A method for manufacturing a photomask and a photomask template

By forming organic and inorganic film layers on the substrate using nanoimprint lithography, the problems of high cost and complex process in manufacturing high PPI photomasks have been solved, enabling high-precision, low-cost photomask manufacturing and improving the hardness and durability of the photomasks.

CN117821898BActive Publication Date: 2026-11-17BOE TECHNOLOGY GROUP CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410063376.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-16
Publication Date
2026-11-17
Estimated Expiration
2044-01-16

AI Technical Summary

Technical Problem

Existing technologies for producing high PPI masks are costly, complex, and difficult to meet the requirements for ultra-fine mask patterns, especially the etching and laser patterning processes, which are expensive and complex.

Method used

An organic film layer and an inorganic film layer are formed on a substrate using nanoimprint lithography. A first pattern is formed on the organic film layer by nanoimprint lithography, and an inorganic film layer is covered on the organic film layer. An opening pattern is formed by conformal etching to obtain a mask that meets the high PPI requirements.

Benefits of technology

It achieves high-precision mask patterns, reduces equipment costs, simplifies the manufacturing process, and improves the hardness and durability of the mask.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117821898B_ABST
    Figure CN117821898B_ABST
Patent Text Reader

Abstract

This disclosure provides a method for fabricating a photomask and the photomask itself. The method includes: providing a substrate; printing an organic film layer with a first pattern on the substrate using nanoimprint lithography; forming an inorganic film layer on the organic film layer, wherein the inorganic film layer conformally covers the first pattern to form a second pattern, the second pattern including recessed areas and non-recessed areas; removing at least a portion of the substrate, the organic film layer, and the inorganic film layer corresponding to the recessed areas, so that the recessed areas form an opening pattern, thereby obtaining the photomask. The method and photomask provided in this disclosure can fabricate photomasks that meet high PPI requirements, and are low in cost and simple in process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of display technology, and in particular to a method for manufacturing a photomask and a photomask template. Background Technology

[0002] Organic light-emitting diodes (OLEDs) are self-emissive display devices. To improve color gamut, contrast, and brightness efficiency, independent red, green, and blue (RGB) light-emitting layers are often used to achieve OLED color displays. These independent RGB light-emitting layers are implemented using a vapor deposition process, which requires a photomask. The photomask is used to deposit organic light-emitting materials onto the designed locations on the backplane, and its quality directly affects the display performance of the OLED panel.

[0003] In related technologies, etching or laser patterning processes are generally used to form the opening pattern on the mask. However, with the development of high PPI (pixel count) technology, if the requirements for ultra-fine mask patterns are to be met, the etching process equipment or laser patterning equipment is expensive, costly, and the manufacturing process is complex. Summary of the Invention

[0004] This disclosure provides a method for manufacturing a photomask and a photomask template, which can manufacture photomasks that meet high PPI requirements, and is low in cost and simple in process.

[0005] The technical solutions provided in this disclosure are as follows:

[0006] In a first aspect, embodiments of this disclosure provide a method for manufacturing a photomask, the method comprising:

[0007] Provide a base;

[0008] An organic film layer with a first pattern is printed on the substrate using nanoimprint lithography.

[0009] An inorganic film layer is formed on the organic film layer, wherein the inorganic film layer conformally covers the first pattern to form a second pattern, the second pattern including grooved areas and non-grooved areas;

[0010] At least the portions of the substrate, the organic film layer, and the inorganic film layer corresponding to the groove region are removed to form an opening pattern in the groove region, thereby obtaining the mask template.

[0011] For example, the step of printing an organic film layer with a first pattern on the substrate using nanoimprint lithography specifically includes:

[0012] An embossing mold is provided, wherein the embossing mold is provided with an embossing pattern;

[0013] A first organic material is coated on the substrate, wherein the first organic material is a curable organic material;

[0014] The embossing mold is attached to the first organic material;

[0015] The first organic material is cured to form the organic film layer having the first pattern;

[0016] Separate the embossing mold from the organic film layer.

[0017] For example, the curing treatment of the first organic material specifically includes: curing the first organic material by means of thermal curing and / or UV curing.

[0018] For example, the first organic material is selected from at least one of vinyl monomers and vinyl oligomers.

[0019] For example, before forming an organic film layer with a first pattern on the substrate using nanoimprint lithography, the method further includes a step of fabricating an imprint mold, specifically including:

[0020] A chip is provided, the chip having a third pattern corresponding to the first pattern;

[0021] A second organic material is coated onto the wafer, wherein the second organic material is a curable organic material;

[0022] A support substrate is pressed onto the second organic material, and the second organic material is cured to form an imprinted film layer with an imprinted pattern.

[0023] The wafer is separated from the imprinting film layer to obtain the imprinting mold.

[0024] For example, the second organic material is selected from at least one of polydimethylsiloxane, acrylic acid, or epoxy resin.

[0025] For example, the step of pressing a support substrate onto the second organic material and curing the second organic material specifically includes curing the second organic material using a thermosetting and / or ultraviolet curing method.

[0026] For example, in the photomask, the thickness of the organic film layer is 10-20 micrometers, and the thickness of the inorganic film layer is 5-15 micrometers.

[0027] For example, the thickness ratio of the organic film layer to the inorganic film layer is 1.33:1 to 1.5:1.

[0028] For example, the step of removing at least the portions of the substrate, the organic film layer, and the inorganic film layer corresponding to the groove region, so that the groove region forms an opening pattern to obtain the mask, specifically includes:

[0029] The substrate includes a first side and a second side disposed opposite to each other. The organic film layer and the inorganic film layer are formed on the first side. The substrate, the organic film layer and the inorganic film layer are etched from the side where the second side of the substrate is located to a predetermined depth, so that the portions of the organic film layer and the inorganic film layer facing the groove area are completely etched away.

[0030] For example, forming an inorganic film layer on the organic film layer specifically includes:

[0031] The inorganic film layer is formed on the organic film layer by chemical vapor deposition or atomic layer deposition, wherein the inorganic film layer is a single-layer structure or a multi-layer structure.

[0032] Secondly, embodiments of this disclosure provide a photomask, which is manufactured using the method described above. The photomask includes an organic film layer and an inorganic film layer stacked on the organic film layer, and the photomask has an opening pattern.

[0033] The beneficial effects of the embodiments disclosed herein are as follows:

[0034] The photomask fabrication method and photomask provided in this disclosure employ nanoimprint lithography to form an organic film layer, resulting in a first pattern on the organic film layer. The shape of the first pattern is adapted to the shape of the opening pattern on the photomask, and the precision meets the requirements for high PPI photomask pattern precision. An inorganic film layer is then conformally covered on the organic film layer. At least the portions corresponding to the groove regions in the substrate, the organic film layer, and the inorganic film layer are removed to form opening patterns in the groove regions, thus obtaining the photomask. In this way, because the organic film layer is formed using nanoimprint lithography, the shape of the first pattern can be adapted to the shape of the opening pattern on the photomask, and the precision of the first pattern meets the requirements for high PPI opening patterns. Furthermore, the inorganic film layer covering the organic film layer increases the hardness and durability of the entire photomask. Compared to traditional etching or laser patterning processes for fabricating photomasks, the above method achieves higher pattern precision requirements, reduces equipment costs, and simplifies the fabrication process. Attached Figure Description

[0035] Figure 1 A flowchart illustrating the method for manufacturing a mask template according to an embodiment of this disclosure;

[0036] Figure 2This represents the front view of the mask template provided in the embodiments of this disclosure;

[0037] Figure 3 This indicates that the mask template provided in one embodiment of the present disclosure is in Figure 2 Sectional view along line E-E';

[0038] Figure 4 This indicates that the mask template provided in another embodiment of this disclosure is in Figure 2 Sectional view along line E-E';

[0039] Figure 5 This is a schematic diagram illustrating one of the steps in the method for manufacturing a mask template provided in this embodiment of the present disclosure;

[0040] Figure 6 This is the second schematic diagram illustrating the steps in the method for manufacturing a mask template provided in this embodiment of the present disclosure;

[0041] Figure 7 This indicates the relationship between the thickness ratio of the organic film layer to the inorganic film layer of the photomask provided in several embodiments of this disclosure and the residual stress.

[0042] Figure 8 A schematic diagram illustrating the relationship between internal stress and thickness of different inorganic films. Detailed Implementation

[0043] To make the objectives, technical solutions, and advantages of the embodiments of this disclosure clearer, the technical solutions of the embodiments of this disclosure will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some, not all, of the embodiments of this disclosure. All other embodiments obtained by those skilled in the art based on the described embodiments of this disclosure without creative effort are within the scope of protection of this disclosure.

[0044] Unless otherwise defined, the technical or scientific terms used in this disclosure shall have the ordinary meaning understood by one of ordinary skill in the art to which this disclosure pertains. The terms “first,” “second,” and similar terms used in this disclosure do not indicate any order, quantity, or importance, but are merely used to distinguish different components. Similarly, the terms “an,” “a,” or “the,” and similar terms do not indicate a quantity limitation, but rather indicate the presence of at least one. The terms “including,” “comprising,” or “containing,” and similar terms mean that the element or object preceding the word encompasses the elements or objects listed following the word and their equivalents, without excluding other elements or objects. The terms “connected,” “linked,” or similar terms are not limited to physical or mechanical connections, but can include electrical connections, whether direct or indirect. The terms “upper,” “lower,” “left,” and “right,” etc., are used only to indicate relative positional relationships, and these relative positional relationships may change accordingly when the absolute position of the described objects changes.

[0045] Before providing a detailed description of the mask fabrication method and the mask provided in the embodiments of this disclosure, the following descriptions of the related technologies are provided:

[0046] In related technologies, etching or laser patterning (LPM) processes are generally used to form fine opening patterns on the OLED mask.

[0047] For etching processes, either wet or dry etching can be used. The etching process generally includes steps such as coating, exposure, development, and etching. During etching, the linewidth of the opening pattern on the resulting mask depends on the wavelength of light used in the exposure process. Given current etching technology, forming ultra-fine opening patterns smaller than 100 nm is extremely difficult. Furthermore, with advancements in pattern refinement, etching equipment, including exposure equipment, becomes increasingly expensive, leading to higher costs and increased prices for high-PPI masks, thus reducing their effectiveness. Moreover, the pattern formation process during etching requires exposure, development, etching, and cleaning, making the fabrication process time-consuming and complex.

[0048] Laser patterning involves using a laser to drill holes in a metal plate to create an opening pattern for the photomask. While laser patterning can achieve high PPI photomasks, it requires expensive lasers, is technically very challenging, and results in high unit prices for the manufactured photomasks.

[0049] To address the aforementioned issues, this disclosure provides a method for manufacturing a photomask and a photomask template that can produce photomasks that meet high PPI requirements, while also being low in cost and simple in process.

[0050] Nanoimprint lithography (NIL) is a technique that utilizes photolithography for nanoscale fabrication, precisely compressing desired patterns to the nanoscale. Unlike traditional optical lithography, nanoimprint lithography does not achieve patterning by altering the photochemical properties of the polymer. Instead, it presses a template onto the surface of a polymer-coated substrate, and the pattern is transferred through the deformation of the polymer under stress. Therefore, the optimal resolution achievable with this lithography method is not affected by diffraction, scattering, interference that may occur on the polymer, or backscattering from the substrate; it is directly determined by the resolution of the pattern on the template.

[0051] Nanoimprint lithography offers several advantages. It boasts low cost, enabling the fabrication of precise nanoscale structures at a low cost, facilitating mass production. Furthermore, it offers high precision, producing structures that meet requirements for accuracy, roughness, and dimensional range. Moreover, nanoimprint lithography allows for the efficient implementation of complex designs, flexible structural modifications, and good self-correcting capabilities.

[0052] Based on this, such as Figure 1 As shown, the method for manufacturing a photomask provided in this embodiment includes:

[0053] Step S01: Provide a substrate 100;

[0054] Step S02: Using nanoimprint lithography, an organic film layer 200 with a first pattern 201 is printed on the substrate 100;

[0055] Step S03: An inorganic film layer 300 is formed on the organic film layer 200, wherein the inorganic film layer 300 conformally covers the first pattern 201 to form a second pattern 301, the second pattern 301 including a groove region A and a non-groove region B.

[0056] Step S04: Remove at least the portion of the substrate 100, the organic film layer 200, and the inorganic film layer 300 corresponding to the groove region A, so that the groove region A forms an opening pattern A1, thereby obtaining the mask template 10.

[0057] In the above scheme, an organic film layer 200 is formed by nanoimprint lithography, so that the organic film layer 200 has a first pattern 201. The shape of the first pattern 201 can be adapted to the shape of the opening pattern A1 on the mask 10. The accuracy can meet the pattern accuracy requirements of the high ppi mask 10. Furthermore, an inorganic film layer 300 is irregularly covered on the organic film layer 200. Then, at least the portion of the substrate 100, the organic film layer 200, and the inorganic film layer 300 corresponding to the groove region A is removed, so that the groove region A forms the opening pattern A1, thus obtaining the mask 10.

[0058] In this way, since the organic film layer 200 is formed by nanoimprint lithography, the shape of the first pattern 201 can be adapted to the shape of the opening pattern A1 on the mask 10, and the precision of the first pattern 201 can meet the requirements of the high PPI opening pattern A1. Furthermore, the inorganic film layer 300 covering the organic film layer 200 can increase the hardness and durability of the entire mask 10. Compared with the traditional etching or laser patterning process for making the mask 10, the above method can achieve higher pattern precision requirements, reduce equipment costs, and simplify the manufacturing process.

[0059] In some exemplary embodiments, since the substrate 100 needs to be removed in step S04, the substrate 100 can be made of a material with low etching resistance, such as a metal-based material, in step S01. It is understood, of course, that the material of the substrate 100 is not limited to this.

[0060] In some exemplary embodiments, please refer to Figure 1 and Figure 5 As shown, step S02 specifically includes:

[0061] Step S021, Provide an embossing mold 400 (e.g. Figure 6 (See diagram (e) for a schematic diagram of the embossing mold 400). The embossing mold 400 is provided with an embossing pattern 401, wherein the embossing pattern 401 is a concave-convex pattern that matches the shape and size of the opening pattern A1 on the final formed mask 10.

[0062] Step S022, please refer to Figure 5 As shown in (a), a first organic material 200' is coated on the substrate 100, wherein the first organic material 200' is a curable organic material;

[0063] In this step, for example, the first organic material 200' can be coated onto the substrate 100 using methods such as inkjet printing or spin coating. The first organic material 200' then cures to form the organic film layer 200. The first organic material 200' can be an organic material that can be cured by heat and / or ultraviolet (UV) light. For example, the first organic material 200' can include, but is not limited to, at least one of vinyl monomers and vinyl oligomers.

[0064] Step S023: Attach the imprinting mold 400 to the first organic material 200';

[0065] Specifically, in this step, please refer to Figure 5 As shown in (b), the embossing pattern 401 of the embossing mold 400 is oriented toward the first organic material 200' on the substrate 100. Please refer to [link / reference]. Figure 5 As shown in (c), the embossing mold 400 is pressed onto the substrate 100 so that the embossed pattern 401 is tightly adhered to the first organic material 200';

[0066] Step S024, please refer to Figure 5 As shown in (d), the first organic material 200' is cured to form the organic film layer 200 having a first pattern 201;

[0067] For example, in this step, after the imprinting mold 400 is pressed onto the first organic material 200', the first organic material 200' is subjected to heat curing and / or ultraviolet curing treatment so that the first organic material 200' is cured to form the organic film layer 200 with the first pattern 201.

[0068] Step S025: Separate the imprinting mold 400 from the organic film layer 200 to obtain the following... Figure 5 The structure shown in (e) is shown in the middle.

[0069] It is understood that the above is only an exemplary description of the nanoimprint lithography process in step S02. In other embodiments, the specific process of step S02 is not limited thereto.

[0070] Furthermore, in some exemplary embodiments, in step S024 above, both thermosetting and ultraviolet curing methods can be used simultaneously to cure the first organic material 200'. This ensures that the first organic material 200' is fully cured, thereby guaranteeing the accuracy of the first pattern 201 on the final organic film layer 200.

[0071] For example, in step S02 above, when ultraviolet curing is used to cure the first organic material 200', the wavelength of the ultraviolet light can be less than or equal to 395 nm. When thermal curing is used to cure the first organic material 200', the curing temperature can be between 80 and 100°C. This ensures that the first organic material 200' is fully cured. For example, the curing temperature can be 80°C, 90°C, or 100°C. Of course, it is understood that the above are only examples, and in practical applications, the curing method and curing conditions are not limited to these.

[0072] It should also be noted that, in some other exemplary embodiments, step S024 above may involve first curing the first organic material 200' using ultraviolet light, and then curing it using heat. This ensures that the first organic material 200' is fully cured, thereby guaranteeing the accuracy of the first pattern 201 on the final organic film layer 200.

[0073] Furthermore, it should be noted that when the first organic material 200' is cured using ultraviolet curing, the imprinting mold 400 can be made of a light-transmitting material.

[0074] For example, such as Figure 6 As shown in (e), the embossing mold 400 may include a support substrate 410 and an embossing film layer 420 disposed on the support substrate 410, wherein the embossing pattern 401 is disposed on the embossing film layer 420, and the support substrate 410 can serve to provide a base plate and support for the embossing film layer 420. Both the embossing film layer 420 and the support substrate 410 may be made of light-transmitting material.

[0075] For example, the imprinting film layer 420 can be made of transparent organic materials such as polydimethylsiloxane (PDMS), acrylic acid, or epoxy resin; the supporting substrate 410 can be made of glass, etc. Of course, it is understood that the specific structure and materials of the imprinting mold 400 are not limited thereto.

[0076] In some exemplary embodiments, please continue to refer to Figure 5 As shown in (e), step S03 specifically includes: forming the inorganic film layer 300 on the organic film layer 200 using chemical vapor deposition (PECVD) or atomic layer deposition (ALD). The inorganic film layer 300 can be a single-layer structure or a multi-layer structure formed by stacking multiple inorganic film layers 300.

[0077] The inorganic film layer 300 can improve the hardness and durability of the final fabricated photomask 10. For example, the material of the inorganic film layer 300 can be selected from silicon-based compounds and aluminum-based compounds. As an exemplary embodiment, the material of the inorganic film layer 300 can be silicon nitride (SiN). x ), silicon dioxide (SiO) x One or more of the following. In other words, the inorganic film layer 300 can be a single silicon nitride film layer, a single silicon oxide film layer, or a multi-layer stacked structure consisting of silicon nitride and silicon oxide film layers stacked sequentially.

[0078] As an exemplary embodiment, when the inorganic film layer 300 is a multi-layer structure, step S03 may specifically include sequentially depositing multiple inorganic film layers, such as a silicon nitride film layer 311 and a silicon oxide film layer 312, on the organic film layer 200. For example, as... Figure 4 As shown, in some embodiments, the inorganic film layer 300 may include a silicon nitride film layer 311 and a silicon oxide film layer 312 stacked sequentially. It is understood, of course, that in other embodiments not shown, the silicon nitride film layer 311 is not limited to one layer, and the silicon oxide film layer 312 is not limited to one layer.

[0079] In some exemplary embodiments, please continue to refer to Figure 1 and Figure 5 As shown, step S04 above specifically includes the following steps:

[0080] like Figure 5 As shown in (f), the substrate 100 includes a first surface 100a and a second surface 100b disposed opposite to each other. The organic film layer 200 and the inorganic film layer 300 are formed on the first surface 100a. Wet etching and / or dry etching are used to etch the substrate, the organic film layer 200, and the inorganic film layer 300 to a predetermined depth from the side where the second surface 100b of the substrate 100 is located, so that the portions of the organic film layer 200 and the inorganic film layer 300 directly opposite the groove region A are completely etched away, forming a shape as shown in (f). Figure 5 The mask shown in (g) is a template.

[0081] Specifically, in an exemplary embodiment, in step S04 above, dry etching can be performed first, followed by wet etching, to etch the substrate, the organic film layer 200, and the inorganic film layer 300, so that the portion of the organic film layer 200 and the inorganic film layer 300 facing the groove region A is completely etched away, so that the groove region A can form the opening pattern A1 on the final mask 10.

[0082] In some exemplary embodiments, prior to step S02 above, the method further includes:

[0083] Step S011, the step of making the embossing mold 400.

[0084] For example, such as Figure 6 As shown, step S011 above may include the following steps:

[0085] Step S0111, as follows Figure 6 As shown in (a), a chip 430 is provided, the chip 430 having a third pattern 421 corresponding to the first pattern 201;

[0086] Step S0112, as follows Figure 6 As shown in (b), a second organic material 420' is coated on the wafer 430, wherein the second organic material 420' is selected as a curable organic material;

[0087] Step S0113, as Figure 6 As shown in (c), a support substrate 410 is pressed onto the second organic material 420', and as... Figure 6 As shown in (d), the second organic material 420' is cured to form an imprinted film layer 420 with an imprinted pattern 401.

[0088] Step S0114: Separate the wafer 430 from the imprinted film layer 420 to obtain the following... Figure 6 The embossing mold 400 shown in (e) is shown in the middle.

[0089] For example, in step S0111 above, the wafer 430 may be a silicon-based wafer. The wafer 430 is not limited to a silicon-based wafer; it may be a wafer 430 containing a thin film formed from organic material components. The wafer 430 may form the third pattern 431 by etching or other methods, and the third pattern 431 is adapted to the shape and size of the finally formed imprinted pattern 401.

[0090] For example, in step S0112 above, the second organic material 420' may include, but is not limited to, at least one of polydimethylsiloxane, polymethacrylate or epoxy resin.

[0091] For example, the coating thickness of the second organic material 420' can be 10 to 20 micrometers, that is, the thickness of the imprinted film layer 420 formed by curing the second organic material 420' can be 10 to 20 micrometers.

[0092] For example, in step S0113 above, pressing the support substrate 410 onto the second organic material 420' and curing the second organic material 420' specifically includes curing the second organic material 420' using a thermosetting and / or ultraviolet curing method.

[0093] For photomasks, lower residual stress indicates less deformation and better hardness and durability. Residual stress can be detected by methods including, but not limited to, X-ray diffraction stress analysis. Taking X-ray diffraction stress analysis as an example, the morphology of the sample is measured using a laser, and the residual stress is calculated by comparing the changes in the radius of curvature of the substrate before and after coating and substituting these changes into Stoney's Equation.

[0094] The Stone equation is as follows:

[0095]

[0096] In the formula, σ film This represents the average residual stress of the thin film;

[0097] E S Indicates the Young's modulus of the thin film;

[0098] V S This represents the Poisson's ratio of the substrate;

[0099] t S Indicates the thickness of the substrate;

[0100] t f Indicates the thickness of the film;

[0101] R s Indicates the initial radius of curvature of the substrate;

[0102] R f This indicates the radius of curvature after coating.

[0103] Using the mask template manufacturing method provided in this disclosure, several embodiment mask templates were manufactured. Residual stress was tested on the mask templates in different embodiments, and the relationship between the film thickness ratio of the organic film layer 200 and the inorganic film layer 300 and the residual stress of the mask template 10 was obtained, as shown in Table 1.

[0104] As shown in Table 1, during the fabrication of the mask 10, the inorganic film layer 300 and the organic film layer 200 have different thicknesses, resulting in different residual stresses in the mask 10. Furthermore, when the thickness ratio of the organic film layer 200 to the inorganic film layer 300 is 1.33:1 to 1.5:1, the residual stress of the mask 10 is 75 MPa and 80 MPa, respectively, which is relatively low. Therefore, in some embodiments, it is preferable that the thickness ratio of the organic film layer 200 to the inorganic film layer 300 be selected from 1.33:1 to 1.5:1.

[0105] For example, in one embodiment, the thickness ratio of the organic film layer 200 to the inorganic film layer 300 is 1.33:1; in another embodiment, the thickness ratio of the organic film layer 200 to the inorganic film layer 300 is 1.5:1.

[0106] also, Figure 8 The diagram shows the relationship between the thickness of an inorganic film and the internal stress of the film. From... Figure 8 It is known that the internal stress of silicon nitride (SiNx) films is positive, exhibiting tensile stress, which increases with increasing thickness; while the internal stress of silicon oxide (SiOx) films is negative, exhibiting compressive stress, which also increases with increasing thickness. Therefore, the internal stresses of the stacked silicon nitride and silicon oxide films can essentially cancel each other out, thereby reducing the residual stress of the mask and improving its durability. Furthermore, the stack thickness of these two inorganic film layers can be deposited to 5–15 micrometers as needed, thereby increasing the hardness of the mask.

[0107] Therefore, in some exemplary embodiments, the inorganic film layer 300 can be a stacked structure formed by stacking silicon oxide thin films and silicon nitride thin films. And, exemplaryly, the thickness of the organic film layer 200 can be 10–20 micrometers, and the thickness of the inorganic film layer 300 can be 5–15 micrometers.

[0108] For example, in one embodiment, the organic membrane layer 200 has a thickness of 20 micrometers and the inorganic membrane layer 300 has a thickness of 15 micrometers; in another embodiment, the organic membrane layer 200 has a thickness of 15 micrometers and the inorganic membrane layer 300 has a thickness of 10 micrometers.

[0109] Specifically, in some embodiments, the first organic material is polymethyl methacrylate, the thickness of the organic film layer is 10 micrometers, and the inorganic film layer is selected from the stacked structure of silicon nitride film and silicon oxide film. For example, silicon oxide film and silicon nitride film are stacked alternately to form a six-layer stacked inorganic film layer, the thickness of the inorganic film layer is 15 micrometers, wherein the thickness of a single layer of silicon nitride film and silicon oxide film is 2.5 μm, and the thickness ratio of the organic film layer to the inorganic film layer is 0.66:1. At this time, the residual stress of the obtained mask is 150 MPa.

[0110] In other embodiments, the first organic material is polymethyl methacrylate, the thickness of the organic film layer is 10 micrometers, and the inorganic film layer is a stacked structure of silicon nitride film and silicon oxide film, for example, silicon oxide film and silicon nitride film are stacked alternately to form a four-layer stacked inorganic film layer, the thickness of the inorganic film layer is 10 micrometers, wherein the thickness of a single layer of silicon nitride film and silicon oxide film is 2.5 μm, the thickness ratio of the organic film layer to the inorganic film layer is 1:1, and the residual stress of the resulting mask is 100 MPa;

[0111] In other embodiments, the first organic material is polydimethylsiloxane, the organic film layer has a thickness of 20 micrometers, the inorganic film layer is a six-layer stacked structure formed by alternating silicon nitride film and silicon oxide film, the inorganic film layer has a thickness of 15 micrometers, wherein each single layer of silicon nitride film and silicon oxide film is 2.5 μm, the thickness ratio of the organic film layer to the inorganic film layer is 1.33:1, and the residual stress of the resulting photomask is 75 MPa.

[0112] In other embodiments, the first organic material is polydimethylsiloxane, the thickness of the organic film is 15 micrometers, the inorganic film is a four-layer stacked structure formed by alternating silicon nitride film and silicon oxide film, the thickness of the inorganic film is 10 micrometers, wherein each single layer of silicon nitride film and silicon oxide film is 2.5 μm, the thickness ratio of the organic film to the inorganic film is 1.5:1, and the residual stress of the resulting photomask is 80 MPa.

[0113] In other embodiments, the first organic material is polydimethylsiloxane, the thickness of the organic film is 20 micrometers, the inorganic film is a two-layer stacked structure formed by alternating silicon nitride film and silicon oxide film, the thickness of the inorganic film is 10 micrometers, wherein the thickness of a single layer of silicon nitride film and silicon oxide film is 2.5 μm, the thickness ratio of the organic film to the inorganic film is 2:1, and the residual stress of the resulting mask is 120 MPa.

[0114] In other embodiments, the first organic material is polydimethylsiloxane, the thickness of the organic film is 20 micrometers, the inorganic film is a two-layer stacked structure formed by stacking silicon nitride film and silicon oxide film, the thickness of the inorganic film is 5 micrometers, wherein the thickness of a single layer of silicon nitride film and silicon oxide film is 2.5 μm, the thickness ratio of the organic film to the inorganic film is 4:1, and the residual stress of the resulting mask is 180 MPa.

[0115] Furthermore, this disclosure provides a mask template. Figure 2 The image shown is a front view of the structure of a mask template 10 provided in one embodiment of this disclosure. Figure 3 and Figure 4 The diagram shows a cross-sectional view of the mask template 10 provided in different embodiments of this disclosure. The mask template 10 provided in one embodiment of this disclosure can be used as a fine metal mask (FMM).

[0116] Please see Figures 2 to 4 As shown, the mask 10 provided in this embodiment can be manufactured using the mask manufacturing method provided in this embodiment. The mask 10 has an opening pattern A1 and includes an organic film layer 200 and an inorganic film layer 300 stacked on the organic film layer 200.

[0117] Obviously, the mask 10 provided in this embodiment also has the beneficial effects brought about by the mask manufacturing method provided in this embodiment. It can be used as a high PPI mask and has the advantages of low cost and high precision of the opening pattern A1. It will not be described in detail here.

[0118] The following points need to be explained:

[0119] (1) The accompanying drawings of the embodiments of this disclosure only involve the structures involved in the embodiments of this disclosure. Other structures can be referred to the general design.

[0120] (2) For clarity, the thickness of layers or regions is enlarged or reduced in the drawings used to describe embodiments of the present disclosure, i.e., these drawings are not drawn to scale. It will be understood that when an element such as a layer, film, region, or substrate 100 is referred to as being “above” or “below” another element, the element may be “directly” located “above” or “below” the other element or there may be intermediate elements.

[0121] (3) Where there is no conflict, the embodiments of this disclosure and the features in the embodiments can be combined with each other to obtain new embodiments.

[0122] The above are merely specific embodiments of this disclosure, but the scope of protection of this disclosure is not limited thereto. The scope of protection of this disclosure shall be determined by the scope of the claims.

Claims

1. A method for manufacturing a mask template, characterized in that, The method includes: Provide a base; An organic film layer with a first pattern is printed on the substrate using nanoimprint lithography. An inorganic film layer is formed on the organic film layer, wherein the inorganic film layer conformally covers the first pattern to form a second pattern, the second pattern including grooved areas and non-grooved areas; At least the portions of the substrate, the organic film layer, and the inorganic film layer corresponding to the groove regions are removed to form an opening pattern in the groove regions, thereby obtaining the mask template; In the photomask, the organic film layer has a thickness of 10-20 micrometers, the inorganic film layer has a thickness of 5-15 micrometers, and the thickness ratio of the organic film layer to the inorganic film layer is 1.33:1 to 1.5:

1.

2. The method for manufacturing a mask template according to claim 1, characterized in that, The method of using nanoimprint lithography to print an organic film layer with a first pattern on the substrate specifically includes: An embossing mold is provided, wherein the embossing mold is provided with an embossing pattern; A first organic material is coated on the substrate, wherein the first organic material is a curable organic material; The embossing mold is attached to the first organic material; The first organic material is cured to form the organic film layer having the first pattern; Separate the embossing mold from the organic film layer.

3. The method for manufacturing a mask template according to claim 2, characterized in that, The curing treatment of the first organic material specifically includes: using a thermosetting method and / or a UV curing method to cure the first organic material.

4. The method for manufacturing a mask template according to claim 2, characterized in that, The first organic material is selected from at least one of vinyl monomers and vinyl oligomers.

5. The method for manufacturing a mask template according to claim 2, characterized in that, Before forming an organic film layer with a first pattern on the substrate using nanoimprint lithography, the method further includes a step of fabricating an imprint mold, specifically including: A chip is provided, the chip having a third pattern corresponding to the first pattern; A second organic material is coated onto the wafer, wherein the second organic material is a curable organic material; A support substrate is pressed onto the second organic material, and the second organic material is cured to form an imprinted film layer with an imprinted pattern. The wafer is separated from the imprinting film layer to obtain the imprinting mold.

6. The method for manufacturing a mask template according to claim 5, characterized in that, The second organic material is selected from at least one of polydimethylsiloxane, acrylic acid, or epoxy resin.

7. The method for manufacturing a mask template according to claim 5, characterized in that, The step of pressing a support substrate onto the second organic material and curing the second organic material specifically includes curing the second organic material using a thermosetting and / or ultraviolet curing method.

8. The method for manufacturing a mask template according to claim 1, characterized in that, The step of removing at least the portions of the substrate, the organic film layer, and the inorganic film layer corresponding to the groove regions to form an opening pattern in the groove regions, thereby obtaining the mask template, specifically includes: The substrate includes a first side and a second side disposed opposite to each other. The organic film layer and the inorganic film layer are formed on the first side. The substrate, the organic film layer and the inorganic film layer are etched from the side where the second side of the substrate is located to a predetermined depth, so that the portions of the organic film layer and the inorganic film layer facing the groove area are completely etched away.

9. The method for manufacturing a mask template according to claim 1, characterized in that, The formation of an inorganic film layer on the organic film layer specifically includes: The inorganic film layer is formed on the organic film layer by chemical vapor deposition or atomic layer deposition, wherein the inorganic film layer is a single-layer structure or a multi-layer structure.

10. A photomask, characterized in that, The mask is manufactured using the method described in any one of claims 1 to 9, wherein the mask comprises an organic film layer and an inorganic film layer stacked on the organic film layer, and the mask has an opening pattern.

Citation Information

Patent Citations

  • Preparation method of flexible mask plate

    CN102747319A

  • Manufacturing process of an organic mask for microelectronic industry

    US20070298333A1