A method for preparing a renewable injection molding grade TPV material for automotive applications

By using renewable PP, EPDM, and paraffin oil as raw materials, combined with a process involving vulcanizing agents and deodorizing agents, a renewable TPV material with excellent aging resistance and low odor was prepared. This solved the problems of dependence on fossil resources and insufficient material performance, and enabled the industrial application of renewable TPV materials.

CN117844125BActive Publication Date: 2026-11-10NINGBO XINTAI MACHINERY +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202311735450.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-12-18
Publication Date
2026-11-10
Estimated Expiration
2043-12-18

AI Technical Summary

Technical Problem

The raw materials for existing TPV materials mainly come from fossil resources, which leads to serious environmental pollution. Furthermore, the application of renewable materials in TPV materials is limited by the availability of raw materials, poor aging performance, and strong odor, making it difficult to meet the performance requirements of automotive TPV materials.

Method used

Using renewable PP, EPDM and paraffin oil as the main raw materials, combined with vulcanizing agents, composite stabilizers and deodorizing agents, a process of dynamic vulcanization, vacuum devolatilization and drying deodorization is used to prepare renewable injection molding grade TPV material with excellent aging resistance and low odor.

Benefits of technology

It significantly improves the aging resistance of TPV materials, reduces odor, realizes the industrial application of renewable TPV materials, and meets the performance requirements of automotive TPV materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The application belongs to the technical field of high polymer materials, and particularly relates to a preparation method of a renewable injection molding grade TPV material for automobiles. The preparation method of the renewable injection molding grade TPV material for automobiles comprises the following steps: (1) feeding renewable PP, EPDM and color master particles into a double-screw extruder, then injecting paraffin oil into the screw, and mixing and granulating to obtain a semi-finished master batch; (2) feeding the semi-finished master batch, a vulcanizing agent, a composite stabilizer and a deodorizing agent into a double-screw extruder, dynamically vulcanizing, vacuum devolatilizing, then extruding and granulating to obtain finished particles, and then drying and deodorizing. The renewable PP, the EPDM, the color master particles and the paraffin oil are used to obtain the semi-finished master batch, and then the vulcanizing agent, the deodorizing agent and other additives are combined to extrude and granulate to obtain the renewable injection molding grade TPV material for automobiles, which has excellent aging resistance and small odor.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of polymer materials technology, specifically relating to a method for preparing a renewable injection-molding grade TPV material for automobiles. Background Technology

[0002] With the advancement of industrial development, the processing methods in the automotive parts industry have become increasingly sophisticated. Thermoplastic vulcanizate (TPV) can be blow-molded to varying degrees, offering advantages such as high efficiency, continuous production, and versatility. It also possesses excellent elasticity, weather resistance, low-temperature resistance, aging resistance, flexural strength, and resistance to ozone and chemicals. Products derived from TPV through extrusion or injection molding are already quite common. However, currently, most TPV raw materials are derived from fossil resources. Given the increasingly severe fossil resource and environmental issues, major OEMs such as Volkswagen and BMW have set corresponding targets. Renewable materials, with their advantages of low pollution, recyclability, and energy conservation and emission reduction, have gained favor among automakers. Simultaneously, some OEMs (such as Volvo) have also set corresponding targets for renewable materials. Therefore, the development of renewable TPV materials has become a future trend in TPV research and development.

[0003] In recent years, many universities and enterprises have carried out research and development on renewable materials, such as PCR PP, PCR PP+GF20 / 30, and PCR PC. However, these renewable materials are only used in the field of plastics and rarely in TPV materials. The reasons for this are mainly twofold: firstly, the renewable materials currently developed are not entirely suitable for the preparation process of TPV materials; secondly, the shortcomings of renewable materials, such as poor raw material availability, poor aging performance, and strong odor, limit their application in automotive TPV materials. Summary of the Invention

[0004] The purpose of this invention is to address the above-mentioned technical problems by providing a method for preparing a renewable injection-molded TPV material for automobiles, which can significantly improve the aging resistance of TPV materials and reduce the odor of the materials, thereby obtaining a renewable injection-molded TPV material.

[0005] The preparation method of automotive renewable injection molding grade TPV material in the technical solution of this invention includes the following steps:

[0006] (1) Feed renewable PP, EPDM and color masterbatch into a twin-screw extruder, then inject paraffin oil into the screw, mix and granulate to obtain semi-finished masterbatch;

[0007] (2) The semi-finished masterbatch, vulcanizing agent, composite stabilizer and deodorizing agent are fed into a twin-screw extruder, dynamically vulcanized and vacuum devoured, then extruded and granulated to obtain finished particles, and then dried and deodorized.

[0008] By using high-quality renewable PP material to replace conventional petroleum-based PP material, energy conservation and emission reduction are achieved, which is conducive to the realization of the goal. At the same time, antioxidants are added to improve the aging resistance of TPV material, and deodorizing agents are added to reduce the odor of TPV material through vacuum volatilization. The resulting renewable TPV material meets the performance requirements of automotive TPV material and also helps to realize the industrial application of renewable TPV material.

[0009] Furthermore, in step (1), the amounts of renewable PP, EPDM, paraffin oil and color masterbatch particles added are 10-35 parts, 25-50 parts, 35-50 parts and 1-5 parts, respectively.

[0010] Preferably, in step (1), the paraffin oil is heated to 80-120°C by a mold temperature controller.

[0011] Furthermore, the temperature during the mixing and granulation process in the twin-screw extruder in step (1) is 200–250°C.

[0012] Furthermore, in step (2), the amounts of semi-finished masterbatch, vulcanizing agent, composite stabilizer, and deodorizing agent added are 90-95 parts, 1-10 parts, 1-5 parts, and 2-10 parts, respectively.

[0013] Furthermore, the vulcanizing agent is one or more of peroxide vulcanizing agents, quinone vulcanizing agents, and amine vulcanizing agents, preferably a peroxide vulcanizing agent.

[0014] Furthermore, the composite stabilizer is a mixture of hindered phenolic antioxidants and hindered amine light stabilizers in a mass ratio of 5–7:3–5.

[0015] Hindered phenolic antioxidants can capture free radicals, generating free radical-producing peroxides ROOR and ROOH. Hindered amine light stabilizers can deactivate ROOR and ROOH, preventing further thermal decomposition or photolysis to generate free radicals, thereby improving the aging resistance of TPV materials. Simultaneously, the transition product alkyl hydroxylamine of hindered amine light stabilizers can react with phenoxy radicals, regenerating the hindered phenols and generating a high concentration of nitroxy radicals under thermo-oxidative aging conditions. When exerting a stabilizing effect, alkyl hydroxylamine is generated, which, through pyrolysis or reaction with peroxy radicals, regenerates nitroxy radicals, allowing the composite stabilizer to exert a longer-lasting stabilizing effect, further improving the aging resistance of TPV materials. Preferably, the hindered phenolic antioxidants include, but are not limited to, one or more of 2,6-di-tert-butyl-4-methylphenol, antioxidant 1010, and antioxidant 1076.

[0016] Furthermore, the deodorizing agent is one or more of the following: compound amine deodorizing agent, phenolic deodorizing agent, adsorbent deodorizing agent, masking deodorizing agent, oxidizing deodorizing agent, and metal salt deodorizing agent.

[0017] Furthermore, the deodorizing agent is a mixture of an adsorbent deodorizing agent and a masking deodorizing agent in a mass ratio of 1 to 2: 1 to 2.

[0018] Preferably, the adsorbent deodorizer includes, but is not limited to, one or more of activated carbon, bamboo charcoal, and coconut fiber charcoal.

[0019] Preferably, the masking and deodorizing agent includes, but is not limited to, one or more of aromatic oils, geraniol, nerol, and ionone.

[0020] Furthermore, in step (2), the length-to-diameter ratio of the twin-screw extruder is 80 to 100:1, and the main engine speed is 200 to 400 rpm / min.

[0021] Furthermore, in step (2), the melting temperature of dynamic vulcanization is 250–300°C, and the time is 1–2 min.

[0022] Furthermore, vacuum devolatilization is carried out using a vacuum pump connected to the screw of a twin-screw extruder.

[0023] By adding an odor-removing agent and combining it with vacuum volatilization treatment, the odor in the TPV material is adsorbed by the odor-removing agent and then removed by vacuum volatilization, thus reducing the odor of the TPV material.

[0024] Furthermore, the drying and deodorization process involves maintaining the temperature at 80–100℃ for 3–5 hours.

[0025] The present invention also provides a renewable injection-molded TPV material for automobiles, which is prepared by the above-mentioned preparation method of renewable injection-molded TPV material for automobiles.

[0026] Compared with the prior art, the technical solution of the present invention has the following beneficial effects:

[0027] (1) The present invention first obtains a semi-finished masterbatch from renewable PP, EPDM, color masterbatch particles and paraffin oil, and then combines it with vulcanizing agent, deodorizing agent and other additives, and extrudes and granulates it to obtain automotive renewable injection molding grade TPV material with excellent aging resistance and low odor.

[0028] (2) The hindered phenolic antioxidant and the hindered amine light stabilizer are combined to form a composite stabilizer, which plays a good stabilizing role over a long period of time and improves the aging resistance of TPV materials.

[0029] (3) By adding deodorizing agent and combining it with vacuum devolatilization treatment, the odor of automotive renewable injection molding grade TPV material is greatly reduced.

[0030] (4) Using renewable PP and EPDM as matrix materials, combined with other additives, the raw materials are renewable, and energy saving and emission reduction are achieved, which helps to obtain renewable TPV materials.

[0031] (5) The preparation method of the renewable injection-molded TPV material for automobiles of the present invention is simple and easy to operate, and is suitable for large-scale industrial application. Detailed Implementation

[0032] The technical solution of the present invention will be further described and illustrated below through specific embodiments. It should be understood that the specific embodiments described herein are only for the purpose of helping to understand the present invention and are not intended to limit the present invention. Unless otherwise specified, the raw materials used in the embodiments of the present invention are all commonly used raw materials in the art, and the methods used in the embodiments are all conventional methods in the art.

[0033] Example 1

[0034] The preparation method of automotive renewable injection molding grade TPV material in this embodiment includes the following steps:

[0035] (1) 18 parts of renewable PP, 35 parts of EPDM and 2 parts of color masterbatch are fed into a twin-screw extruder, and then 45 parts of paraffin oil heated to 100°C by a mold temperature controller are injected into the screw. The mixture is granulated at 230°C to obtain a semi-finished masterbatch.

[0036] (2) 90 parts of semi-finished masterbatch, 4 parts of dicumyl peroxide, 2 parts of composite stabilizer (2,6-di-tert-butyl-4-methylphenol and hindered amine light stabilizer mixed at a mass ratio of 6:4) and 4 parts of deodorizing agent (activated carbon and aromatic oil mixed at a mass ratio of 1:1) are fed into a twin-screw extruder. The length-to-diameter ratio of the twin-screw extruder is 90:1, the main engine speed is 300 rpm / min, dynamic vulcanization is performed at 260℃ for 2 min, vacuum devolatilization is performed by vacuum pump connected to the screw of the twin-screw extruder, and the finished particles are extruded and granulated. Then, the particles are dried and deodorized by keeping them at 80℃ for 3 h.

[0037] Example 2

[0038] The preparation method of automotive renewable injection molding grade TPV material in this embodiment includes the following steps:

[0039] (1) 20 parts of renewable PP, 30 parts of EPDM and 3 parts of color masterbatch are fed into a twin-screw extruder, and then 40 parts of paraffin oil heated to 100°C by a mold temperature controller are injected into the screw. The mixture is granulated at 235°C to obtain a semi-finished masterbatch.

[0040] (2) 92 parts of semi-finished masterbatch, 6 parts of dicumyl peroxide, 3 parts of composite stabilizer (antioxidant 1010 and hindered amine light stabilizer mixed at a mass ratio of 6:4) and 6 parts of deodorizing agent (activated carbon and geraniol mixed at a mass ratio of 1:1) were fed into a twin-screw extruder. The length-to-diameter ratio of the twin-screw extruder was 90:1, the main engine speed was 300 rpm / min, and dynamic vulcanization was carried out at 270℃ for 2 min. Vacuum devolatilization was carried out by a vacuum pump connected to the screw of the twin-screw extruder. The finished particles were extruded and granulated, and then dried and deodorized at 85℃ for 3 h.

[0041] Example 3

[0042] The preparation method of automotive renewable injection molding grade TPV material in this embodiment includes the following steps:

[0043] (1) 25 parts of renewable PP, 40 parts of EPDM and 5 parts of color masterbatch are fed into a twin-screw extruder, and then 35 parts of paraffin oil heated to 100°C by a mold temperature controller are injected into the screw. The mixture is granulated at 240°C to obtain a semi-finished masterbatch.

[0044] (2) 95 parts of semi-finished masterbatch, 8 parts of dicumyl peroxide, 4 parts of composite stabilizer (antioxidant 1076 and hindered amine light stabilizer mixed at a mass ratio of 6:4) and 8 parts of deodorizer (coconut charcoal and aromatic oil mixed at a mass ratio of 1:1) were fed into a twin-screw extruder. The length-to-diameter ratio of the twin-screw extruder was 90:1, the main engine speed was 300 rpm / min, and dynamic vulcanization was carried out at 280℃ for 2 min. Vacuum devolatilization was carried out by a vacuum pump connected to the screw of the twin-screw extruder. The finished particles were extruded and granulated, and then dried and deodorized at 90℃ for 3 h.

[0045] Example 4

[0046] The difference between this embodiment and Example 1 is only in step (2): 90 parts of semi-finished masterbatch, 4 parts of dicumyl peroxide, 2 parts of composite stabilizer (2,6-di-tert-butyl-4-methylphenol and hindered amine light stabilizer mixed in a mass ratio of 5:5), and 4 parts of deodorizer (activated carbon and aromatic oil mixed in a mass ratio of 1:2) are fed into a twin-screw extruder. The length-to-diameter ratio of the twin-screw extruder is 90:1, the main engine speed is 300 rpm / min, dynamic vulcanization is performed at 260℃ for 2 min, vacuum devolatilization is performed by a vacuum pump connected to the screw of the twin-screw extruder, and the finished particles are extruded and granulated. Then, the particles are dried and deodorized by keeping them at 80℃ for 3 h.

[0047] Example 5

[0048] The difference between this embodiment and Example 1 is only in step (2): 90 parts of semi-finished masterbatch, 4 parts of dicumyl peroxide, 2 parts of composite stabilizer (2,6-di-tert-butyl-4-methylphenol and hindered amine light stabilizer mixed at a mass ratio of 7:3), and 4 parts of deodorizer (activated carbon and aromatic oil mixed at a mass ratio of 2:1) are fed into a twin-screw extruder. The length-to-diameter ratio of the twin-screw extruder is 90:1, the main engine speed is 300 rpm / min, dynamic vulcanization is performed at 260℃ for 2 min, vacuum devolatilization is performed by a vacuum pump connected to the screw of the twin-screw extruder, extrusion granulation is performed to obtain finished particles, and then drying and deodorizing are carried out at 80℃ for 3 h.

[0049] Example 6

[0050] The difference between this embodiment and embodiment 1 is only in step (1) feeding 5 parts of renewable PP, 48 parts of EPDM and 2 parts of color masterbatch into a twin-screw extruder, and then injecting 45 parts of paraffin oil heated to 100°C by a mold temperature controller into the screw, and mixing and granulating at 230°C to obtain a semi-finished masterbatch.

[0051] Example 7

[0052] The difference between this embodiment and embodiment 1 is only in step (1): 40 parts of renewable PP, 25 parts of EPDM and 2 parts of color masterbatch are fed into a twin-screw extruder, and then 45 parts of paraffin oil heated to 100°C in a mold temperature controller are injected into the screw. The mixture is then granulated at 230°C to obtain a semi-finished masterbatch.

[0053] Example 8

[0054] The difference between this embodiment and Example 1 is only in step (2): 90 parts of semi-finished masterbatch, 4 parts of dicumyl peroxide, 0.5 parts of composite stabilizer (2,6-di-tert-butyl-4-methylphenol and hindered amine light stabilizer mixed at a mass ratio of 6:4) and 4 parts of deodorizer (activated carbon and aromatic oil mixed at a mass ratio of 1:1) are fed into a twin-screw extruder. The length-to-diameter ratio of the twin-screw extruder is 90:1, the main engine speed is 300 rpm / min, dynamic vulcanization is performed at 260℃ for 2 min, vacuum devolatilization is performed by a vacuum pump connected to the screw of the twin-screw extruder, extrusion granulation is performed to obtain finished particles, and then drying and deodorizing are carried out at 80℃ for 3 h.

[0055] Example 9

[0056] The difference between this embodiment and Example 1 is only in step (2): 90 parts of semi-finished masterbatch, 4 parts of dicumyl peroxide, 6.0 parts of composite stabilizer (2,6-di-tert-butyl-4-methylphenol and hindered amine light stabilizer mixed in a mass ratio of 6:4) and 4 parts of deodorizer (activated carbon and aromatic oil mixed in a mass ratio of 1:1) are fed into a twin-screw extruder. The length-to-diameter ratio of the twin-screw extruder is 90:1, the main engine speed is 300 rpm / min, dynamic vulcanization is performed at 260℃ for 2 min, vacuum devolatilization is performed by a vacuum pump connected to the screw of the twin-screw extruder, extrusion granulation is performed to obtain finished particles, and then drying and deodorizing are carried out at 80℃ for 3 h.

[0057] Example 10

[0058] The difference between this embodiment and Example 1 is only in step (2): 90 parts of semi-finished masterbatch, 4 parts of dicumyl peroxide, 2 parts of composite stabilizer (2,6-di-tert-butyl-4-methylphenol and hindered amine light stabilizer mixed at a mass ratio of 6:4), and 1 part of deodorizer (activated carbon and aromatic oil mixed at a mass ratio of 1:1) are fed into a twin-screw extruder. The length-to-diameter ratio of the twin-screw extruder is 90:1, the main engine speed is 300 rpm / min, dynamic vulcanization is performed at 260℃ for 2 min, vacuum devolatilization is performed by a vacuum pump connected to the screw of the twin-screw extruder, and the finished particles are extruded and granulated. Then, the particles are dried and deodorized by keeping them at 80℃ for 3 h.

[0059] Example 11

[0060] The difference between this embodiment and Example 1 is only in step (2): 90 parts of semi-finished masterbatch, 4 parts of dicumyl peroxide, 2 parts of composite stabilizer (2,6-di-tert-butyl-4-methylphenol and hindered amine light stabilizer mixed at a mass ratio of 6:4), and 12 parts of deodorizer (activated carbon and aromatic oil mixed at a mass ratio of 1:1) are fed into a twin-screw extruder. The length-to-diameter ratio of the twin-screw extruder is 90:1, the main engine speed is 300 rpm / min, dynamic vulcanization is performed at 260℃ for 2 min, vacuum devolatilization is performed by a vacuum pump connected to the screw of the twin-screw extruder, and the finished particles are extruded and granulated. Then, the particles are dried and deodorized by keeping them at 80℃ for 3 h.

[0061] Comparative Example 1

[0062] The only difference between this comparative example and Example 1 is that in step (2), 90 parts of semi-finished masterbatch, 4 parts of dicumyl peroxide, 2 parts of 2,6-di-tert-butyl-4-methylphenol, and 4 parts of deodorizing agent (activated carbon and aromatic oil mixed in a mass ratio of 1:1) are fed into a twin-screw extruder. The length-to-diameter ratio of the twin-screw extruder is 90:1, the main engine speed is 300 rpm / min, dynamic vulcanization is performed at 260°C for 2 min, vacuum devolatilization is performed by a vacuum pump connected to the screw of the twin-screw extruder, and the finished particles are extruded and granulated. Then, the particles are dried and deodorized by keeping them at 80°C for 3 h.

[0063] Comparative Example 2

[0064] The only difference between this comparative example and Example 1 is that in step (2), 90 parts of semi-finished masterbatch, 4 parts of dicumyl peroxide, 2 parts of hindered amine light stabilizer, and 4 parts of deodorizer (activated carbon and aromatic oil mixed in a mass ratio of 1:1) are fed into a twin-screw extruder. The length-to-diameter ratio of the twin-screw extruder is 90:1, the main engine speed is 300 rpm / min, dynamic vulcanization is performed at 260°C for 2 min, vacuum devolatilization is performed by a vacuum pump connected to the screw of the twin-screw extruder, and the finished particles are extruded and granulated. Then, the particles are dried and deodorized by keeping them at 80°C for 3 h.

[0065] Comparative Example 3

[0066] The only difference between this comparative example and Example 1 is that in step (2), 90 parts of semi-finished masterbatch, 4 parts of dicumyl peroxide, 2 parts of composite stabilizer (2,6-di-tert-butyl-4-methylphenol and hindered amine light stabilizer mixed at a mass ratio of 6:4) and 4 parts of deodorizer (activated carbon and aromatic oil mixed at a mass ratio of 1:1) are fed into a twin-screw extruder. The length-to-diameter ratio of the twin-screw extruder is 90:1, the main engine speed is 300 rpm / min, dynamic vulcanization is performed at 260℃ for 2 min, extrusion granulation is performed to obtain finished particles, and then drying and deodorizing are carried out at 80℃ for 3 h.

[0067] The mechanical properties of the TPV materials obtained in the above examples and comparative examples were tested: Shore hardness (15s) (ISO868:2003(E)); tensile strength (ISO 37:2017(E), 500mm / min); elongation at break (ISO 37:2017(E), type 1 dumbbell type, 500mm / min); melt flow index (ISO 1133-1:2022(E), 230℃*5kg). The test results are shown in Table 1.

[0068] Table 1. Mechanical Properties of TPV Materials

[0069]

[0070] The automotive-grade renewable injection-molding TPV materials obtained in Examples 1-5 exhibited excellent mechanical properties and low odor. In Example 6, the addition of a small amount of renewable PP significantly reduced the hardness of the final product, resulting in poorer mechanical properties. In Example 7, the addition of excessive renewable PP significantly increased the hardness of the final product; however, since renewable PP is the primary source of odor, the excessive addition resulted in a high odor level in the final product. Furthermore, the poor performance stability of renewable PP and its excessive addition also led to suboptimal weather resistance. In Example 8, the insufficient addition of composite stabilizer resulted in poor weather resistance stability of the TPV material, making it difficult to meet weathering requirements. In Example 9, the excessive addition of composite stabilizer caused it to slowly precipitate from the surface during weathering tests, making it difficult to meet the grayscale requirements of the weathering tests. Example 10: Insufficient deodorizer dosage resulted in incomplete adsorption of odors during processing, leading to a strong odor in the final TPV material. Example 11: Excessive deodorizer dosage resulted in incomplete adsorption of the deodorizer's own odor, also leading to a strong odor in the final TPV material. Comparative Example 1: Only hindered phenolic antioxidants were added, without hindered amine light stabilizers. The lack of synergistic effect of hindered amine light stabilizers resulted in the final TPV material failing to meet weather resistance requirements. Comparative Example 2: Only hindered amine light stabilizers were added, without hindered phenolic antioxidants. The final TPV material also failed to meet weather resistance requirements. Comparative Example 3: No vacuum devolatilization was performed, resulting in the inability to adsorb and remove gases during processing, leading to a strong odor in the final TPV material.

[0071] Finally, it should be noted that the specific embodiments described herein are merely illustrative of the spirit of the invention and are not intended to limit the implementation of the invention. Those skilled in the art can make various modifications or additions to the described embodiments or use similar methods to replace them; it is neither necessary nor possible to exemplify all embodiments here. However, these obvious variations or modifications derived from the essential spirit of the invention still fall within the scope of protection of the invention, and interpreting them as any additional limitation would contradict the spirit of the invention.

Claims

1. A method for preparing a renewable injection-molding grade TPV material for automobiles, characterized in that, Includes the following steps: (1) Feed renewable PP, EPDM and color masterbatch into a twin-screw extruder, then inject paraffin oil into the screw, mix and granulate to obtain semi-finished masterbatch; (2) The semi-finished masterbatch, vulcanizing agent, composite stabilizer and deodorizing agent are fed into a twin-screw extruder, dynamically vulcanized and vacuum devoured, then extruded and granulated to obtain finished particles, and then dried and deodorized. In step (1), the amounts of renewable PP, EPDM, paraffin oil and color masterbatch particles added are 10~35 parts, 25~50 parts, 35~50 parts and 1~5 parts, respectively; In step (2), the amount of semi-finished masterbatch added to vulcanizing agent, composite stabilizer and deodorizing agent is 90~95 parts, 1~10 parts, 1~5 parts and 2~10 parts respectively; The composite stabilizer is a mixture of hindered phenolic antioxidants and hindered amine light stabilizers in a mass ratio of 5~7:3~5; The deodorizing agent is a mixture of an adsorbent deodorizing agent and a masking deodorizing agent in a mass ratio of 1~2:1~2; The regenerable PP is PCR PP; The dynamic vulcanization process involves melting at 250-300℃ for 1-2 minutes; the drying and deodorization process involves holding the product at 80-100℃ for 3-5 hours. The hindered phenolic antioxidant can capture free radicals and generate peroxides ROOR and ROOH. The hindered amine light stabilizer deactivates ROOR and ROOH. The transition product alkyl hydroxylamine of the hindered amine light stabilizer reacts with phenolic oxygen free radicals to regenerate the hindered phenol, enabling the composite stabilizer to exert a long-term stabilizing effect. The odor in the TPV material is adsorbed by the deodorizing agent and then removed through vacuum volatilization.

2. The preparation method according to claim 1, characterized in that, In step (2), vacuum devouring is performed by a vacuum pump connected to the screw of a twin-screw extruder.

3. A renewable injection-molding grade TPV material for automotive applications, characterized in that, It is prepared by the preparation method described in claim 1.

Citation Information

Patent Citations

  • Thermoplastic dynamic vulcanized rubber and preparation method thereof

    CN110256770A

  • Low-odor TPV material and preparation method thereof

    CN117209903A