlorine with a purity of 99.99% is introduced into the aluminum alloy liquid for 15 minutes for dehydrogenation treatment. The volume percentage of chlorine in the mixed gas is 12%, and the flow rate of the mixed gas is 1.6m 3 / min;
[0050] S4: extruding the aluminum alloy liquid into an aluminum alloy under the conditions of an aluminum alloy liquid pouring temperature of 695° C., a mold temperature of 380° C., an extrusion pressure of 120 MPa, a filling speed of 0.7 m / s, and a holding time of 6 s;
[0051] S5: The aluminum alloy is heated at 545°C for 2.5 hours for solution treatment, then placed in water and cooled to room temperature, then heated at 165°C for 3.5 hours for aging treatment, and then cooled to room temperature with the furnace to obtain the high-strength and high-plasticity extrusion casting aluminum alloy.
[0052] Example 2
[0053] like Figure 2 As shown, a high-strength and high-plasticity extrusion casting aluminum alloy is composed of the following components in mass percentage: Si (7.2%), Mg (0.39%), Ti (0.11%), Sr (0.017%), Fe accounts for no more than 0.15%, and the rest is Al and other inevitable impurities. Among other impurities, the proportion of a single element is no more than 0.05%, and the total amount is no more than 0.15%.
[0054] A method for preparing an aluminum alloy, for preparing the high-strength and high-plasticity aluminum alloy disclosed in this embodiment 2, comprises the following steps:
[0055] S1: melting the aluminum alloy into a liquid aluminum alloy in a furnace according to the composition and mass percentage of the aluminum alloy, and raising the temperature of the aluminum alloy liquid to 720° C.;
[0056] S2: using argon gas with a purity of 99.99% as a carrier and a refining agent accounting for 0.1% of the weight of the aluminum alloy liquid, spraying and refining the aluminum alloy liquid for 10 minutes to remove slag, and then removing the slag on the surface of the aluminum alloy liquid;
[0057] S3: The bottom of the furnace is evenly distributed with air-permeable bricks, and bubbles are blown into the aluminum alloy liquid in the furnace through the air-permeable bricks. A mixed gas consisting of argon with a purity of 99.99% and chlorine with a purity of 99.99% is introduced into the aluminum alloy liquid for 20 minutes for dehydrogenation treatment. The volume percentage of chlorine in the mixed gas is 15%, and the flow rate of the mixed gas is 2m 3 / min;
[0058] S4: extruding the aluminum alloy liquid into an aluminum alloy under the conditions of an aluminum alloy liquid pouring temperature of 695° C., a mold temperature of 360° C., an extrusion pressure of 140 MPa, a filling speed of 0.6 m / s, and a holding time of 8 s;
[0059] S5: The aluminum alloy is heated at 540° C. for 3 hours for solution treatment, then placed in water and cooled to room temperature, then heated at 170° C. for 3 hours for aging treatment, and then cooled to room temperature with the furnace to obtain the high-strength and high-plasticity extrusion casting aluminum alloy.
[0060] Example 3
[0061] like Figure 3 As shown, a high-strength and high-plasticity extrusion casting aluminum alloy is composed of the following components in mass percentage: Si (7.5%), Mg (0.25%), Ti (0.12%), Sr (0.01%), Fe accounts for no more than 0.15%, and the rest is Al and other inevitable impurities. Among other impurities, the proportion of a single element is no more than 0.05%, and the total amount is no more than 0.15%.
[0062] A method for preparing an aluminum alloy, for preparing the high-strength and high-plasticity aluminum alloy disclosed in this embodiment 3, comprises the following steps:
[0063] S1: melting the aluminum alloy into a liquid aluminum alloy in a furnace according to the composition and mass percentage of the aluminum alloy, and raising the temperature of the aluminum alloy liquid to 730° C.;
[0064] S2: using argon gas with a purity of 99.99% as a carrier and a refining agent accounting for 0.2% of the weight of the aluminum alloy liquid, spraying and refining the aluminum alloy liquid for 20 minutes to remove slag, and then removing the scum on the surface of the aluminum alloy liquid;
[0065] S3: The bottom of the furnace is evenly distributed with air-permeable bricks. Bubbles are introduced into the aluminum alloy liquid in the furnace through the air-permeable bricks. A mixed gas consisting of argon with a purity of 99.99% and chlorine with a purity of 99.99% is introduced into the aluminum alloy liquid for 10 minutes for dehydrogenation treatment. The volume percentage of chlorine in the mixed gas is 10%, and the flow rate of the mixed gas is 1m 3 / min;
[0066] S4: extruding the aluminum alloy liquid into an aluminum alloy under the conditions of an aluminum alloy liquid pouring temperature of 700° C., a mold temperature of 350° C., an extrusion pressure of 150 MPa, a filling speed of 0.5 m / s, and a holding time of 10 s;
[0067] S5: The aluminum alloy is heated at 540° C. for 3 hours for solution treatment, then placed in water and cooled to room temperature, then heated at 160° C. for 4 hours for aging treatment, and then cooled to room temperature with the furnace to obtain the high-strength and high-plasticity extrusion casting aluminum alloy.
[0068] Example 4
[0069] like Figure 3 As shown, a high-strength and high-plasticity extrusion casting aluminum alloy is composed of the following components in mass percentage: Si (6.5%), Mg (0.45%), Ti (0.08%), Sr (0.03%), Fe accounts for no more than 0.15%, and the rest is Al and other inevitable impurities. Among other impurities, the proportion of a single element is no more than 0.05%, and the total amount is no more than 0.15%.
[0070] A method for preparing an aluminum alloy, for preparing the high-strength and high-plasticity aluminum alloy disclosed in Example 4, comprising the following steps:
[0071] S1: melting the aluminum alloy into liquid aluminum in a furnace according to the composition and mass percentage of the aluminum alloy, and raising the temperature of the aluminum alloy liquid to 700°C;
[0072] S2: using argon gas with a purity of 99.99% as a carrier and a refining agent accounting for 0.1% of the weight of the aluminum alloy liquid, spraying and refining the aluminum alloy liquid for 10 minutes to remove slag, and then removing the slag on the surface of the aluminum alloy liquid;
[0073] S3: The bottom of the furnace is evenly distributed with air-permeable bricks, and bubbles are blown into the aluminum alloy liquid in the furnace through the air-permeable bricks. A mixed gas consisting of argon with a purity of 99.99% and chlorine with a purity of 99.99% is introduced into the aluminum alloy liquid for 20 minutes for dehydrogenation treatment. The volume percentage of chlorine in the mixed gas is 15%, and the flow rate of the mixed gas is 2m 3 / min;
[0074] S4: extruding the aluminum alloy liquid into an aluminum alloy under the conditions of an aluminum alloy liquid pouring temperature of 690° C., a mold temperature of 400° C., an extrusion pressure of 100 MPa, a filling speed of 0.8 m / s, and a holding time of 5 s;
[0075] S5: The aluminum alloy is heated at 550° C. for 2 hours for solution treatment, then placed in water and cooled to room temperature, then heated at 170° C. for 3 hours for aging treatment, and then cooled to room temperature with the furnace to obtain the high-strength and high-plasticity extrusion casting aluminum alloy.
[0076] Example 5
[0077] Any one of Examples 1-4 proposes a powdered refining agent with a particle size not greater than 2 mm, which is used as the refining agent in any one of Examples 1-4, and is composed of the following components in mass percentage: 45.1% ZnCl2, 25.3% K2CO3, 7.6% NaNO3, 11.5% KF, 6.3% K2SO4, and 4.2% Li2SO4. The method for preparing the refining agent is as follows: comprising the following steps:
[0078] A1: Select ZnCl2, K2CO3, NaNO3, KF, K2SO4, Li2SO4 with a purity of 99.8% as raw materials and mix them according to the composition and mass percentage of the refining agent;
[0079] A2: The raw materials are heated and melted at 1150°C under the protection of argon gas with a purity of 99.99%, and then cooled and solidified into a refining agent block;
[0080] A3: The refining agent block is crushed into powder with a particle size of 2 mm to obtain the refining agent.
[0081] Example 6
[0082] This embodiment provides some comparative examples that can be compared with the contents disclosed in Examples 1-5; the details are as follows:
[0083] Comparative Example 1 provides an extrusion casting aluminum alloy, which is specifically as follows.
[0084] The preparation process parameters of the aluminum alloy are the same as those in Example 1, except that no aluminum-titanium alloy is added to the aluminum alloy, that is, the aluminum alloy disclosed in this comparative example 1 does not contain Ti; specifically, the aluminum alloy in this comparative example is composed of the following components in mass percentage: Si (6.9%), Mg (0.41%), Sr (0.02%), Fe≤0.15%, and the rest are Al and other inevitable impurities, and the other impurities are individually ≤0.05% and the total amount is ≤0.15%.
[0085] Comparative Example 2 provides an extrusion casting aluminum alloy, which is specifically as follows.
[0086] The component composition of the aluminum alloy and its preparation process parameters are the same as those in Example 2, except that in the preparation method of the aluminum alloy in this comparative example 2, the refining agent used in step S2 is a currently commonly used commercially available refining agent, that is, the refining agent is composed of the following components in mass percentage: 26.1% NaCl, 10.6% Na2S iF6, 17.1% Na2SO4, 6.9% CaF2, 9.3% C6Cl6, 14.3% Na2S2O3 and 15.7% NaF, and the preparation method of the refining agent is to directly crush the raw materials into powders with a particle size not greater than 2 mm and then mix them.
[0087] Comparative Example 3 provides an extrusion casting aluminum alloy, as follows.
[0088] The component composition of the aluminum alloy and its preparation process parameters are the same as those in Example 3. The difference is that in the preparation method of the aluminum alloy in this comparative example 3, step S3 does not pass a mixed gas composed of argon and chlorine into the aluminum alloy liquid in the furnace through a breathable brick for dehydrogenation treatment.
[0089] Comparative Example 4 provides an extrusion casting aluminum alloy, as follows.
[0090] The component composition of the aluminum alloy and its preparation process parameters are the same as those in Example 4, except that in the preparation method of the aluminum alloy in this comparative example 3, the aging process of the aluminum alloy in step S5 is heating at 140° C. for 8 hours.
[0091] The contents disclosed in Examples 1-5 are compared and analyzed with the comparative examples disclosed in Example 6. Specific examples 1-4 are as follows.
[0092] Verification Example 1
[0093] The melting points of the refining agent disclosed in Example 5 (refining agent-Example 5) and the refining agent used in Comparative Example 2 (refining agent-Comparative Example 2) were respectively measured using an OXFORD-DSC500 differential scanning calorimeter. The results are shown in Table 1.
[0094] Table 1: Comparison of melting points of refining agents
[0095] Refining agent - Example 5 Refining agent-Comparative Example 2 Melting start temperature / ℃ 290 564 Melting end temperature / ℃ 716 1249
[0096] It can be seen from Table 1 that the melting start temperature of the refining agent-Example 5 is 290°C, and the melting end temperature is only 716°C. The melting start temperature of the refining agent-Comparative Example 2 is 564°C, and the melting end temperature is 1249°C. By comparison, it can be seen that the refining agent developed by the present invention has a lower melting start temperature and melting end temperature, indicating that the refining agent developed by the present invention is easier to dissolve in the aluminum alloy liquid, which is beneficial to improving the slag removal effect.
[0097] Verification Example 2
[0098] The hydrogen content and slag content of the aluminum alloy liquid before extrusion casting of Examples 1-4 and Comparative Examples 1-4 were tested on-site using a HDA-V hydrogen meter and an Analyze PoDFA slag meter. The results are shown in Table 2.
[0099] Table 2: Comparison of hydrogen content and slag content in aluminum alloy liquid
[0100] Hydrogen content / (ml / 100gAl) <![CDATA[Sludge content / (mm 2 / kg)]]> Example 1 0.085 0.065 Example 2 0.092 0.078 Example 3 0.079 0.071 Example 4 0.089 0.073 Comparative Example 1 0.084 0.067 Comparative Example 2 0.093 0.152 Comparative Example 3 0.168 0.079 Comparative Example 4 0.091 0.074
[0101] It can be seen from Table 2 that the hydrogen content of the aluminum alloy liquid in Examples 1-4 is less than 0.1 ml / 100 gAl, and the slag content is less than 0.08 mm 2 / kgAl. However, since Comparative Example 2 uses a traditional commercially available refining agent for in-furnace spray refining, and Comparative Example 3 does not pass argon and chlorine through the furnace bottom air bricks for dehydrogenation, the gas slag content of the aluminum alloy liquid before extrusion casting in Comparative Example 2 and Comparative Example 3 is higher than the gas slag content of the aluminum alloy liquid before extrusion casting in the embodiment. By comparison, it can be seen that the cleanliness of the extrusion casting aluminum alloy can be greatly improved by the method of the present invention.
[0102] Verification Example 3
[0103] Samples were taken from the high-strength and high-plasticity extrusion cast aluminum alloys obtained in Examples 1-4 and the extrusion cast aluminum alloys obtained in Comparative Examples 1-4, and stretched at room temperature on an electronic tensile testing machine at a stretching rate of 2 mm / min. The tensile strength, yield strength and elongation after fracture of the extrusion cast aluminum alloys were tested. The results are shown in Table 3.
[0104] Table 3: Room temperature tensile mechanical properties of squeeze cast aluminum alloys
[0105]
[0106]
[0107] It can be seen from Table 3 that the tensile strength of the aluminum alloys obtained in Examples 1-4 is not less than 300MPa, the yield strength is not less than 270MPa, and the elongation after fracture is not less than 8%. The aluminum alloy disclosed in Comparative Example 1 does not add aluminum-titanium alloy for grain refinement treatment, the aluminum alloy disclosed in Comparative Example 2 uses conventional commercially available refining agents for slag removal, the aluminum alloy disclosed in Comparative Example 3 does not use furnace bottom air bricks for hydrogen removal, and the aluminum alloy disclosed in Comparative Example 4 uses conventional aging processes, resulting in low strength and plasticity of the extrusion casting aluminum alloy. By comparison, it can be seen that the present invention can greatly improve the strength and plasticity of the extrusion casting aluminum alloy by scientifically designing the composition and preparation process of the die-casting aluminum alloy, refining the coarse dendritic α-Al grains and the coarse lamellar eutectic Si phase, improving the purity of the aluminum alloy liquid, and eliminating the harm of the coarse dendritic α-Al grains, the coarse lamellar eutectic Si phase, the hydrogen pores and the inclusions to the strength and plasticity of the extrusion casting aluminum alloy.
[0108] Verification Example 4
[0109] Samples were taken from the aluminum alloy obtained in Examples 1-4, and after grinding, polishing and etching, they were observed on a LEIKA-1800 metallographic microscope. Figure 1 This is a microstructure diagram of the aluminum alloy in Example 1 magnified 100 times. Figure 2 This is a microstructure diagram of the aluminum alloy in Example 2 magnified 100 times. Figure 3 This is a microstructure diagram of the aluminum alloy in Example 3 magnified 100 times. Figure 4 The microstructure of the aluminum alloy in Example 4 is magnified 100 times. Figure 1-4 It can be seen that the α-Al grains and eutectic Si phase of the squeeze casting aluminum alloy of the present invention are fine, and there are no coarse dendritic α-Al grains and coarse lamellar eutectic Si phases.
[0110] The present invention is not limited to the above-mentioned specific embodiments, but extends to any new features or any new combination disclosed in this specification, as well as any new method or process steps or any new combination disclosed.
Claims
1. A method for preparing a high-strength and high-plasticity extrusion casting aluminum alloy, characterized in that: The aluminum alloy is composed of the following components in mass percentage: Si (6.5-7.5%), Mg (0.25-0.45%), Ti (0.08-0.12%), Sr (0.01-0.03%), Fe not exceeding 0.15%, and the rest being Al and other inevitable impurities; among other impurities, a single element is ≤0.05%, and the total amount is ≤0.15%; the preparation method comprises the following steps: S1: melting and preparing aluminum alloy liquid according to the composition and mass percentage of the aluminum alloy, and raising the temperature of the aluminum alloy liquid to 700-730°C; S2: Using argon as a carrier and a current refining agent, the aluminum alloy liquid is subjected to a slag removal treatment by a spray refining method, and then the slag on the surface of the aluminum alloy liquid is removed; S3: introducing a mixed gas consisting of argon and chlorine into the aluminum alloy liquid in a bubbling manner to perform a dehydrogenation treatment; S4: forming an aluminum alloy by extrusion casting the aluminum alloy liquid; S5: subjecting the aluminum alloy to solid solution and aging treatment to obtain an extrusion casting aluminum alloy with high strength and high plasticity; the aging treatment is to heat the aluminum alloy after solid solution treatment in an environment of 160-170°C for 3-4h, and then cool it to room temperature with the furnace; In step S2, the amount of the refining agent is 0.1-0.2% of the weight of the aluminum alloy liquid, and the blowing refining time is 10-20min; the refining agent is a powder with a particle size not greater than 2mm, and is composed of the following components in mass percentage: 45.1% ZnCl2, 25.3% K2CO3, 7.6% NaNO3, 11.5% KF, 6.3% K2SO4, and 4.2% Li2SO4; the preparation of the refining agent includes the following steps: A1: mixing the raw materials according to the composition and mass percentage of the refining agent; A2: heating and melting the raw materials under argon protection, and then cooling and solidifying them into a refining agent block; A3: crushing the refining agent block into powder to obtain the refining agent; In step S3, the purity of argon is not less than 99.99%, the purity of chlorine is not less than 99.99%, the volume percentage of chlorine in the mixed gas is 10-15%; the flow rate of the mixed gas is 1-2m 3 / min, and the dehydrogenation time is 10-20min.
2. The preparation method according to claim 1, characterized in that: In step S2, the purity of argon gas is not less than 99.99%.
3. The preparation method according to claim 1, characterized in that: In step S4, during extrusion casting, the pouring temperature of the aluminum alloy liquid is 690-700°C, the mold temperature is 350-400°C, the extrusion pressure ratio is 100-150MPa, the filling speed is 0.5-0.8m / s, and the holding time is 5-10s.
4. The preparation method according to claim 1, characterized in that: In step S5, the solution treatment is to heat the aluminum alloy in an environment of 540-550° C. for 2-3 hours and then water-cool it to room temperature.
5. The preparation method according to claim 1, characterized in that: The purity of the raw material in step A1 is not less than 99.8%; the purity of the argon gas in step A2 is not less than 99.99%.
Citation Information
Cited By
Preparation method of cast aluminum alloy
CN121653475A
A method of producing a cast aluminium alloy