A coking wastewater treatment agent and preparation method thereof

By subjecting natural seaweed powder to microwave-ultrasonic collaborative treatment and cross-linking with ceramic powder and other materials, an efficient coking wastewater treatment agent is prepared, which solves the problem of ineffective removal of aromatic compounds in coking wastewater in the existing technology. It solves the problem of secondary pollution and achieves effective water purification.

CN117861628BActive Publication Date: 2024-10-22SHANDONG BAODING COAL COKING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410025484.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-08
Publication Date
2024-10-22
Estimated Expiration
2044-01-08

AI Technical Summary

Technical Problem

Existing wastewater treatment agents are not effective in removing aromatic compounds such as phenol and aniline from coking wastewater, and there are secondary pollution problems.

Method used

A coking wastewater treatment agent is prepared by using natural seaweed powder through microwave-ultrasonic collaborative treatment, heating and stirring, vacuum distillation and grinding with ceramic powder, cross-linking agent and antioxidant.

Benefits of technology

This treatment agent has a good removal effect on aromatic compounds such as phenol and aniline in coking wastewater without secondary pollution, and provides a new method for coking wastewater treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004654290950000071
    Figure BDA0004654290950000071
  • Figure BDA0004654290950000081
    Figure BDA0004654290950000081
Patent Text Reader

Abstract

The present invention relates to a coking wastewater treatment agent and a preparation method thereof, and to the technical field of wastewater treatment. The preparation method comprises the following steps: placing dry laver powder in a microwave-ultrasonic composite field for microwave-ultrasonic coordinated treatment to obtain modified laver powder; adding the modified laver powder, ceramic powder, a cross-linking agent and an antioxidant to a solvent for heating and stirring, and then cooling to room temperature to obtain a first mixture; performing reduced pressure distillation on the first mixture, and then drying and grinding to obtain the coking wastewater treatment agent. The present invention uses natural laver as a raw material for the first time and performs microwave-ultrasonic coordinated treatment, and then performs cross-linking treatment on the obtained modified laver powder and ceramic powder to obtain a natural coking wastewater treatment agent. The coking wastewater treatment agent has a good removal effect on aromatic compounds such as phenol and aniline in coking wastewater, and there is no secondary pollution, which provides a new means for coking wastewater treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wastewater treatment, and in particular to a coking wastewater treatment agent and a preparation method thereof. Background Art

[0002] Coking wastewater mainly comes from the primary cooling of coke oven gas and the production water and steam condensation wastewater in the coking production process. It is the wastewater generated in the process of coal coking, gas purification, chemical product recovery and chemical product refining. It is a typical toxic and difficult to degrade organic wastewater. There are many kinds of pollutants in coking wastewater with complex components. The organic pollutants contained in it are mainly in the form of aromatic compounds such as phenol and aniline. These substances are difficult to degrade, which not only seriously inhibits the growth and normal metabolic activities of microorganisms, but also causes serious pollution to water bodies; they are also carcinogenic and cause great harm to human health.

[0003] At present, the treatment methods of industrial wastewater mainly include: flocculation, membrane filtration, catalytic oxidation, biological method, adsorption method, etc. Among them, the adsorption method mainly uses adsorbent materials as wastewater treatment agents to adsorb and remove pollutants in the water to purify the water quality. It has the advantages of simple treatment and low cost and is widely used. However, the existing wastewater treatment agents are not effective in removing aromatic compounds such as phenol and aniline in coking wastewater, and there are problems such as secondary pollution. Summary of the invention

[0004] In order to solve the above problems, the present invention provides a coking wastewater treatment agent and a preparation method thereof.

[0005] In a first aspect, the present invention provides a method for preparing a coking wastewater treatment agent, the preparation method comprising the following steps:

[0006] placing the dried laver powder in a microwave-ultrasonic composite field for microwave-ultrasonic coordinated treatment to obtain modified laver powder;

[0007] Adding the modified laver powder, ceramic powder, cross-linking agent and antioxidant into a solvent, heating and stirring, and then cooling to room temperature to obtain a first mixed material;

[0008] The first mixed material is subjected to reduced pressure distillation, and then dried and ground to obtain the coking wastewater treatment agent.

[0009] Furthermore, the working parameters of the microwave-ultrasonic coordinated processing include: microwave power of 520-600W, ultrasonic power of 300-450W, and processing time of 25-40s.

[0010] Furthermore, the working parameters of the microwave-ultrasonic coordinated processing include: microwave power of 560W, ultrasonic power of 380W, and processing time of 35s.

[0011] Furthermore, the weight ratio of the modified laver powder, the ceramic powder, the cross-linking agent, the antioxidant and the solvent is 100:(10-15):(1-5):(0.01-0.05):(45-55).

[0012] Furthermore, the cross-linking agent includes at least one of dicumyl peroxide and dibenzoyl tert-butyl peroxide.

[0013] Furthermore, the antioxidant includes at least one of 2,6-di-tert-butyl-4-methylphenol and tris(2,4-di-tert-butylphenyl)phosphite.

[0014] Further, the solvent includes at least one of xylene and toluene.

[0015] Furthermore, the working parameters of the heating and stirring include: a temperature of 65 to 75° C. and a time of 1 to 3 hours.

[0016] Furthermore, the grinding working parameters include: a grinding speed of 500 to 700 rpm and a grinding time of 20 to 35 minutes.

[0017] In a second aspect, the present invention provides a coking wastewater treatment agent, which is prepared by the preparation method described in any one of the first aspects.

[0018] The above technical solution provided by the present invention has at least the following advantages compared with the prior art:

[0019] The invention provides a method for preparing a coking wastewater treatment agent. The invention uses natural laver as a raw material for the first time and performs microwave-ultrasonic coordinated treatment, then cross-links the obtained modified laver powder and ceramic powder to prepare a natural coking wastewater treatment agent. The coking wastewater treatment agent has a good removal effect on aromatic compounds such as phenol, aniline, etc. in the coking wastewater, and has no secondary pollution, thereby providing a new means for coking wastewater treatment. DETAILED DESCRIPTION

[0020] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described in combination with the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0021] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods.

[0022] In a first aspect, the present invention provides a method for preparing a coking wastewater treatment agent, the preparation method comprising the following steps:

[0023] placing the dried laver powder in a microwave-ultrasonic composite field for microwave-ultrasonic coordinated treatment to obtain modified laver powder;

[0024] Adding the modified laver powder, ceramic powder, cross-linking agent and antioxidant into a solvent, heating and stirring, and then cooling to room temperature to obtain a first mixed material;

[0025] The first mixed material is subjected to reduced pressure distillation, and then dried and ground to obtain the coking wastewater treatment agent.

[0026] The invention provides a method for preparing a coking wastewater treatment agent. The invention uses natural laver as a raw material for the first time and performs microwave-ultrasonic coordinated treatment, then cross-links the obtained modified laver powder and ceramic powder to prepare a natural coking wastewater treatment agent. The coking wastewater treatment agent has a good removal effect on aromatic compounds such as phenol, aniline, etc. in the coking wastewater, and has no secondary pollution, thereby providing a new means for coking wastewater treatment.

[0027] In some specific embodiments, the working parameters of the microwave-ultrasonic coordinated treatment include: microwave power of 520-600 W, ultrasonic power of 300-450 W, and treatment time of 25-40 s.

[0028] In some specific embodiments, the working parameters of the microwave-ultrasonic coordinated treatment include: microwave power of 560W, ultrasonic power of 380W, and treatment time of 35s.

[0029] In some specific embodiments, the weight ratio of the modified laver powder, the ceramic powder, the cross-linking agent, the antioxidant and the solvent is 100:(10-15):(1-5):(0.01-0.05):(45-55).

[0030] In some specific embodiments, the cross-linking agent includes at least one of dicumyl peroxide and dibenzoyl tert-butyl peroxide.

[0031] In some specific embodiments, the antioxidant includes at least one of 2,6-di-tert-butyl-4-methylphenol and tris(2,4-di-tert-butylphenyl)phosphite.

[0032] In some specific embodiments, the solvent includes at least one of xylene and toluene.

[0033] In some specific embodiments, the working parameters of the heating and stirring include: a temperature of 65 to 75° C. and a time of 1 to 3 hours.

[0034] In some specific embodiments, the grinding working parameters include: a grinding speed of 500 to 700 rpm, and a grinding time of 20 to 35 minutes.

[0035] In some specific embodiments, the Porphyra includes at least one of Porphyra circumflexa, Porphyra corrugateda, Porphyra longi, Porphyra haitanensis, Porphyra yezoensis and Porphyra lanuginosa.

[0036] In some specific embodiments, the microwave-ultrasonic coordinated processing can be implemented using existing ultrasonic-microwave combined reaction instruments, such as the commercially available XO-SM series ultrasonic-microwave combined reaction systems, ultrasonic-microwave reactors, and microwave-ultrasonic combined reactors.

[0037] In some specific embodiments, the ceramic powder can be commercially available products such as the far-infrared ceramic powder produced by Henan Xinzhiyuan Chemical Products Co., Ltd.

[0038] It should be noted that, unless otherwise specified or described, the components and raw materials involved in the preparation process of the coking wastewater treatment agent provided by the present invention can be directly commercially available products or homemade according to existing preparation processes. At the same time, the process steps involved in the preparation method can be carried out according to existing technologies or using existing equipment unless otherwise specified or described, and this application document will not repeat them one by one.

[0039] In a second aspect, based on a general inventive concept, the present invention provides a coking wastewater treatment agent, wherein the coking wastewater treatment agent is prepared by the preparation method described in any one of the first aspects.

[0040] The coking wastewater treatment agent provided by the present invention is realized based on the preparation method described in any one of the first aspects, and therefore has at least the beneficial effects of the technical solutions described in any one of the first aspects, which will not be described one by one here.

[0041] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.

[0042] Example 1

[0043] This example provides a coking wastewater treatment agent, and its preparation method comprises the following steps:

[0044] Step (1): crushing the dried corrugated laver and passing it through a 200-mesh sieve to obtain dried corrugated laver powder; then placing the obtained dried corrugated laver powder in an ultrasonic-microwave combined reaction instrument for microwave-ultrasonic synergistic treatment to obtain modified corrugated laver powder; wherein the working parameters of the microwave-ultrasonic synergistic treatment include: microwave power of 560 W, ultrasonic power of 380 W, and treatment time of 35 s;

[0045] Step (2): adding the modified wrinkled laver powder, ceramic powder, cross-linking agent and antioxidant obtained in step (1) into a solvent for mixing, heating and stirring at a temperature of 70° C. and a rotation speed of 200 rpm for 2 hours, and then cooling to room temperature to obtain a first mixed material; wherein the weight ratio of the modified laver powder, the ceramic powder, the cross-linking agent, the antioxidant and the solvent is 100:13:2:0.02:50; the cross-linking agent is tert-butyl dibenzoyl peroxide; the antioxidant is 2,6-di-tert-butyl-4-methylphenol; and the solvent is composed of xylene and toluene in a weight ratio of 1:1;

[0046] Step (3): The first mixed material obtained in step (2) is subjected to reduced pressure distillation and vacuum drying to obtain a solid; then the solid is ground at a rotation speed of 600 rpm for 25 minutes to obtain the coking wastewater treatment agent.

[0047] Example 2

[0048] This example provides a coking wastewater treatment agent, and its preparation method comprises the following steps:

[0049] Step (1): crushing the dried Porphyra chinensis and passing it through a 200-mesh sieve to obtain dried Porphyra chinensis powder; then placing the obtained dried Porphyra chinensis powder in an ultrasonic-microwave combined reaction instrument for microwave-ultrasonic synergistic treatment to obtain modified Porphyra chinensis powder; wherein the working parameters of the microwave-ultrasonic synergistic treatment include: microwave power of 520 W, ultrasonic power of 450 W, and treatment time of 25 s;

[0050] Step (2): adding the modified wrinkled laver powder, ceramic powder, cross-linking agent and antioxidant obtained in step (1) into a solvent and mixing them, heating and stirring at a temperature of 65° C. and a rotation speed of 200 rpm for 3 hours, and then cooling to room temperature to obtain a first mixed material; wherein the weight ratio of the modified laver powder, the ceramic powder, the cross-linking agent, the antioxidant and the solvent is 100:10:1:0.01:45; the cross-linking agent is tert-butyl dibenzoyl peroxide; the antioxidant is 2,6-di-tert-butyl-4-methylphenol; and the solvent is composed of xylene and toluene in a weight ratio of 1:1;

[0051] Step (3): The first mixed material obtained in step (2) is subjected to reduced pressure distillation and vacuum drying to obtain a solid; then the solid is ground at a rotation speed of 600 rpm for 25 minutes to obtain the coking wastewater treatment agent.

[0052] Example 3

[0053] This example provides a coking wastewater treatment agent, and its preparation method comprises the following steps:

[0054] Step (1): crushing the dried corrugated laver and passing it through a 200-mesh sieve to obtain dried corrugated laver powder; then placing the obtained dried corrugated laver powder in an ultrasonic-microwave combined reaction instrument for microwave-ultrasonic synergistic treatment to obtain modified corrugated laver powder; wherein the working parameters of the microwave-ultrasonic synergistic treatment include: microwave power of 600 W, ultrasonic power of 300 W, and treatment time of 40 s;

[0055] Step (2): adding the modified wrinkled laver powder, ceramic powder, cross-linking agent and antioxidant obtained in step (1) into a solvent and mixing them, heating and stirring at a temperature of 75° C. and a rotation speed of 200 rpm for 1 hour, and then cooling to room temperature to obtain a first mixed material; wherein the weight ratio of the modified laver powder, the ceramic powder, the cross-linking agent, the antioxidant and the solvent is 100:15:5:0.05:55; the cross-linking agent is tert-butyl dibenzoyl peroxide; the antioxidant is 2,6-di-tert-butyl-4-methylphenol; and the solvent is composed of xylene and toluene in a weight ratio of 1:1;

[0056] Step (3): The first mixed material obtained in step (2) is subjected to reduced pressure distillation and vacuum drying to obtain a solid; then the solid is ground at a rotation speed of 600 rpm for 25 minutes to obtain the coking wastewater treatment agent.

[0057] Comparative Example 1

[0058] This example provides a coking wastewater treatment agent, and its preparation method comprises the following steps:

[0059] Step (1): crushing the dried Porphyra chinensis and passing it through a 200-mesh sieve to obtain dried Porphyra chinensis powder; placing the obtained dried Porphyra chinensis powder in a reaction chamber of a microwave plasma treatment device, using an atmospheric pressure open chamber, and subjecting the chamber to non-ionizing radiation treatment for 45 seconds at a microwave treatment power of 890 W and air as a working medium to obtain modified Porphyra chinensis powder;

[0060] Step (2): adding the modified wrinkled laver powder, ceramic powder, cross-linking agent and antioxidant obtained in step (1) into a solvent for mixing, heating and stirring at a temperature of 70° C. and a rotation speed of 200 rpm for 2 hours, and then cooling to room temperature to obtain a first mixed material; wherein the weight ratio of the modified laver powder, the ceramic powder, the cross-linking agent, the antioxidant and the solvent is 100:13:2:0.02:50; the cross-linking agent is tert-butyl dibenzoyl peroxide; the antioxidant is 2,6-di-tert-butyl-4-methylphenol; and the solvent is composed of xylene and toluene in a weight ratio of 1:1;

[0061] Step (3): The first mixed material obtained in step (2) is subjected to reduced pressure distillation and vacuum drying to obtain a solid; then the solid is ground at a rotation speed of 600 rpm for 25 minutes to obtain the coking wastewater treatment agent.

[0062] Comparative Example 2

[0063] This example provides a coking wastewater treatment agent, and its preparation method comprises the following steps:

[0064] Step (1): crushing the dried corrugated laver and passing it through a 200-mesh sieve to obtain dried corrugated laver powder; then placing the obtained dried corrugated laver powder in an ultrasonic device for ultrasonic treatment, and then transferring it to a microwave instrument for further microwave treatment to obtain modified corrugated laver powder; wherein the working parameters of the ultrasonic treatment include: ultrasonic power of 380 W and treatment time of 35 s; the working parameters of the microwave treatment include: microwave power of 560 W and treatment time of 35 s;

[0065] Step (2): adding the modified wrinkled laver powder, ceramic powder, cross-linking agent and antioxidant obtained in step (1) into a solvent for mixing, heating and stirring at a temperature of 70° C. and a rotation speed of 200 rpm for 2 hours, and then cooling to room temperature to obtain a first mixed material; wherein the weight ratio of the modified laver powder, the ceramic powder, the cross-linking agent, the antioxidant and the solvent is 100:13:2:0.02:50; the cross-linking agent is tert-butyl dibenzoyl peroxide; the antioxidant is 2,6-di-tert-butyl-4-methylphenol; and the solvent is composed of xylene and toluene in a weight ratio of 1:1;

[0066] Step (3): The first mixed material obtained in step (2) is subjected to reduced pressure distillation and vacuum drying to obtain a solid; then the solid is ground at a rotation speed of 600 rpm for 25 minutes to obtain the coking wastewater treatment agent.

[0067] Comparative Example 3

[0068] This example provides a coking wastewater treatment agent, and its preparation method comprises the following steps:

[0069] Step (1): crushing the dried corrugated laver and passing it through a 200-mesh sieve to obtain dried corrugated laver powder; then placing the obtained dried corrugated laver powder in an ultrasonic-microwave combined reaction instrument for microwave-ultrasonic synergistic treatment to obtain modified corrugated laver powder; wherein the working parameters of the microwave-ultrasonic synergistic treatment include: microwave power of 380 W, ultrasonic power of 560 W, and treatment time of 35 s;

[0070] Step (2): adding the modified wrinkled laver powder, ceramic powder, cross-linking agent and antioxidant obtained in step (1) into a solvent for mixing, heating and stirring at a temperature of 70° C. and a rotation speed of 200 rpm for 2 hours, and then cooling to room temperature to obtain a first mixed material; wherein the weight ratio of the modified laver powder, the ceramic powder, the cross-linking agent, the antioxidant and the solvent is 100:13:2:0.02:50; the cross-linking agent is tert-butyl dibenzoyl peroxide; the antioxidant is 2,6-di-tert-butyl-4-methylphenol; and the solvent is composed of xylene and toluene in a weight ratio of 1:1;

[0071] Step (3): The first mixed material obtained in step (2) is subjected to reduced pressure distillation and vacuum drying to obtain a solid; then the solid is ground at a rotation speed of 600 rpm for 25 minutes to obtain the coking wastewater treatment agent.

[0072] Comparative Example 4

[0073] This example provides a coking wastewater treatment agent, and its preparation method comprises the following steps:

[0074] Step (1): crushing the dried agar-agar and passing it through a 200-mesh sieve to obtain dried agar-agar powder; then placing the obtained dried agar-agar powder in an ultrasonic microwave combined reaction instrument for microwave-ultrasonic synergistic treatment to obtain modified agar-agar powder; wherein the working parameters of the microwave-ultrasonic synergistic treatment include: microwave power of 560 W, ultrasonic power of 380 W, and treatment time of 35 s;

[0075] Step (2): adding the modified agar powder, ceramic powder, cross-linking agent and antioxidant obtained in step (1) into a solvent and mixing them, heating and stirring at 70° C. and 200 rpm for 2 hours, and then cooling to room temperature to obtain a first mixture; wherein the weight ratio of the modified agar powder, the ceramic powder, the cross-linking agent, the antioxidant and the solvent is 100:13:2:0.02:50; the cross-linking agent is tert-butyl dibenzoyl peroxide; the antioxidant is 2,6-di-tert-butyl-4-methylphenol; and the solvent is composed of xylene and toluene in a weight ratio of 1:1;

[0076] Step (3): The first mixed material obtained in step (2) is subjected to reduced pressure distillation and vacuum drying to obtain a solid; then the solid is ground at a rotation speed of 600 rpm for 25 minutes to obtain the coking wastewater treatment agent.

[0077] Test Case

[0078] This example tests the effects of the coking wastewater treatment agents provided in Examples 1 to 3 and Comparative Examples 1 to 4.

[0079] Test method: The coking wastewater treatment agent provided in Examples 1 to 3 and Comparative Examples 1 to 4 was added to the coking wastewater containing organic pollutants at a dosage of 5 g / L for adsorption purification. The phenol content in the water was determined by 4-aminoantipyrine photometry before and after the coking wastewater treatment, and the aniline content was determined by naphthylethylenediamine hydrochloride spectrophotometry, and then the removal rate was calculated according to Formula 1; wherein, Formula 1: Removal rate (%) = (C1-C2) / C1×100%; C1 is the initial concentration before treatment, and C2 is the equilibrium concentration after treatment.

[0080] The test results are shown in Table 1. All results are the average removal rates of three experiments.

[0081] Table 1

[0082]

[0083]

[0084] In summary, the present invention provides a coking wastewater treatment agent and a preparation method thereof. For the first time, natural laver is used as a raw material and subjected to microwave-ultrasonic coordinated treatment, and then the obtained modified laver powder and ceramic powder are cross-linked to obtain a natural coking wastewater treatment agent. The coking wastewater treatment agent has a good removal effect on aromatic compounds such as phenol and aniline in coking wastewater, and has no secondary pollution, thereby providing a new means for coking wastewater treatment.

[0085] The foregoing is merely a specific embodiment of the present invention, which enables those skilled in the art to understand or implement the present invention. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein may be implemented in other embodiments without departing from the spirit or scope of the present invention. Therefore, the present invention will not be limited to the embodiments shown herein, but rather to the widest scope consistent with the principles and novel features claimed herein.

Claims

1. A method for preparing a coking wastewater treatment agent, characterized in that: The preparation method comprises the following steps: placing the dried laver powder in a microwave-ultrasonic composite field for microwave-ultrasonic coordinated treatment to obtain modified laver powder; Adding the modified laver powder, ceramic powder, cross-linking agent and antioxidant into a solvent, heating and stirring, and then cooling to room temperature to obtain a first mixed material; The first mixed material is subjected to reduced pressure distillation, followed by drying and grinding to obtain the coking wastewater treatment agent; The working parameters of the microwave-ultrasonic coordinated processing include: microwave power of 520-600 W, ultrasonic power of 300-450 W, and processing time of 25-40 s.

2. The method for preparing a coking wastewater treatment agent according to claim 1, characterized in that: The working parameters of the microwave-ultrasonic coordinated treatment include: microwave power of 560 W, ultrasonic power of 380 W, and treatment time of 35 s.

3. The method for preparing a coking wastewater treatment agent according to claim 1, characterized in that: The weight ratio of the modified laver powder, the ceramic powder, the cross-linking agent, the antioxidant and the solvent is 100: (10-15): (1-5): (0.01-0.05): (45-55).

4. The method for preparing a coking wastewater treatment agent according to claim 3, characterized in that: The cross-linking agent is dicumyl peroxide.

5. The method for preparing the coking wastewater treating agent according to claim 3, characterized in that: The antioxidant includes at least one of 2,6-di-tert-butyl-4-methylphenol and tris(2,4-di-tert-butylphenyl)phosphite.

6. The method for preparing a coking wastewater treatment agent according to claim 3, characterized in that: The solvent includes at least one of xylene and toluene.

7. The method for preparing a coking wastewater treatment agent according to claim 1, characterized in that: The working parameters of the heating and stirring include: temperature of 65-75° C. and time of 1-3 hours.

8. The method for preparing a coking wastewater treatment agent according to claim 1, characterized in that: The grinding working parameters include: grinding speed of 500-700 rpm, and grinding time of 20-35 minutes.

9. A coking wastewater treatment agent, characterized in that: The coking wastewater treatment agent is prepared by the preparation method described in any one of claims 1 to 8.