A waterproof preparation method for solder paste
By adding water blocking agent, desiccant and temperature recovery agent to the solder paste, the water vapor condensation and temperature problems caused by insufficient temperature recovery of the solder paste are solved, ensuring the appropriate temperature of the solder paste and the printing quality.
Patent Information
- Application Number
- CN202410084160.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-19
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-01-19
AI Technical Summary
Insufficient temperature recovery of solder paste can easily cause water vapor to condense, leading to dryness, and too low temperature affects viscosity and expandability, resulting in poor printing.
It is composed of solder paste including 20% flux, 1-5% water blocking agent, 0.5-1% desiccant and 0.5-2% temperature recovery agent. The water blocking agent reacts with moisture to volatilize the water, and uses heat release to adjust the temperature. , and use the desiccant to reduce moisture condensation, and the temperature recovery agent to speed up the temperature recovery.
It effectively prevents water vapor from condensing, adjusts solder paste temperature, ensures appropriate operating temperature, and reduces drying and poor printing problems.
Smart Images

Figure CN117862745B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of tin preparation, and in particular to a waterproof preparation method of solder paste. Background Art
[0002] Solder paste is mainly used for welding electronic components such as resistors, capacitors, ICs, etc. on PCB surface in the SMT industry. It is widely used in surface mount welding process. As the main solder, the performance of solder paste determines the reliability of welding.
[0003] Solder paste usually needs to be stored in a refrigerator (2-10℃). Before printing and using, the solder paste should be placed in standard room temperature for warming up. A standard 500g package of solder paste should be warmed up for at least 2 hours, so that the temperature of the solder paste is the same as the ambient temperature. If the sealed can lid is opened before the temperature is fully warmed up, the water vapor in the air will condense due to the temperature difference and enter the solder paste, causing the solder paste to dry out; in addition, too low a temperature will affect the viscosity and expansibility of the solder paste, which is prone to poor printing. Summary of the invention
[0004] In order to improve the problem that insufficient temperature recovery during use of solder paste may easily cause water vapor to condense in the solder paste, causing the solder paste to dry out, and that too low temperature may affect the viscosity and expansibility of the solder paste, the present application provides a waterproof preparation method for solder paste.
[0005] The present application provides a method for preparing a waterproof solder paste using the following technical solution:
[0006] A method for preparing waterproof solder paste, the solder paste comprises 20% of flux, 1-5% of water-blocking agent, 0.5-1% of desiccant, 0.5-2% of warming agent, and the remainder is solder alloy powder. The specific preparation steps are as follows:
[0007] The water blocking agent is prepared by mixing 25-35% quicklime, 25-35% calcium chloride and 30-50% barium chloride by mass, and then ultrasonically dispersing the mixture for 3-5 minutes, and then ball milling the mixture for 3-4 hours at a stirring speed of 400-600 r / min to obtain a powder.
[0008] The desiccant is 30-50% sodium carbonate and 50-70% magnesium sulfate by mass percentage, the above materials are mixed and ground into fine powder;
[0009] The solder paste is prepared by mixing the flux, solder alloy powder, water barrier agent, desiccant and reheating agent evenly with stirring.
[0010] Furthermore, the temperature recovery agent uses graphene particles and grinds them into fine powder, and the ground powder is screened so that the particle diameter is less than 1 mm.
[0011] The solder paste mixing and preparation equipment includes a support base, a preliminary mixing component and a deep mixing component, and the preliminary mixing component and the deep mixing component are both installed and fixed on the inner side of the support base. The preliminary mixing component and the deep mixing component are connected so that the raw materials can be input from the preliminary mixing component to the deep mixing component.
[0012] Furthermore, a bottom reinforcement frame and a side reinforcement frame are respectively welded and fixed to the bottom and side of the support seat, and the support seat is in an inclined state under the support of the bottom reinforcement frame and the side reinforcement frame.
[0013] Furthermore, the preliminary mixing assembly may include a stirring tank, a stirring shaft, stirring blades and a driving motor. The driving motor is mounted and fixed on the outer wall of the stirring tank, and the output end of the driving motor is connected to the end of the stirring shaft, so that the stirring shaft is rotatably arranged in the stirring tank. A plurality of groups of stirring blades are evenly welded and fixed on the outer wall of the stirring shaft along its length direction, so that the stirring blades stir the raw materials as the stirring shaft rotates.
[0014] Furthermore, the preliminary mixing component also includes a feed inlet and a material guide inlet, and the material guide inlet is connected to the deep mixing component, so that the raw materials can be introduced from the preliminary mixing component into the deep mixing component.
[0015] Furthermore, the deep mixing component may include an outer shell, two groups of drive shafts, two groups of spiral blades, multiple groups of rubber springs, multiple groups of support columns, at least one group of vibration motors and a discharge port, the bottom ends of the multiple groups of support columns are fixed to the bottom inner wall of the support seat, and a group of rubber springs are fixed to the top of each group of support columns, the tops of the multiple groups of rubber springs are connected to the outer shell, two groups of drive shafts are installed in parallel in the outer shell, and a group of spiral blades are welded on the outer wall of each group of drive shafts, a drive motor is fixed at the end of the outer shell, so that its output end drives the end of the drive shaft connected to it, so that the two groups of drive shafts can respectively drive the spiral blades connected thereto to rotate, the vibration motor is connected and installed below the outer shell, so that when the vibration motor is enabled, it can be used to drive the outer shell to produce a certain vibration, and the discharge port is arranged below the outer shell for discharging the mixed solder paste.
[0016] The beneficial technical effects of the present application are as follows: by adding a water-blocking agent to the solder paste, after the solder paste is opened and taken out from a storage environment with a lower temperature, the water can be volatilized by the reaction between the water-blocking agent and water, and the heat release effect during the reaction can be utilized to better adjust the solder paste to a temperature suitable for use, thereby reducing the condensation of water vapor in the air and entering the solder paste due to the temperature difference, thereby causing the solder paste to dry out; by adding a desiccant to the solder paste, the condensation and accumulation of water in the solder paste can be reduced during the unopened storage process, and the failure of the water-blocking agent can be helped to reduce; by adding a warming agent, the solder paste can be warmed up to a suitable temperature for use more quickly by utilizing the heat released by the reaction between the water-blocking agent and water. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 This is a graph showing the temperature of the solder paste after use versus time when the water blocking agent is used in different ratios in the embodiment of the present application;
[0018] Figure 2 is a graph showing changes in humidity over time after solder paste is taken when the water blocking agent is used in different ratios in the embodiment of the present application;
[0019] Figure 3 is a schematic diagram of the structure of a mixing device used in preparing solder paste in an embodiment of the present application;
[0020] Figure 4 It is a schematic diagram of the structure of the mixing component after being cut open in the embodiment of the present application.
[0021] Figure numerals: 10, support base; 11, bottom reinforcement frame; 12, side reinforcement frame; 20, preliminary mixing assembly; 21, feeding port; 22, material guide port; 30, mixing assembly; 31, discharge port; 32, driving shaft; 33, spiral blade; 34, vibration motor; 35, rubber pile spring; 36, support column. DETAILED DESCRIPTION
[0022] The technical solution of the present application will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present application.
[0023] The embodiment of the present application discloses a waterproof preparation method of solder paste. When preparing the solder paste, flux, solder alloy powder, water barrier agent, desiccant and temperature recovery agent can be stirred and mixed evenly to form the solder paste.
[0024] The composition of the solder paste may include 20% of flux, 1-5% of water barrier, 0.5-1% of desiccant, 0.5-2% of warming agent, and the remaining component is solder alloy powder.
[0025] In this embodiment, the water-blocking agent is made of 25-35% quicklime, 25-35% calcium chloride and 30-50% barium chloride by mass percentage. After the above materials are mixed, they are ultrasonically dispersed for 3-5 minutes, and ball-milled for 3-4 hours at a stirring speed of 400-600 r / min to form a powder. The experimental performance of the water-blocking agent with different mass percentages of quicklime, calcium chloride and barium chloride is characterized as follows:
[0026] Reference example: Only flux, solder alloy powder, desiccant and reheating agent are taken and stirred to make solder paste, and the solder paste is sealed in a can and placed at 5℃ for 5 hours, then taken out and placed at 25℃ for 1.5 hours before opening the can;
[0027] Comparative Example 1: A solder paste was prepared by mixing flux, solder alloy powder, water barrier agent, desiccant and rewarming agent, and the water barrier agent was prepared by 25% quicklime, 25% calcium chloride and 50% barium chloride by mass. The solder paste was sealed in a can and stored at 5°C for 5 hours. The can was then taken out and placed at 25°C for 1.5 hours before being opened.
[0028] Comparative Example 2: A solder paste was prepared by mixing flux, solder alloy powder, water-blocking agent, desiccant and rewarming agent, and the water-blocking agent was prepared by 35% quicklime, 25% calcium chloride and 40% barium chloride by mass. The solder paste was sealed in a can and stored at 5°C for 5 hours. The can was then taken out and placed at 25°C for 1.5 hours before being opened.
[0029] Comparative Example 3: A solder paste was prepared by mixing flux, solder alloy powder, water barrier agent, desiccant and rewarming agent, and the mixture was prepared by stirring. The water barrier agent was composed of 25% quicklime, 35% calcium chloride and 40% barium chloride by mass. The solder paste was sealed in a can and stored at 5°C for 5 hours. The can was then taken out and placed at 25°C for rewarming for 1.5 hours and then the can was opened.
[0030] The experimental results of the above reference examples and comparative examples 1-3 are shown in the following table:
[0031] Temperature(℃) Reference example Comparative Example 1 Comparative Example 2 Comparative Example 3 Initial time 15℃ 15℃ 15℃ 15℃ +10min 15.8℃ 16.1℃ 19.1℃ 17.8℃ +20min 16.4℃ 19.2℃ 20.2℃ 19.4℃ +30min 17.2℃ 20.1℃ 21.1℃ 20.5℃ +40min 18.1℃ 21.2℃ 22.4℃ 21.7℃ +50min 18.8℃ 22.4℃ 23.5℃ 23.1℃ +60min 20.1℃ 23.8℃ 25.2℃ 24.4℃
[0032] Table 1 Temperature change comparison table
[0033] Humidity (%RH) Reference example Comparative Example 1 Comparative Example 2 Comparative Example 3 Initial time 1% 1% 1% 1% +10min 8% 7% 8% 7% +20min 15% 3% 5% 6% +30min 25% 1% 3% 3% +40min 32% 2% 1% 1% +50min 35% 2% 2% 1% +60min 35% 1% 1% 1%
[0034] Table 2 Humidity change comparison table
[0035] In this embodiment, the desiccant is 30-50% sodium carbonate and 50-70% magnesium sulfate by mass percentage, and the above materials are mixed and ground into fine powder. The desiccant can be used to reduce the penetration of water vapor when the solder paste is sealed and stored, and can also help maintain the effect of the water barrier and avoid the failure of the water barrier.
[0036] In this embodiment, the temperature recovery agent is graphene particles, which are ground into fine powder. The ground powder is screened so that the particle diameter is less than 1 mm. 2 The hybrid orbitals form a two-dimensional carbon nanomaterial with a hexagonal honeycomb lattice, and the thermal conductivity is as high as 5300W / m·K. When the water barrier agent in the solder paste reacts with water to release heat, the temperature recovery agent can absorb the heat and help accelerate the solder paste to a suitable temperature for use.
[0037] When preparing solder paste, you can use Figure 3 and Figure 4 The mixing equipment shown is operated, and flux, solder alloy powder, water barrier agent, desiccant and temperature recovery agent can be added from the feeding port 21 of the preliminary mixing component 20. After the preliminary mixing component 20 and the deep mixing component 30 mix the above raw materials evenly, the solder paste can be discharged from the discharge port 31 and collected.
[0038] In this embodiment, the support seat 10 can be made of carbon steel plate through cutting, bending, welding and spraying to form the shape shown in the figure, and the bottom reinforcement frame 11 and the side reinforcement frame 12 are respectively welded and fixed to the bottom and side of the support seat 10. Under the support of the bottom reinforcement frame 11 and the side reinforcement frame 12, the support seat 10 is in an inclined state. Anti-skid pads can also be installed at the bottom of the bottom reinforcement frame 11 and the side reinforcement frame 12, so that the equipment is more stable when placed in the processing workshop.
[0039] In the present embodiment, the preliminary mixing assembly 20 is fixed on the upper part of the support seat 10 by bolts. The preliminary mixing assembly 20 may include a stirring tank, a stirring shaft, stirring blades and a driving motor. The driving motor is used to drive the stirring shaft with stirring blades on the outer wall to rotate, and the flux, solder alloy powder, water barrier agent, desiccant and temperature recovery agent put into the stirring tank are preliminarily mixed. The top of the stirring tank is provided with a feed port 21, and the bottom of the stirring tank is provided with a feed guide port 22, and the feed port 21 and the feed guide port 22 are respectively located at the two ends of the stirring tank, so that the raw materials can be introduced into the deep mixing assembly 30 from the feed guide port 22 by the gravity in the inclined state during the stirring process. It should be understood that the preliminary mixing assembly 20 can be implemented by other known structures that achieve the above-mentioned effects, which will not be repeated here. The material guide port 22 is made of a tubular structure made of elastic rubber material. Both ends of the material guide port 22 are sleeved on the preliminary mixing component 20 and the deep mixing component 30, and the two ends of the material guide port 22 are fastened at the connection position by a clamp to prevent leakage of raw materials during transmission and to prevent vibration in the deep mixing component 30 from being affected by interference from the material guide port 22.
[0040] In this embodiment, the deep mixing assembly 30 may include an outer shell, two groups of drive shafts 32, two groups of spiral blades 33, multiple groups of rubber springs 35, multiple groups of support columns 36, at least one group of vibration motors 34, and a discharge port 31. The bottom ends of the multiple groups of support columns 36 are fixed to the bottom inner wall of the support seat 10, and a group of rubber springs 35 are fixed to the top of each group of support columns 36. The tops of the multiple groups of rubber springs 35 are connected to the outer shell, so that the outer shell can generate vibration by the deformation of the rubber springs 35. The hollow shell structure can be supported by a steel plate through bending, welding and other processing procedures, and notches for input and output are respectively opened on the outer shell. Two groups of drive shafts 32 are installed in parallel in the outer shell, and a group of spiral blades 33 are welded on the outer wall of each group of drive shafts 32. The drive motor is fixed at the end of the outer shell so that its output end drives the end of the drive shaft 32, so that the two groups of drive shafts 32 can respectively drive the spiral blades connected thereto to rotate. During use, the two sets of drive shafts 32 can be driven to rotate in opposite directions. In addition, the spiral blades 33 continue along the axial direction of the drive shaft 32, and the blade structures of the two sets of spiral blades 33 are staggered, so that the spiral blades 33 on the two sets of drive shafts 32 avoid interference, and the two sets of spiral blades 33 can rotate and stir the mixed raw materials while conveying them to the discharge port 31 for discharge. The vibration motor 34 is connected and installed below the outer shell, so that when the vibration motor 34 is enabled, it can be used to drive the outer shell to generate a certain vibration, so that the raw materials are mixed and conveyed in the outer shell, while reducing blockage and stagnation, and reducing the accumulation of raw materials on the inner wall of the outer shell.
[0041] The system of the present invention may further include a control system for controlling the operation of the motor to automatically mix and convey the solder paste raw materials. It should be understood that the control system has no particular limitation and can be implemented by control technology in the prior art, which will not be described in detail here.
[0042] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.
Claims
1. A waterproof preparation method for solder paste, characterized in that: The composition of solder paste includes 20% flux, 1-5% water barrier, 0.5-1% desiccant, 0.5-2% reheating agent, and the balance is solder alloy powder. The specific preparation steps are as follows: The water blocking agent is prepared by mixing 25-35% quicklime, 25-35% calcium chloride and 30-50% barium chloride by mass, and then ultrasonically dispersing the mixture for 3-5 minutes, and then ball milling the mixture for 3-4 hours at a stirring speed of 400-600 r / min to obtain a powder. The desiccant is 30-50% sodium carbonate and 50-70% magnesium sulfate by mass percentage. The above materials are mixed and ground into fine powder; The reheating agent is made of graphene particles, which are ground into fine powder. The ground powder is screened to make the particle diameter less than 1 mm. The solder paste is prepared by mixing the flux, solder alloy powder, water barrier agent, desiccant and reheating agent evenly with stirring.
2. The solder paste mixing and preparation device according to claim 1, characterized in that: The invention comprises a support base (10), a preliminary mixing component (20) and a deep mixing component (30), wherein the preliminary mixing component (20) and the deep mixing component (30) are both mounted and fixed on the inner side of the support base (10), and the preliminary mixing component (20) and the deep mixing component (30) are connected to each other so that raw materials can be input from the preliminary mixing component (20) to the deep mixing component (30). The preliminary mixing assembly (20) comprises a stirring tank, a stirring shaft, stirring blades and a driving motor, wherein the driving motor is mounted and fixed on the outer wall of the stirring tank, and the output end of the driving motor is connected to the end of the stirring shaft, so that the stirring shaft is rotatably arranged in the stirring tank, and a plurality of groups of stirring blades are uniformly welded and fixed on the outer wall of the stirring shaft along its length direction, so that the stirring blades stir the raw materials when the stirring shaft rotates, and the stirring tank is respectively formed with a feeding port (21) and a material guide port (22) for guiding the introduction and discharge of the raw materials; The deep mixing assembly (30) comprises an outer shell, two groups of drive shafts (32), two groups of spiral blades (33), multiple groups of rubber springs (35), multiple groups of support columns (36), at least one group of vibration motors (34) and a discharge port (31). The bottom ends of the multiple groups of support columns (36) are fixed to the bottom inner wall of the support seat (10), and a group of rubber springs (35) are fixed to the top of each group of support columns (36). The tops of the multiple groups of rubber springs (35) are connected to the outer shell. The two groups of drive shafts (32) are installed in parallel in the outer shell, and a group of spiral blades (33) are welded on the outer wall of each group of drive shafts (32). The drive motor is fixedly installed at the end of the outer shell so that its output end drives the end of the drive shaft (32) so that the two groups of drive shafts (32) can respectively drive the spiral blades (33) connected thereto to rotate. The vibration motor is connected and installed below the outer shell. The discharge port (31) is formed below the outer shell and communicates with its inner cavity.
Citation Information
Patent Citations
Low-temperature halogen-free lead-free solder paste
CN102990242A
Low-residue no-clean soldering flux and preparation method thereof
CN110091098A
High-stability environment-friendly soldering paste and preparation method thereof
CN114633046A
Resin composition for fluxes, solder paste and package structure
WO2023013732A1