A kind of high melt strength polypropylene for foaming and preparation method thereof
By introducing natural phenol substances and peroxides containing unsaturated double bonds into polypropylene, the high melt strength polypropylene is solved, and the problems of low melt strength and poor foaming performance of polypropylene are achieved. Application and environmentally friendly production process.
Patent Information
- Application Number
- CN202410020148.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-07
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-01-07
AI Technical Summary
Polypropylene's bubble cells are prone to burst and collapse during the extrusion foaming process, the foaming temperature range is narrow, and the melt strength is low, which limits its expansion in the application fields of extrusion foaming, thermoforming and coating.
By mixing polypropylene, peroxide initiator and natural phenolic substances containing unsaturated double bonds in a molten state, high melt strength polypropylene is formed, and free radicals are trapped by double bond grafting and phenolic hydroxyl groups to form branches. chain or crosslinked structure to improve melt strength and foaming properties.
It significantly improves the melt strength and foaming properties of polypropylene, expands its application possibilities in extrusion foaming, thermoforming, coating, blow molding and other fields, and uses biologically sourced natural phenolic substances to avoid contamination. and environmental hazards.
Smart Images

Figure CN117843873B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer material processing, and in particular to high melt strength polypropylene for foaming and a preparation method thereof. Background Art
[0002] Polypropylene (PP) is a general-purpose plastic that has important applications in many industries such as automobiles, electrical appliances, construction, and food packaging. However, polypropylene generally has a linear structure, low molecular weight, narrow molecular weight distribution, low melt strength, and a narrow processing temperature window, which greatly limits the application of polypropylene in other fields such as extrusion foaming, coating, and blow molding. Therefore, the preparation of high melt strength polypropylene (HMSPP) is the key to broadening its application areas. HMSPP has high melt strength and strain hardening during melt stretching, which largely overcomes the problems of cell collapse in linear polypropylene during extrusion foaming, uneven wall thickness in thick-walled containers during thermoforming, and edge curling and shrinkage during extrusion coating calendering.
[0003] There are four main ways to improve the melt strength of polypropylene: 1. Increase the relative molecular weight; 2. Widen the molecular weight distribution of PP; 3. Directly introduce long chain branches on the main chain; 4. Construct a cross-linked structure. Introducing long chain branches or constructing a cross-linked structure can significantly improve the melt strength of polypropylene. The methods commonly used to introduce long chain branches and construct a cross-linked structure are irradiation, direct polymerization, and reactive extrusion. Among them, the reactive extrusion method has the characteristics of simple operation and continuous production. Therefore, this method is often used in industry to prepare high melt strength polypropylene. The principle is to use an initiator in the extruder to induce the PP molecular chain to produce macromolecular free radicals, and branch or cross-link reactions occur with the participation of reactive functional monomers, thereby obtaining high melt strength PP. However, in general, PP will face the problem of degradation during reactive processing, which has a serious negative impact on the performance of PP materials. Therefore, inhibiting the degradation of PP is crucial for the preparation of high melt strength PP.
[0004] Some researchers have shown that by introducing styrene, furan, and thiophene derivatives as comonomers in the PP reactive processing system, the active PP tertiary carbon radicals can be converted into carbon radicals with a resonance-stabilized structure, thereby inhibiting the degradation of PP. The patent (CN202310173532.4) discloses a method for using natural phenolic acids containing unsaturated double bonds as grafting aids to regulate the grafting, degradation, and cross-linking reactions in the reactive processing of maleic anhydride grafted PP. The prepared cross-linked PP can be used as a foaming material, but the foaming performance is poor and the application is limited. Therefore, significantly improving the melt strength of PP to obtain high melt strength PP with excellent foaming performance is still the focus of current research. Summary of the invention
[0005] Based on this, the present invention provides a high melt strength polypropylene for foaming and a preparation method thereof, so as to solve the technical problems in the prior art that the PP melt strength is low, the bubbles are easy to rupture and collapse during the extrusion foaming process, and the foaming temperature range is narrow.
[0006] To achieve the above object, the present invention provides a method for preparing high melt strength polypropylene for foaming, which comprises the following steps:
[0007] The polypropylene, peroxide initiator and natural phenolic substances containing unsaturated double bonds are mixed and added into a mixing device for melt blending at a temperature of 190-200° C., extruded in a molten state, and dried to obtain high melt strength polypropylene for foaming;
[0008] The chemical structure of the double-bonded natural phenolic substance is as follows (1):
[0009]
[0010] In formula (1), R1 is absent or is selected from -OH, -OCH3, and a double bond.
[0011] As a further preferred technical solution of the present invention, by weight percentage: 0.01-0.5wt% peroxide initiator, 0.2-3wt% natural phenolic substance containing unsaturated double bonds, and the balance polypropylene.
[0012] As a further preferred technical solution of the present invention, the peroxide initiator is one or more of diisopropylbenzene oxide, di-tert-butyl peroxide, di-tert-butylperoxyisopropylbenzene, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane, and benzoyl peroxide.
[0013] As a further preferred technical solution of the present invention, the mixing equipment is a twin-screw extruder with a screw speed of 50 r / min.
[0014] As a further preferred technical solution of the present invention, the natural phenolic substance containing unsaturated double bonds is one or a mixture of 4-vinylguaiacol, 4-vinylphenol, styrenated phenol, and 3,4-dihydroxystyrene.
[0015] According to another aspect of the present invention, the present invention also provides a high melt strength polypropylene for foaming, which is prepared by the above method.
[0016] Compared with the prior art, the present invention can achieve the following beneficial effects:
[0017] 1) The natural phenolic substances containing unsaturated double bonds used in the present invention are used as grafting monomers, which are of biological origin, green, environmentally friendly and pollution-free, thus avoiding harm to the human body and the environment;
[0018] 2) The grafting monomer used in the present invention is a natural phenolic substance containing an unsaturated double bond, which has high reactivity and can inhibit the degradation of polypropylene;
[0019] 3) The present invention can obtain a high melt strength PP with branched and cross-linked structure and excellent foaming performance by changing the amount of grafted monomer and initiator added during the melt blending process, thereby providing new possibilities for expanding the application of polypropylene in extrusion foaming, thermoforming, coating, blow molding, etc. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The present invention will be further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0021] Figure 1 The scanning electron microscope images of the products prepared in Comparative Examples 1, 2 and Example 1 after foaming.
[0022] Figure 2 Schematic diagram of the operation of measuring the melt strength of the product using the melt flow rate method.
[0023] Figure 3 The figure is a cross-linking mechanism diagram of a polypropylene system using natural phenolic substances containing unsaturated double bonds of the present invention.
[0024] The purpose, features and advantages of the present invention will be further described with reference to the accompanying drawings in conjunction with the embodiments. DETAILED DESCRIPTION
[0025] The specific implementation of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.
[0026] Unless otherwise defined, the technical terms used in the following examples have the same meanings as those generally understood by those skilled in the art to which the present invention belongs. The test reagents used in the following examples, unless otherwise specified, are all conventional biochemical reagents; the experimental methods, unless otherwise specified, are all conventional methods.
[0027] The innovative idea of the present invention is that the natural phenolic substance containing unsaturated double bonds has multiple (≥2) reactive functional groups (double bonds, phenolic hydroxyl groups), the double bonds of which can be used for grafting, and the phenolic hydroxyl groups can be used to capture free radicals to form a resonance-stabilized structure, which can not only inhibit the degradation of PP during reactive processing, but also introduce a branched chain or a cross-linked structure on the PP molecular chain through the coupling effect between the resonance-stabilized free radicals, thereby improving the melt strength of polypropylene and broadening its application in the fields of extrusion foaming, thermoforming, coating, and film blowing. The chemical structure of the natural phenolic substance containing unsaturated double bonds is as follows (1):
[0028]
[0029] In the molecular structure formula (1), R1 does not exist (i.e., is H), or is selected from one of -OH, -OCH3, and a double bond; depending on the difference in R1, it can be 4-vinylguaiacol (VG), 4-vinylphenol (4-VP), styrenated phenol (SP), or 3,4-dihydroxystyrene (4-Vb).
[0030] In order to enable those skilled in the art to better understand and implement the technical solution of the present invention, the technical solution of the present invention will be further described in detail below through specific embodiments.
[0031] It should be noted that the dicumyl peroxide (DCP), di-tert-butyl peroxide, di-tert-butyl peroxy isopropylbenzene, 2,5-dimethyl-2,5-bis(tert-butylperoxy)hexane and benzoyl peroxide in the present invention are all peroxide initiators commonly used in polypropylene processes. The peroxide initiators in the following comparative examples and embodiments all use dicumyl peroxide (DCP), and the performance of the other peroxide initiators is similar to that of dicumyl oxide, so they are not given one by one here.
[0032] Comparative Example 1: Preparation of PP / VG, wherein the amount of VG added is 0.2 wt % and the balance is polypropylene.
[0033] S1. Dry the polypropylene pellets in a vacuum oven at 80°C overnight;
[0034] S2. The tetravinylguaiacol (VG) was added to the dry polypropylene and mixed at room temperature to obtain a mixture;
[0035] S3. The mixture was added to an internal mixer and melt-blended at 190° C. and a rotation speed of 50 rpm for 10 min to obtain modified polypropylene PP / VG.
[0036] Comparative Example 2: Preparation of PP / DCP / MAH / VG, wherein the addition amount of MAH is 5wt%, the addition amount of VG is 1wt%, the addition amount of peroxide initiator is 0.5wt%, and the balance is polypropylene.
[0037] S1. Dry the polypropylene pellets in a vacuum oven at 80°C overnight;
[0038] S2. adding a peroxide initiator, tetravinylguaiacol (VG), and maleic anhydride (MAH) to dry polypropylene and mixing them uniformly at room temperature to obtain a mixture;
[0039] S3. The mixture was added to an internal mixer and melt-blended at 190° C. and a rotation speed of 50 rpm for 10 min to obtain modified polypropylene PP / DCP / MAH / VG.
[0040] Example 1: Preparation of PP / DCP / VG, wherein the addition amount of VG is 0.2wt%, the addition amount of peroxide initiator is 0.36wt%, and the balance is polypropylene.
[0041] S1. Dry the polypropylene pellets in a vacuum oven at 80°C overnight;
[0042] S2. The peroxide initiator, tetravinylguaiacol (VG) is added to the dry polypropylene, and mixed at room temperature to obtain a mixture;
[0043] S3. The mixture is added to an internal mixer, and melt-blended at 190° C. and a rotation speed of 50 rpm for 10 min to obtain modified polypropylene PP / DCP / VG, that is, the high melt strength polypropylene for foaming of the present invention.
[0044] Example 2: Preparation of PP / DCP / VG, wherein the addition amount of VG is 0.2 wt%, the addition amount of peroxide initiator is 0.28% wt, and the balance is polypropylene.
[0045] S1. Dry the polypropylene pellets in a vacuum oven at 80°C overnight;
[0046] S2. The peroxide initiator, tetravinylguaiacol (VG) is added to the dry polypropylene, and mixed at room temperature to obtain a mixture;
[0047] S3. The mixture is added to an internal mixer, and melt-blended at 190° C. and a rotation speed of 50 rpm for 10 min to obtain modified polypropylene PP / DCP / VG, that is, the high melt strength polypropylene for foaming of the present invention.
[0048] Example 3: Preparation of PP / DCP / VG, wherein the addition amount of VG is 0.2 wt%, the addition amount of peroxide initiator is 0.18% wt, and the balance is polypropylene.
[0049] S1. Dry the polypropylene pellets in a vacuum oven at 80°C overnight;
[0050] S2. The peroxide initiator, tetravinylguaiacol (VG) is added to the dry polypropylene, and mixed at room temperature to obtain a mixture;
[0051] S3. The mixture is added to an internal mixer, and melt-blended at 190° C. and a rotation speed of 50 rpm for 10 min to obtain modified polypropylene PP / DCP / VG, that is, the high melt strength polypropylene for foaming of the present invention.
[0052] Example 4: Preparation of PP / DCP / VG, wherein the addition amount of VG is 0.5wt%, the addition amount of peroxide initiator is 0.5wt%, and the balance is polypropylene.
[0053] S1. Dry the polypropylene pellets in a vacuum oven at 80°C overnight;
[0054] S2. The peroxide initiator and tetravinyl guaiacol (VG) are added to dry polypropylene and mixed at room temperature to obtain a mixture;
[0055] S3. The mixture is added to an internal mixer, and melt-blended at 190° C. and a rotation speed of 50 rpm for 10 min to obtain modified polypropylene PP / DCP / VG, that is, the high melt strength polypropylene for foaming of the present invention.
[0056] Example 5: Preparation of PP / DCP / VG, wherein the addition amount of VG is 1wt%, the addition amount of peroxide initiator is 0.5wt%, and the balance is polypropylene.
[0057] S1. Dry the polypropylene pellets in a vacuum oven at 80°C overnight (drying overnight here may refer to drying for about 12 hours, and of course different drying times may be set according to specific circumstances);
[0058] S2. The peroxide initiator and tetravinyl guaiacol (VG) are added to the dry polypropylene and mixed at room temperature to obtain a mixture;
[0059] S3. The mixture is added to an internal mixer, and melt-blended at 190° C. and a rotation speed of 50 rpm for 10 min to obtain modified polypropylene PP / DCP / VG, that is, the high melt strength polypropylene for foaming of the present invention.
[0060] Example 6: Preparation of PP / DCP / VG, wherein the added amount of VG is 3wt%, the added amount of peroxide initiator is 0.5wt%, and the balance is polypropylene.
[0061] S1. Dry the polypropylene pellets in a vacuum oven at 80°C overnight (drying overnight here may refer to drying for about 12 hours, and of course different drying times may be set according to specific circumstances);
[0062] S2. The peroxide initiator and VG (tetravinyl guaiacol) were added to the dry polypropylene and mixed at room temperature to obtain a mixture;
[0063] S3. The mixture is added to an internal mixer, and melt-blended at 190° C. and a rotation speed of 50 rpm for 10 min to obtain modified polypropylene PP / DCP / VG, that is, the high melt strength polypropylene for foaming of the present invention.
[0064] Example 7: Preparation of PP / DCP / 4-VP, wherein the addition amount of 4-VP is 3wt%, the addition amount of peroxide initiator is 0.5wt%, and the balance is polypropylene.
[0065] S1. Dry the polypropylene pellets in a vacuum oven at 80°C overnight (drying overnight here may refer to drying for about 12 hours, and of course different drying times may be set according to specific circumstances);
[0066] S2. The peroxide initiator and 4-VP (4-vinylphenol) were added to the dry polypropylene and mixed at room temperature to obtain a mixture;
[0067] S3. The mixture is added to an internal mixer and melt-blended at 190° C. and a rotation speed of 50 rpm for 10 min to obtain modified polypropylene PP / DCP / 4-VP, that is, the high melt strength polypropylene for foaming of the present invention.
[0068] Example 8: Preparation of PP / DCP / 4-Vb, wherein the addition amount of 4-Vb is 3wt%, the addition amount of peroxide initiator is 0.5wt%, and the balance is polypropylene.
[0069] S1. Dry the polypropylene pellets in a vacuum oven at 80°C overnight (drying overnight here may refer to drying for about 12 hours, and of course different drying times may be set according to specific circumstances);
[0070] S2. adding a peroxide initiator and 3,4-dihydroxystyrene (4-Vb) to dry polypropylene and mixing them uniformly at room temperature to obtain a mixture;
[0071] S3. The mixture is added to an internal mixer and melt-blended at 190° C. and a rotation speed of 50 rpm for 10 min to obtain modified polypropylene PP / DCP / 4-Vb, that is, the high melt strength polypropylene for foaming of the present invention.
[0072] Performance Test:
[0073] The modified polypropylene samples obtained in the above comparative examples and examples were tested for foaming rate, melt strength, melt flow rate and gel content.
[0074] Foaming rate test: put the modified PP sample into the reactor and heat it to 155 degrees Celsius, keep the pressure for 1 hour, release the pressure and cool it to get the foamed sample, calculate the foaming rate of the foamed sample, and observe its microscopic morphology after foaming with a scanning electron microscope. The results are as follows: Figure 1 shown.
[0075] Melt flow rate measurement: Weigh a certain mass of sample particles to be tested, and use a melt flow rate meter to test the melt flow rate (MFR) of the sample at 230° C. and 2160 g load conditions.
[0076] Melt strength test: The melt flow rate method is used to test the melt strength. The test temperature is 230°C and a 2160g weight is used. After preheating, the weight is loaded and the melt flows out of the die. The melt is allowed to flow downward and solidify under its own gravity. Figure 2 As shown in (a), when the lower end of the melt is flush with the tray, rotate the instrument cutter to cut off the melt column; lay it flat to cool, and 3 melt columns should be cut for each sample to be tested. Lay the melt column flat on the table and follow the Figure 2 As shown in the lower end of (b), take the lower end of the melt column as the origin, make a mark every 1 cm with a marker, and then make marking lines with a marker at intervals of 1 cm, 2 cm, 3 cm, and 4 cm from the origin. Use a micrometer electronic caliper to measure the diameters D0, D1, D2, D3, and D4 of the five points on the marking line, and measure the diameters of two mutually perpendicular lines at each point to find the average value to prevent the melt column from becoming elliptical when cooled. Use Origin software to plot the average diameter and length, and draw a fitting curve. In the origin software, find ΔL through data fitting, which is the length of the melt column corresponding to the general reduction in the melt diameter.
[0077]
[0078] MS- melt strength of the sample, Pa.s (Pa.s)
[0079] ΔL-The length of the melt column when the diameter is reduced to half of the origin (mm)
[0080] D0-diameter of the sample melt column at the origin (mm)
[0081] MFR-melt flow rate (g / 10min)
[0082] Gel content test: Weigh a certain mass of modified PP and put it into a 200-mesh copper mesh. Use xylene to perform Soxhlet extraction for 72 hours, then dry it, and calculate the gel content in the sample by weighing method.
[0083] The above test results are shown in Table 1.
[0084] Table 1
[0085]
[0086] It can be seen from Table 1 that the introduction of natural phenolic substances containing unsaturated double bonds can inhibit the degradation of macromolecular PP matrix during reactive processing, and significantly improve the melt strength and foaming rate of the sample. In addition, by changing the addition amount of natural phenolic substances containing unsaturated double bonds, effective regulation of the degree of degradation and crosslinking of the PP matrix can be achieved. By comparing the scanning electron microscope, it is found that under the same component addition condition, uniform-sized pores can be observed in Example 5, while only a small amount of pores in Comparative Example 1 are small and uneven in size, which is caused by the weak melt strength of Comparative Example 1 itself; No pore structure is observed in Comparative Example 2. It can be seen from Table 1 that Comparative Example 2 has a higher melt index, which may be due to the introduction of MAH, which can react with the phenolic hydroxyl groups of VG used to capture free radicals and inhibit the degradation of the PP matrix, thereby causing its degradation to be more serious, so the melt strength is greatly reduced and it cannot be foamed. Based on Comparative Example 2, the inventors conducted a large number of experiments and still could not achieve foaming by adjusting the types and ratios of natural phenolic substances containing unsaturated double bonds (such as 4-vinylguaiacol, 4-vinylphenol, styrenated phenol, 3,4-dihydroxystyrene).
[0087] The natural phenolic substances containing unsaturated double bonds in the present invention can significantly improve the melt strength of PP, which specifically includes the following mechanisms: on the one hand, the natural phenolic substances containing unsaturated double bonds are grafted onto the polypropylene molecular chain through double bonds; on the other hand, the phenolic hydroxyl groups thereof capture free radicals in the system to form a resonance-stabilized structure, and couple with another stable macromolecular free radical in the system to form a branched or cross-linked structure, thereby significantly improving the melt strength of PP. The branching and cross-linking mechanisms are as follows: Figure 3 shown.
[0088] Although specific embodiments of the present invention are described above, those skilled in the art should understand that these are merely examples and that various changes or modifications may be made to the embodiments without departing from the principles and essence of the present invention. The scope of protection of the present invention is limited only by the appended claims.
Claims
1. A method for preparing high melt strength polypropylene for foaming, It is characterized in that The following steps are involved: The polypropylene, peroxide initiator and natural phenolic substance containing unsaturated double bonds are mixed and added into a mixing device for melt blending at a temperature of 190-200°C, extruded in a molten state, and dried to obtain high melt strength polypropylene for foaming; the amount of each component is as follows by weight percentage: 0.5 wt % of peroxide initiator, 0.5 wt % of natural phenolic substance containing unsaturated double bonds, and the balance of polypropylene; The natural phenolic substance is 4-vinylguaiacol.
2. The method for preparing high melt strength polypropylene for foaming according to claim 1, It is characterized in that The peroxide initiator is one or more of dicumyl peroxide, di-tert-butyl peroxide and benzoyl peroxide.
3. The method for preparing high melt strength polypropylene for foaming according to claim 1, It is characterized in that The mixing equipment is a twin-screw extruder with a screw speed of 50 r / min.
4. A high melt strength polypropylene for foaming, It is characterized in that The method is prepared by any one of claims 1 to 3.