A method for recycling lithium from waste batteries based on alkaline substances
By using an alkaline substance-assisted lithium extraction method in lithium-ion battery recycling to destroy the solid electrolyte membrane, the problem of low recycling efficiency of lithium-ion batteries in the existing technology is solved, and efficient and low-cost lithium ion extraction and reuse are achieved. .
Patent Information
- Application Number
- CN202311866859.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-28
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2043-12-28
AI Technical Summary
Existing lithium-ion battery recycling methods require long reaction times and a large amount of lithium extraction reagents, resulting in high time and economic costs and low efficiency.
Using a lithium extraction method assisted by alkaline substances, by adding dissolved organic solvents containing aromatic hydrocarbons and alkaline substances into the lithium extraction reagent, the solid electrolyte membrane on the surface of the graphite is destroyed, promoting the leaching and migration of lithium ions, and optimizing the leaching conditions to shorten the lithium extraction time and improve efficiency.
It significantly shortens the extraction time of lithium ions, improves the efficiency of lithium extraction, reduces energy consumption and costs, and avoids side reactions by optimizing the types and contents of alkaline substances and aromatic hydrocarbon compounds, achieving efficient recovery and regeneration of lithium. use.
Smart Images

Figure CN117821757B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of waste battery recycling, and more specifically, relates to a waste battery lithium recycling method based on alkaline substances. Background Art
[0002] Lithium-ion battery is a secondary battery, with the negative electrode made of graphite and other materials, and the positive electrode made of lithium iron phosphate, lithium cobalt oxide, lithium titanate, etc. Lithium-ion batteries are widely used in modern digital products such as mobile phones and laptops. At the same time, with the rapid development of the new energy vehicle industry, the production of lithium-ion batteries has increased rapidly, and a large number of waste lithium-ion batteries will inevitably be generated. Waste lithium-ion batteries contain a large amount of lithium. If the efficient circulation of lithium metal can be achieved, it can not only avoid environmental pollution, but also alleviate the dilemma of lithium resource shortage in my country to a large extent.
[0003] In the prior art, CN113061726B discloses a method for safely and efficiently recycling lithium from waste batteries, which is to obtain a lithium-rich solution by directly immersing the negative electrode material in an organic reagent of polycyclic aromatic hydrocarbons. Since the surface of the waste graphite material is coated with a dense solid electrolyte membrane (SEI), the electron exchange reaction between the waste graphite and the lithium extraction reagent is blocked, so that the direct immersion method requires a long reaction time and a large amount of lithium extraction reagent to extract active lithium, which greatly increases the time cost and economic cost. Summary of the invention
[0004] In view of the defects of the prior art, the purpose of the present invention is to provide a method for recycling lithium from waste batteries assisted by alkaline substances, aiming to solve the problems of long reaction time and low efficiency of the existing lithium recycling methods.
[0005] To achieve the above object, the present invention provides a method for recycling lithium from waste batteries assisted by alkaline substances, the method comprising the following steps:
[0006] S1 uses a lithium extraction reagent to leach the negative electrode material of the waste lithium-ion battery to obtain a solid-liquid mixture, wherein the lithium extraction reagent is an organic solvent in which aromatic hydrocarbon compounds and alkaline substances are dissolved, and the alkaline substances destroy the solid electrolyte membrane on the surface of the graphite during operation to accelerate the leaching of lithium;
[0007] S2 separates the solid-liquid mixture obtained in step S1 to obtain a lithium-rich solution, and then achieves efficient recovery of lithium from waste lithium-ion batteries with the assistance of alkaline substances.
[0008] As further preferred, the alkaline substance is one or more of sodium hydroxide, potassium hydroxide and ammonia water, and the mass fraction of the alkaline substance in the lithium extraction reagent is 0.01% to 1%.
[0009] As further preferred, the molar concentration of the aromatic hydrocarbon compound in the lithium extraction reagent is 0.2 mol / L to 3 mol / L.
[0010] As a further preference, the aromatic hydrocarbon compound is one or more of benzene, naphthalene, phenanthrene, anthracene, tetracene, pyrene and perylene, and the aromatic hydrocarbon compound includes at least one substituent, and the substituent is an alkyl group, a hydroxyl group, a nitro group, a halogen atom, an amino group, a carboxyl group, an aldehyde group, a carbonyl group, a sulfonic acid group, a disulfide bond, an ester bond or an ether bond.
[0011] As a further preference, the organic solvent is one or more of ethers, esters and aromatics, the ethers include one or more of tetrahydrofuran, ethylene glycol dimethyl ether, 1,3-dioxolane, diethanol dimethyl ether, triethanol dimethyl ether and tetraethanol dimethyl ether; the esters are one or more of ethylene carbonate, propylene carbonate, diethyl carbonate and vinylene carbonate; the aromatics are benzene and / or toluene.
[0012] As further preferred, in step S1, the leaching time is 10 min to 10 h, and the leaching temperature is -10°C to 100°C.
[0013] As further preferred, in step S1, during leaching, the mass ratio of the active substance in the negative electrode material to the lithium extraction reagent is 1:1 to 1:5.
[0014] As a further preferred embodiment, the method for obtaining the negative electrode material is: charging the waste lithium-ion battery to a fully charged state, and then disassembling the battery in a safe environment with a relative humidity of less than 20% to obtain the negative electrode material.
[0015] As a further preferred embodiment, the method for efficiently recovering lithium from waste lithium-ion batteries also includes step S3, specifically: soaking the material to be treated with the lithium-rich solution, thereby lithiation of the material to be treated to achieve lithium recycling.
[0016] As a further preference, the material to be treated is a positive electrode of a lithium-ion battery, and the positive electrode of the lithium-ion battery is mixed with a lithium extraction solution and subjected to a hydrothermal reaction, and then dried and washed to obtain a pre-lithiated positive electrode.
[0017] In general, the above technical solution conceived by the present invention has the following beneficial effects compared with the prior art:
[0018] 1. The present invention adds alkaline substances to the lithium extraction reagent to destroy the dense solid electrolyte membrane on the graphite surface, expose the active lithium surface, promote electron exchange at the interface, make lithium ions more likely to react with aromatic compounds, thereby optimizing the migration rate at the lithium ion interface and the lithium extraction speed, greatly shortening the lithium extraction time and improving the lithium extraction efficiency;
[0019] 2. In particular, the present invention optimizes the type, content and soaking time of the alkaline substance, so as to ensure that the added alkaline substance fully destroys the solid electrolyte membrane, effectively shortens the lithium extraction time and improves the lithium extraction efficiency, and avoids the reaction of excessive alkaline substances with lithiated graphite, causing side reactions and reducing the lithium extraction yield. Through fine control of the type, addition amount and soaking time of the alkaline substance, the lithium extraction time can be shortened while avoiding the reduction of the lithium extraction yield caused by excessive alkaline substances;
[0020] 3. In addition, the present invention also optimizes the types and contents of aromatic hydrocarbon compounds and organic solvents, so that active lithium can be extracted in a shorter time, maximizing the effect of lithium extraction reagents and avoiding waste of lithium extraction reagents and extension of lithium extraction time;
[0021] 4. At the same time, the present invention can complete lithium extraction at lower energy consumption and cost by optimizing the leaching conditions;
[0022] 5. In addition, the present invention also proposes to soak the material to be treated in a lithium-rich solution, thereby enabling the recovery of lithium to be quickly and conveniently reused. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The present invention provides a flowchart of lithium recovery from waste batteries based on the assistance of alkaline substances. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings and embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0025] like Figure 1 As shown, the present invention provides a method for recycling lithium from waste batteries based on the assistance of alkaline substances, the method comprising the following steps:
[0026] S1 uses a lithium extraction reagent to leach the negative electrode material of the waste lithium-ion battery to obtain a solid-liquid mixture. The lithium extraction reagent is an organic solvent dissolved with aromatic compounds and alkaline substances. When working, the alkaline substance destroys the solid electrolyte membrane on the graphite surface, exposing the active surface of the graphite, promoting electron exchange at the interface, making it easier for lithium ions to react with aromatic compounds, thereby accelerating the leaching of lithium and shortening the reaction time;
[0027] S2: separating the solid-liquid mixture obtained in step S1 to obtain a lithium-rich solution, thereby efficiently recovering lithium from waste lithium-ion batteries with the assistance of alkaline substances;
[0028] S3 soaks the material to be treated with a lithium-rich solution, thereby lithiation the material to be treated to achieve lithium recycling.
[0029] Furthermore, in a safe environment with a relative humidity of less than 20% (preferably less than 10%), the waste lithium-ion batteries are fully charged and then disassembled to separate the negative electrode materials and the positive electrode materials. The negative electrode materials are selected from lithium metal negative electrodes, including carbon-based active substances (selected from one or more of natural graphite, artificial graphite, soft carbon, hard carbon, and mesophase carbon microspheres), silicon-based active substances (silicon-based active substances are selected from one or more of silicon element, silicon alloy, and silicon oxide), and the positive electrode materials are selected from lithium iron phosphate in different lithium-containing states, layered ternary materials, lithium manganese oxide, lithium cobalt oxide, lithium-rich manganese materials, etc.
[0030] Further, the amount of alkaline substance added in the present invention is relatively small, and the acidity and alkalinity of the lithium extraction reagent will not be changed too much. This is mainly because the present invention uses alkaline substances to destroy the protective film SEI and accelerate the reaction of aromatic compounds with active lithium, while the prior art usually uses strong alkaline substances to dissolve all substances non-selectively so that active lithium is dissolved. Therefore, the alkaline substance in the present invention is one or more of sodium hydroxide, potassium hydroxide and ammonia water, and the mass fraction of the alkaline substance in the lithium extraction reagent is 0.01% to 1%. The alkaline substance here is mainly to destroy SEI. In theory, it does not need too high a content. Within a given range, the rate and degree of destruction of SEI increase with the increase of the alkaline substance content, which is conducive to completing the lithium extraction process faster and shortening the production time. When the alkaline substance content is too low, SEI cannot be effectively destroyed, and the effect of improving the lithium extraction rate is not obvious. When the content of alkaline substances is too high, the remaining lithium after destroying SEI will react with lithiated graphite, reducing the lithium extraction yield. At the same time, it will also cause the alkalinity of lithium extraction reagents to increase, which will cause corrosion or damage to the pre-lithiation materials in the subsequent pre-lithiation process based on this solution, and will also lead to increased production costs and potential corrosion and environmental hazards during the treatment process. In addition, the introduction of a large amount of alkaline substances such as sodium hydroxide and potassium hydroxide may lead to impurity cation contamination brought by sodium ions and potassium ions, so that the lithium-rich solution obtained after solid-liquid separation contains a large amount of other impurity ions and cannot be directly used for lithiation.
[0031] Further, the aromatic compound is one or more of benzene, naphthalene, phenanthrene, anthracene, tetracene, pyrene and perylene, and the aromatic compound includes at least one substituent, and the substituent is an alkyl, hydroxyl, nitro, halogen atom, amino, carboxyl, aldehyde, carbonyl, sulfonic acid, disulfide bond, ester bond or ether bond. The molar concentration of the aromatic compound in the lithium extraction reagent is 0.2mol / L to 3mol / L. Within a given range, the lithium extraction time is shortened as the content of the aromatic compound increases, and the maximum lithium extraction degree increases as the content of the aromatic compound increases. When the content of the aromatic compound is lower than the content of active lithium in the material, it cannot be guaranteed that all active lithium reacts and complexes with the aromatic compound, and the maximum lithium extraction degree is reduced. When the content of aromatic hydrocarbons is too large, the lithium extraction efficiency will not continue to increase after the reaction reaches equilibrium, but will cause the viscosity of the lithium extraction solution to increase, which is not conducive to practical operation. On the other hand, the maximum content of the aromatic compound is also limited by the maximum solubility of the substance in the organic solvent, so the above molar concentration is the result of comprehensive consideration.
[0032] Furthermore, the organic solvent is one or more of ethers, esters and aromatics, the ethers include one or more of tetrahydrofuran, ethylene glycol dimethyl ether, 1,3-dioxolane, diethanol dimethyl ether, triethanol dimethyl ether and tetraethanol dimethyl ether; the esters are one or more of ethylene carbonate, propylene carbonate, diethyl carbonate and vinylene carbonate; the aromatics are benzene and / or toluene.
[0033] Further, within a certain range, the degree and rate of extraction of active lithium are related to the amount of lithium extraction reagent added (at a certain concentration of aromatic compounds, the more lithium extraction reagents there are, the more aromatic compounds that can participate in the reaction). When the amount of lithium extraction reagent added is insufficient, some lithium in the active substance cannot be combined with aromatic hydrocarbon substances, and the active lithium cannot be completely extracted, resulting in a low degree of final active lithium extraction. On the contrary, when the lithium extraction reagent is much higher than the active substance, the lithium extraction speed and degree no longer increase significantly, which will cause a waste of lithium extraction reagents and is not conducive to large-scale production. Therefore, in step S1, the mass ratio of the mass of the active substance in the negative electrode material to the mass of the lithium extraction reagent during leaching is 1:1 to 1:5, wherein the mass of the active substance in the negative electrode material is the total mass of the negative electrode material minus the mass of copper foil, binder and conductive agent. The leaching time is 10min to 10h, and the leaching temperature is -10℃ to 100℃. If the time is too short, the active lithium and aromatic compounds will not have enough time to react, resulting in unsatisfactory lithium extraction results. If the leaching time is too long, the production time cost will increase, and too long a time will not lead to further improvement of the lithium extraction level. The lithium extraction reaction involves a thermodynamic process. A higher temperature will promote the forward reaction, but too high a temperature will cause solvent volatilization and potential side reactions. If the temperature is too low, the reaction will be slow, and some solvents may solidify and fail to function.
[0034] Furthermore, the lithium-rich solution can be applied to the pre-lithiation of the positive electrode of a lithium-ion battery, that is, the material to be treated is the positive electrode of a lithium-ion battery, and the pre-lithiation method includes but is not limited to immersing in the lithium-rich solution, spraying the lithium-rich solution on the surface of the lithium-ion battery positive electrode material, mixing the lithium-ion battery positive electrode material with the lithium-rich solution, performing a hydrothermal reaction, and then drying and washing to obtain the pre-lithiation positive electrode.
[0035] The technical solution provided by the present invention is further described below based on specific embodiments.
[0036] Example 1
[0037] (a) dismantling the waste lithium-ion battery in a drying room with a relative humidity of 5%, taking out the dismantled negative electrode sheet and positive electrode sheet, and cutting them into suitable sizes; then preparing a lithium extraction reagent, dissolving 1 mol of biphenyl reagent in 1 L of diethylene glycol dimethyl ether, and then adding 1% by mass of sodium hydroxide;
[0038] (b) immersing the negative electrode material in a lithium extraction reagent, wherein the mass ratio of the active material in the negative electrode material to the lithium extraction reagent is 1:2, leaching at 40° C. for 30 min, and then filtering and washing to obtain a lithium-rich solution;
[0039] (c) Immersing the waste positive electrode material in the above lithium-rich solution, stirring and reacting for 5 hours at a temperature of 50° C. After the reaction is completed, washing with diethylene glycol dimethyl ether and drying to obtain a regenerated positive electrode material.
[0040] Example 2
[0041] (a) dismantling the waste lithium-ion battery in a dry room with a relative humidity of 5%, taking out the dismantled negative electrode sheet and positive electrode sheet, and cutting them into suitable sizes; then preparing a lithium extraction reagent, dissolving 0.2 mol of tetracene reagent in 1 L of tetrahydrofuran, and then adding 0.05% by mass of potassium hydroxide;
[0042] (b) immersing the negative electrode material in a lithium extraction reagent, wherein the mass ratio of the active material in the negative electrode material to the lithium extraction reagent is 1:1, leaching for 20 min at -10°C, and then filtering and washing to obtain a lithium-rich solution;
[0043] (c) Immersing the waste positive electrode material in the above lithium-rich solution, stirring and reacting for 5 hours at a temperature of 50° C. After the reaction is completed, washing with diethylene glycol dimethyl ether and drying to obtain a regenerated positive electrode material.
[0044] Example 3
[0045] (a) dismantling the waste lithium-ion battery in a drying room with a relative humidity of 5%, taking out the dismantled negative electrode sheet and positive electrode sheet, and cutting them into suitable sizes; then preparing a lithium extraction reagent, dissolving 3 mol of naphthalene reagent in 1 L of 1,3-dioxolane, and then adding 0.06% by mass of ammonia water;
[0046] (b) immersing the negative electrode material in a lithium extraction reagent, wherein the mass ratio of the active material in the negative electrode material to the lithium extraction reagent is 1:5, leaching at 100° C. for 10 h, and then filtering and washing to obtain a lithium-rich solution;
[0047] (c) Immersing the waste positive electrode material in the above lithium-rich solution, stirring and reacting for 5 hours at a temperature of 50° C. After the reaction is completed, washing with diethylene glycol dimethyl ether and drying to obtain a regenerated positive electrode material.
[0048] Example 4
[0049] (a) dismantling the waste lithium-ion battery in a dry room with a relative humidity of 5%, taking out the dismantled negative electrode sheet and positive electrode sheet, and cutting them into suitable sizes; then preparing a lithium extraction reagent, dissolving 1.5 mol of phenanthrene reagent in 1 L of triethanol dimethyl ether, and then adding 0.1% by mass of ammonia water;
[0050] (b) immersing the negative electrode material in a lithium extraction reagent, wherein the mass ratio of the active material in the negative electrode material to the lithium extraction reagent is 1:3, leaching at 50° C. for 3 h, and then filtering and washing to obtain a lithium-rich solution;
[0051] (c) Immersing the waste positive electrode material in the above lithium-rich solution, stirring and reacting for 5 hours at a temperature of 50° C. After the reaction is completed, washing with diethylene glycol dimethyl ether and drying to obtain a regenerated positive electrode material.
[0052] Example 5
[0053] (a) dismantling the waste lithium-ion battery in a dry room with a relative humidity of 5%, taking out the dismantled negative electrode sheet and positive electrode sheet, and cutting them into suitable sizes; then preparing a lithium extraction reagent, dissolving 2 mol of 2-methylbiphenyl reagent in 1 L of vinylene carbonate, and then adding 0.5% by mass of ammonia water;
[0054] (b) immersing the negative electrode material in a lithium extraction reagent, wherein the mass ratio of the active material in the negative electrode material to the lithium extraction reagent is 1:2, leaching at 70° C. for 3 h, and then filtering and washing to obtain a lithium-rich solution;
[0055] (c) Immersing the waste positive electrode material in the above lithium-rich solution, stirring and reacting for 5 hours at a temperature of 50° C. After the reaction is completed, washing with diethylene glycol dimethyl ether and drying to obtain a regenerated positive electrode material.
[0056] Comparative Example 1
[0057] Same as Example 1, except that no alkaline substance is introduced into the lithium extraction reagent
[0058] Comparative Example 2
[0059] Same as Example 2, except that no alkaline substance is introduced into the lithium extraction reagent
[0060] Comparative Example 3
[0061] As in Example 3, no alkaline substance is introduced into the lithium extraction reagent.
[0062] The reaction conditions and leaching efficiency of Examples 1-5 and Comparative Examples 1-3 are shown in Table 1. It can be seen that alkaline substances are introduced in Examples 1-5, and the extraction efficiency reaches a high level in a short time. Compared with Example 1, no alkaline substances are applied in Comparative Example 1, and the lithium extraction efficiency in half an hour is only 74%. Compared with Example 2, the lithium extraction efficiency of Comparative Example 2 is still lower under the same time. Compared with Example 3, Comparative Example 3 does not add alkaline substances. Although the leaching time is extended to 10h, its lithium extraction efficiency is still only 85%, which is difficult to reach the level of Example 3, indicating the effectiveness of the method provided by the present invention.
[0063] Table 1 Reaction conditions and leaching efficiency of Examples 1-5 and Comparative Examples 1-3
[0064]
[0065]
[0066] The regenerated positive electrode materials obtained in Examples 1-5 and Comparative Examples 1-3 were respectively combined with graphite to form full batteries, and performance tests were performed on them. The data are shown in Figure 2. It can be seen that the first-cycle charging capacity of the lithium iron phosphate positive electrode material after regeneration in Example 1-5 can basically be restored to the level of theoretical capacity (172mAhg-1). Some results are higher than this value, which may be caused by excessive lithium insertion during the regeneration process or slight errors. In contrast, although the performance of the waste lithium iron phosphate can be restored to a certain extent in Comparative Examples 1-3, the degree of recovery is lower than that in Example 1-5. In terms of cycle performance, there is a certain gap in the first-cycle efficiency, which may be due to the higher lithium content in the lithium-rich solution of Example 1-5, which further reflects the high efficiency of the method. Comparative Example 4 is a full battery reassembled from waste lithium iron phosphate. It can be seen that its performance is poor and it is difficult to continue to meet the use requirements.
[0067] Table 2 Performance data of the full battery composed of regenerated positive electrode materials and graphite
[0068]
[0069]
[0070] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for recycling lithium from waste batteries assisted by alkaline substances, characterized in that: The method comprises the following steps: S1: using a lithium extraction reagent to leach the negative electrode material of the waste lithium-ion battery to obtain a solid-liquid mixture, wherein the lithium extraction reagent is an organic solvent in which aromatic hydrocarbon compounds and alkaline substances are dissolved, and the alkaline substance destroys the solid electrolyte membrane on the surface of the graphite during operation to accelerate the leaching of lithium, and the alkaline substance is one or more of sodium hydroxide, potassium hydroxide and ammonia water; S2 separates the solid-liquid mixture obtained in step S1 to obtain a lithium-rich solution, and then achieves efficient recovery of lithium from waste lithium-ion batteries with the assistance of alkaline substances.
2. The method for recycling lithium from waste batteries based on alkaline substances as claimed in claim 1, characterized in that: The mass fraction of the alkaline substance in the lithium extraction reagent is 0.01% to 1%.
3. The method for recycling lithium from waste batteries assisted by alkaline substances according to claim 1, characterized in that: The molar concentration of the aromatic hydrocarbon compound in the lithium extraction reagent is 0.2 mol / L to 3 mol / L.
4. The method for recycling lithium from waste batteries assisted by alkaline substances according to claim 1, characterized in that: The aromatic hydrocarbon compound is one or more of benzene, naphthalene, phenanthrene, anthracene, tetracene, pyrene and perylene, and the aromatic hydrocarbon compound includes at least one substituent, and the substituent is an alkyl group, a hydroxyl group, a nitro group, a halogen atom, an amino group, a carboxyl group, an aldehyde group, a carbonyl group, a sulfonic acid group, a disulfide bond, an ester bond or an ether bond.
5. The method for recycling lithium from waste batteries based on alkaline substances as claimed in claim 1, characterized in that: The organic solvent is one or more of ethers, esters and aromatics, the ethers include one or more of tetrahydrofuran, ethylene glycol dimethyl ether, 1,3-dioxolane, diethanol dimethyl ether, triethanol dimethyl ether and tetraethanol dimethyl ether; the esters are one or more of ethylene carbonate, propylene carbonate, diethyl carbonate and vinylene carbonate; the aromatics are benzene and / or toluene.
6. The method for recycling lithium from waste batteries based on alkaline substances as claimed in claim 1, characterized in that: In step S1, the leaching time is 10 min to 10 h, and the leaching temperature is -10°C to 100°C.
7. The method for recycling lithium from waste batteries assisted by alkaline substances according to claim 1, characterized in that: In step S1, during leaching, the mass ratio of the active substance in the negative electrode material to the lithium extraction reagent is 1:1 to 1:
5.
8. The method for recycling lithium from waste batteries based on alkaline substances as claimed in claim 1, characterized in that: The method for obtaining the negative electrode material is: charging the waste lithium-ion battery to a fully charged state, and then disassembling it in a safe environment with a relative humidity of less than 20% to obtain the negative electrode material.
9. The method for recycling lithium from waste batteries based on the assistance of alkaline substances according to any one of claims 1 to 8, characterized in that The method for efficiently recovering lithium from waste lithium-ion batteries also includes step S3, which specifically comprises: soaking the material to be treated with the lithium-rich solution, thereby lithiation the material to be treated to achieve lithium recycling.
10. The method for recycling lithium from waste batteries based on alkaline substances as claimed in claim 9, characterized in that: The material to be treated is a lithium-ion battery positive electrode. The lithium-ion battery positive electrode is mixed with a lithium-rich solution and subjected to a hydrothermal reaction, and then dried and washed to obtain a pre-lithiated positive electrode.
Citation Information
Patent Citations
A method for safely and efficiently recycling lithium from waste batteries
CN113061726B
Method for safely and efficiently recycling lithium from waste battery
CN113061726A
Battery negative electrode all-component recovery method and graphite obtained through recovery
CN115954573A
Lithium recovery method based on weak-polarity organic solvent and application thereof
CN116516176A
Electrolyte and battery
CN116826173A