A porous aromatic framework material, its preparation method and application

By preparing the porous aromatic framework material PAF-68 as a photocatalyst, the problem of low degradation efficiency of mustard gas under air conditions was solved, and rapid selective oxidation to non-toxic products was achieved. It has high specific surface area and chemical stability and is suitable for industrial production.

CN117866176BActive Publication Date: 2026-11-17NORTHEAST NORMAL UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310726688.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-06-19
Publication Date
2026-11-17
Estimated Expiration
2043-06-19

AI Technical Summary

Technical Problem

Existing photocatalysts have low efficiency in degrading mustard gas under air conditions, and it is inconvenient to use pure oxygen or hydrogen peroxide under complex conditions, making it difficult to achieve rapid and selective oxidation to low-toxicity sulfoxide products.

Method used

A porous aromatic framework material (PAF-68) was used as a photocatalyst and prepared by Sonogashira-Hagihara coupling polymerization. Porphyrin derivatives and triphenylamine were used as raw materials to catalyze the oxidation of mustard gas simulant (CEES) to the non-toxic oxidation product CEESO in an air atmosphere.

Benefits of technology

Ultrafast oxidation of mustard gas simulants was achieved under air conditions, with a conversion half-life of 2.3 minutes, which can be shortened to 1.9 minutes under humid air. The simulants also maintained good performance after multiple cycles, which is superior to existing materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117866176B_ABST
    Figure CN117866176B_ABST
Patent Text Reader

Abstract

This invention provides a porous aromatic framework material, its preparation method, and its application. The structural formula of the material is shown below; where n≥1. The material is prepared under a protective atmosphere using 5,10,15,20-tetra(4-bromophenyl)porphyrin and tris(4-ethynylphenyl)amine as raw materials, or 5,10,15,20-tetra(4-ethynylphenyl)porphyrin and tris(4-bromophenyl)amine as raw materials, followed by a catalytic reaction with the addition of a catalyst to obtain the porous aromatic framework material. As a photocatalyst, this material exhibits an ultra-fast rate of oxidation of mustard gas simulant CEES to the non-toxic oxidation product CEESO in an air atmosphere, especially under humid air, where the conversion half-life can reach as fast as 1.9 minutes. Furthermore, it maintains good photocatalytic degradation performance even after multiple cycles, solving the technical problem of how to rapidly degrade mustard gas under air conditions.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to the field of porous materials, specifically to a porous aromatic framework material, its preparation method, and its application as a photocatalyst for simulating mustard gas. Background Technology

[0002] Regarding the toxicity of mustard gas, it is generally believed that as a dialkylating agent, mustard gas can react with DNA, thereby inhibiting DNA replication and precise repair capabilities; it can also react with proteins, causing denaturation of the alkylated proteins.

[0003] Common methods for detoxifying mustard gas include dehydrohalogenation, hydrolysis, and oxidation. Dehydrohalogenation is too slow and can lead to incomplete degradation, potentially producing relatively toxic byproducts. Hydrolysis inhibits the formation of hydrolysis products due to the immiscibility of mustard gas with water, while also producing hydrochloric acid, which can poison the catalyst. Oxidation, particularly the partial oxidation of mustard gas to sulfoxides, is a promising detoxification method. However, excessive oxidation leads to the formation of sulfones, which are almost as toxic as mustard gas itself. Therefore, this method requires a selective oxidant to control product formation.

[0004] Currently, the commonly reported method utilizes the photocatalytic ability of photocatalysts to convert the oxidant into reactive oxygen species, and then selectively converts mustard gas into low-toxicity sulfoxides while avoiding the generation of highly toxic sulfones. The oxidant is primarily hydrogen peroxide or oxygen. However, pure oxygen or hydrogen peroxide conditions are not convenient for use under complex conditions, and most photocatalysts have low conversion efficiency for mustard gas under air conditions. Therefore, how to rapidly degrade mustard gas under air conditions is one of the main research challenges. Summary of the Invention

[0005] To address the technical problem of how to rapidly degrade mustard gas under air conditions, the present invention aims to provide a porous aromatic framework material, its preparation method, and its application as a photocatalyst for simulating mustard gas.

[0006] Porous materials are currently the most common photocatalysts used in the catalytic conversion of mustard gas, thanks to their large specific surface area and tunable active sites. Porous aromatic frameworks (PAFs) are a class of porous materials composed of linked organic units, possessing a large specific surface area, abundant porosity, and a rigid and stable structure. Their good cycling stability and excellent adsorption-diffusion capabilities make them suitable for use as functional porous materials in many fields such as separation, catalysis, and solid electrolytes. Currently, there are relatively few examples of PAFs in photocatalysis. Therefore, constructing photosensitive PAFs for reactive oxygen species-related reactions is a highly promising research direction.

[0007] Porphyrin derivatives possess tunable chemical structures and excellent photophysical properties, leading to their widespread application in photocatalysis and photodynamic therapy. Meanwhile, triphenylamine, an important photochromic molecule, has been widely used as a photoactive unit in the manufacture of various photoactive materials for applications such as organic semiconductors, solar cells, and photodynamic therapy. Therefore, porphyrin derivatives and triphenylamine are theoretically promising building blocks for constructing photosensitive photosensitive elements (PAFs) for applications involving reactive oxygen species (ROS).

[0008] This invention provides a high specific surface area and high stability photosensitive PAF material (named PAF-68) as a photocatalyst for the degradation of mustard gas simulant (2-chloroethyl ethyl sulfide, abbreviated as CEES). This material is obtained through Sonogashira-Hagihara coupling polymerization using m-tetra(p-bromophenyl)porphyrin (abbreviated as TBPP) and tris(4-ethynylphenyl)amine (abbreviated as EPA) as raw materials, or 5,10,15,20-tetra(4-ethynylphenyl)porphyrin (abbreviated as TEPP) and tris(4-bromophenyl)amine (abbreviated as BPA) as raw materials. Photocatalytic degradation experiments using mustard gas simulants show that this catalyst achieves an ultra-fast conversion half-life of 2.3 minutes in air to oxidize CEES to the non-toxic oxidation product CEESO, which is superior to all previously reported porous material photocatalysts. In humid air, the half-life is shortened to 1.9 minutes, and it maintains good photocatalytic degradation performance even after multiple cycles.

[0009] To achieve the above objectives, the technical solution of the present invention is as follows.

[0010] A porous aromatic framework material, the structural formula of which is shown below: ; Where n≥1.

[0011] This invention also provides a method for preparing a porous aromatic framework material, comprising the following steps: Under a protective atmosphere, a porous aromatic framework material (PAF-68) was prepared by using 5,10,15,20-tetra(4-bromophenyl)porphyrin (compound A-1) and tris(4-ethynylphenyl)amine (compound A-2) as raw materials and then adding a catalyst for catalytic reaction. The specific synthesis route is as follows: ; Alternatively, under a protective atmosphere, using 5,10,15,20-tetra(4-ethynylphenyl)porphyrin (compound B-1) and tri(4-bromophenyl)amine (compound B-2) as raw materials, and then adding a catalyst to carry out a catalytic reaction, a porous aromatic framework material (PAF-68) can be prepared. The specific synthesis route is as follows: ; Where n≥1.

[0012] Furthermore, the specific method includes the following steps: 5,10,15,20-tetra(4-bromophenyl)porphyrin and tris(4-ethynylphenyl)amine were mixed in a solvent, and triethylamine and a catalyst were added. After thorough mixing, the mixture was heated to 60–120 °C under a protective atmosphere. After the reaction was complete, the mixture was filtered to prepare a porous aromatic framework material; or… 5,10,15,20-tetra(4-ethynylphenyl)porphyrin and tri(4-bromophenyl)amine were mixed in a solvent, and triethylamine and a catalyst were added. After mixing evenly, the mixture was heated to 60–120 °C under a protective atmosphere. After the reaction was completed, the mixture was filtered to prepare a porous aromatic framework material.

[0013] Furthermore, the mass ratio of 5,10,15,20-tetra(4-bromophenyl)porphyrin to tris(4-ethynylphenyl)amine is 250:113.6; The mass ratio of 5,10,15,20-tetra(4-ethynylphenyl)porphyrin to tris(4-bromophenyl)amine is 250:226.

[0014] Furthermore, the ratio of 5,10,15,20-tetra(4-bromophenyl)porphyrin to triethylamine is 250 mg: 15-18 mL; The ratio of 5,10,15,20-tetra(4-ethynylphenyl)porphyrin to triethylamine is 250 mg: 15-18 mL.

[0015] Furthermore, the catalyst is tetra(triphenylphosphine)palladium and cuprous iodide; The mass ratio of tetra(triphenylphosphine)palladium to cuprous iodide is 45–59:15–19; The mass ratio of 5,10,15,20-tetra(4-bromophenyl)porphyrin to tetra(triphenylphosphine)palladium is 250:45-59; The mass ratio of 5,10,15,20-tetra(4-ethynylphenyl)porphyrin to tetra(triphenylphosphine)palladium is 250:45-59.

[0016] Furthermore, the uniform mixing is achieved by ultrasonic mixing of the mixed solution.

[0017] Furthermore, the protective atmosphere is a nitrogen atmosphere; the heating reaction time is 2 to 4 days.

[0018] Furthermore, the solvent is any one of toluene, mesitylene, o-dichlorobenzene, N,N-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran, and dichloromethane.

[0019] The present invention also provides an application of a porous aromatic framework material, which is used as a photocatalyst for the photocatalytic degradation of mustard gas simulants.

[0020] Furthermore, the conditions for photocatalytic degradation of mustard gas simulants were in an air atmosphere with a humidity of 0–60%.

[0021] The beneficial effects of this invention are: 1. This invention successfully prepared a photocatalyst material for the rapid degradation of mustard gas simulants under air conditions, solving the problem of mustard gas degradation under everyday and even harsh conditions. The photosensitive porous aromatic framework (PAF-68) material prepared by this invention has high specific surface area, high thermal stability and chemical stability, and also has application potential in harsh environments.

[0022] 2. The porous aromatic framework (PAF-68) material prepared in this invention, as a photocatalyst, has an ultra-fast rate of oxidizing mustard gas analog CEES to non-toxic oxidation product CEESO in an air atmosphere. Especially in humid air, the conversion half-life can reach as fast as 1.9 minutes, and it still maintains good photocatalytic degradation performance after multiple cycles, which is superior to all porous material photocatalysts reported to date.

[0023] 3. The preparation process of the present invention is mild, simple, easy to operate, and has a high yield, which can meet the requirements of actual industrial production. Attached Figure Description

[0024] Figure 1 The Fourier transform infrared spectrum of the porous aromatic framework PAF-68 material prepared in Example 1 of this invention.

[0025] Figure 2 Thermogravimetric analysis curves of the porous aromatic framework PAF-68 material prepared in Example 1 of this invention.

[0026] Figure 3 The nitrogen adsorption isotherm at 77 K for the porous aromatic framework PAF-68 material prepared in Example 1 of this invention.

[0027] Figure 4 This is an experimental diagram of the photocatalytic degradation of mustard gas simulants by the porous aromatic framework PAF-68 material prepared in Example 1 of the present invention. Detailed Implementation

[0028] To make the objectives, technical solutions, and advantages of this invention clearer, the invention will be further described in detail below with reference to embodiments. It should be understood that the specific embodiments described herein are merely illustrative and not intended to limit the invention.

[0029] Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without creative effort are within the scope of protection of the present invention.

[0030] Unless otherwise specified, the experimental methods used in the following examples are conventional methods; reagents and materials, unless otherwise specified, are commercially available.

[0031] The following details specific embodiments of the preparation of the porous aromatic framework PAF-68 material of the present invention.

[0032] Example 1 A method for preparing a porous aromatic framework material includes the following steps: Under a nitrogen protective atmosphere, a porous aromatic framework material (PAF-68) was polymerized from 5,10,15,20-tetra(4-bromophenyl)porphyrin (TBPP) and tris(4-ethynylphenyl)amine (EPA) in the presence of a catalyst. The synthetic route is as follows: .

[0033] The specific synthesis method is as follows: Weigh 250 mg (0.269 mmol) of 5,10,15,20-tetra(4-bromophenyl)porphyrin and 113.6 mg (0.358 mmol) of tris(4-ethynylphenyl)amine into a 100 mL double-necked flask, add 15 mL of N,N-dimethylformamide (DMF) and 15 mL of triethylamine (TEA, Et3N), and add 45 mg (0.0389 mmol) of tetra(triphenylphosphine)palladium and 15 mg (0.0789 mmol) of cuprous iodide under nitrogen protection. Sonicate the mixture for 5 minutes.

[0034] The reaction mixture was subjected to freeze-drying under nitrogen protection and liquid nitrogen, undergoing three cycles of freezing-vacuuming-thawing. It was then placed in an oil bath at 100 °C for two days. The product was filtered and then washed with ethanol, dichloromethane, tetrahydrofuran, ethanol, and water, respectively. It was then vacuum-dried overnight at 80 °C to obtain a porous aromatic framework material (PAF-68) with a yield of 95.0%.

[0035] Fourier transform infrared (IR) spectroscopy analysis was performed on the porous aromatic framework material (PAF-68) prepared in Example 1, see below. Figure 1 .Depend on Figure 1It can be seen that 564 and 515cm -1 The peak at 3281 cm⁻¹ is related to the stretching vibration of C-Br on the monomer TBPP, while the peak at 3281 cm⁻¹ is related to the stretching vibration of C-Br on the monomer TBPP. -1 The peak at 2204 cm⁻¹ is attributed to the characteristic vibration of the terminal alkynyl C≡H bond in EPA. The disappearance of these characteristic peaks in the product indicates that the monomer has reacted sufficiently, and a new, low-intensity peak at 2204 cm⁻¹ appears. -1 The peaks are attributed to the stretching vibrations of the newly formed alkyne bonds in PAF-68. These findings confirm the successful synthesis of PAF-68.

[0036] Example 2 A method for preparing a porous aromatic framework material includes the following steps: Under a nitrogen protective atmosphere, a porous aromatic framework material (PAF-68) was polymerized from 5,10,15,20-tetra(4-bromophenyl)porphyrin (TBPP) and tris(4-ethynylphenyl)amine (EPA) in the presence of a catalyst. The synthetic route is as follows: .

[0037] The specific synthesis method is as follows: Weigh 500 mg (0.538 mmol) of 5,10,15,20-tetra(4-bromophenyl)porphyrin and 227.2 mg (0.716 mmol) of tris(4-ethynylphenyl)amine into a 250 mL double-necked flask, add 30 mL of N,N-dimethylformamide (DMF) and 30 mL of triethylamine (TEA, Et3N), and add 90 mg (0.0778 mmol) of tetra(triphenylphosphine)palladium and 30 mg (0.1578 mmol) of cuprous iodide under nitrogen protection. Sonicate the mixture for 5 minutes.

[0038] Under nitrogen protection and liquid nitrogen, a freeze-drying operation was performed, involving three cycles of freezing, vacuuming, and thawing. The product was then placed in an oil bath at 120 °C for two days. The product was filtered, washed with ethanol, dichloromethane, tetrahydrofuran, ethanol, and water, and then vacuum-dried overnight at 80 °C to obtain a porous aromatic framework material (PAF-68) with a yield of 96.3%.

[0039] Fourier transform infrared (IR) spectroscopy analysis was performed on the porous aromatic framework material (PAF-68) prepared in Example 2. Specifically, the values ​​at 564 and 515 cm⁻¹ were... -1 The peak at 3281 cm⁻¹ is related to the stretching vibration of C-Br on the monomer TBPP, while the peak at 3281 cm⁻¹ is related to the stretching vibration of C-Br on the monomer TBPP. -1 The peak at 2204 cm⁻¹ is attributed to the characteristic vibration of the terminal alkynyl C≡H bond in EPA. The disappearance of these characteristic peaks in the product indicates that the monomer has reacted sufficiently, and a new, low-intensity peak at 2204 cm⁻¹ appears. -1The peaks are attributed to the stretching vibrations of the newly formed alkyne bonds in PAF-68. These findings confirm the successful synthesis of PAF-68.

[0040] Example 3 A method for preparing a porous aromatic framework material includes the following steps: Under a nitrogen protective atmosphere, a porous aromatic framework material (PAF-68) was polymerized from 5,10,15,20-tetra(4-bromophenyl)porphyrin (TBPP) and tris(4-ethynylphenyl)amine (EPA) in the presence of a catalyst. The synthetic route is as follows: .

[0041] The specific synthesis method is as follows: Weigh 50 mg (0.0538 mmol) of 5,10,15,20-tetra(4-bromophenyl)porphyrin and 22.72 mg (0.0716 mmol) of tris(4-ethynylphenyl)amine into a 50 mL double-necked flask, add 5 mL of N,N-dimethylformamide and 5 mL of triethylamine, and under nitrogen protection, add 9 mg (0.00778 mmol) of tetra(triphenylphosphine)palladium and 3 mg (0.01578 mmol) of cuprous iodide, and sonicate the mixture for 5 minutes.

[0042] Under nitrogen protection and liquid nitrogen, a freeze-drying operation was performed, involving three cycles of freezing, vacuuming, and thawing. The product was then placed in a 60°C oil bath for 4 days. The product was filtered, washed with ethanol, dichloromethane, tetrahydrofuran, ethanol, and water, respectively, and dried under vacuum at 80°C overnight to obtain a porous aromatic framework material (PAF-68) with a yield of 95.8%.

[0043] Fourier transform infrared (IR) spectroscopy analysis was performed on the porous aromatic framework material (PAF-68) prepared in Example 3. Specifically, the values ​​at 564 and 515 cm⁻¹ were... -1 The peak at 3281 cm⁻¹ is related to the stretching vibration of C-Br on the monomer TBPP, while the peak at 3281 cm⁻¹ is related to the stretching vibration of C-Br on the monomer TBPP. -1 The peak at 2204 cm⁻¹ is attributed to the characteristic vibration of the terminal alkynyl C≡H bond in EPA. The disappearance of these characteristic peaks in the product indicates that the monomer has reacted sufficiently, and a new, low-intensity peak at 2204 cm⁻¹ appears. -1 The peaks are attributed to the stretching vibrations of the newly formed alkyne bonds in PAF-68. These findings confirm the successful synthesis of PAF-68.

[0044] Example 4 A method for preparing a porous aromatic framework material includes the following steps: Under a nitrogen protective atmosphere, a porous aromatic framework material (PAF-68) was polymerized from 5,10,15,20-tetra(4-bromophenyl)porphyrin (TBPP) and tris(4-ethynylphenyl)amine (EPA) in the presence of a catalyst. The synthetic route is as follows: .

[0045] The specific synthesis method is as follows: Weigh 250 mg (0.269 mmol) of 5,10,15,20-tetra(4-bromophenyl)porphyrin and 113.6 mg (0.358 mmol) of tris(4-ethynylphenyl)amine into a 100 mL double-necked flask, add 18 mL of N,N-dimethylformamide (DMF) and 18 mL of triethylamine (TEA, Et3N), and add 59 mg of tetra(triphenylphosphine)palladium and 19 mg of cuprous iodide under nitrogen protection. Sonicate the mixture for 5 minutes.

[0046] Under nitrogen protection and liquid nitrogen, a freeze-drying operation was performed, involving three cycles of freezing, vacuuming, and thawing. The product was then placed in an oil bath at 100 °C for two days. The product was filtered, washed with ethanol, dichloromethane, tetrahydrofuran, ethanol, and water, and then vacuum-dried overnight at 80 °C to obtain a porous aromatic framework material (PAF-68) with a yield of 96.4%.

[0047] Fourier transform infrared (IR) spectroscopy analysis was performed on the porous aromatic framework material (PAF-68) prepared in Example 4. Specifically, the values ​​at 564 and 515 cm⁻¹ were [missing information]. -1 The peak at 3281 cm⁻¹ is related to the stretching vibration of C-Br on the monomer TBPP, while the peak at 3281 cm⁻¹ is related to the stretching vibration of C-Br on the monomer TBPP. -1 The peak at 2204 cm⁻¹ is attributed to the characteristic vibration of the terminal alkynyl C≡H bond in EPA. The disappearance of these characteristic peaks in the product indicates that the monomer has reacted sufficiently, and a new, low-intensity peak at 2204 cm⁻¹ appears. -1 The peaks are attributed to the stretching vibrations of the newly formed alkyne bonds in PAF-68. These findings confirm the successful synthesis of PAF-68.

[0048] Example 5 A method for preparing a porous aromatic framework material includes the following steps: Under a nitrogen protective atmosphere, a porous aromatic framework material (PAF-68) was polymerized from 5,10,15,20-tetratetra(4-ethynylphenyl)porphyrin (TEPP) and tri(4-bromophenyl)amine (BPA) in the presence of a catalyst. The synthetic route is as follows: .

[0049] The specific synthesis method is as follows: Weigh 250 mg (0.352 mmol) of 5,10,15,20-tetra(4-ethynylphenyl)porphyrin and 226 mg (0.469 mmol) of tri(4-bromophenyl)amine into a 100 mL double-necked flask, add 18 mL of N,N-dimethylformamide and 18 mL of triethylamine, and under nitrogen protection, add 59 mg (0.0510 mmol) of tetra(triphenylphosphine)palladium and 19 mg (0.1034 mmol) of cuprous iodide, and sonicate the mixture for 5 minutes.

[0050] The reaction mixture was subjected to freeze-drying under nitrogen protection and liquid nitrogen, undergoing three cycles of freezing-vacuuming-thawing. It was then placed in an oil bath at 100 °C for two days. The product was filtered, washed with ethanol, dichloromethane, tetrahydrofuran, ethanol, and water, respectively, and dried under vacuum at 80 °C overnight to obtain a porous aromatic framework material with a yield of 95.2%.

[0051] Fourier transform infrared (IR) spectroscopy analysis was performed on the porous aromatic framework material (PAF-68) prepared in Example 5. Specifically, the values ​​at 564 and 515 cm⁻¹ were [missing information]. -1 The peak at 3281 cm⁻¹ is related to the stretching vibration of C-Br on the monomer TBPP, while the peak at 3281 cm⁻¹ is related to the stretching vibration of C-Br on the monomer TBPP. -1 The peak at 2204 cm⁻¹ is attributed to the characteristic vibration of the terminal alkynyl C≡H bond in EPA. The disappearance of these characteristic peaks in the product indicates that the monomer has reacted sufficiently, and a new, low-intensity peak at 2204 cm⁻¹ appears. -1 The peaks are attributed to the stretching vibrations of the newly formed alkyne bonds in PAF-68. These findings confirm the successful synthesis of PAF-68.

[0052] Example 6 A method for preparing a porous aromatic framework material includes the following steps: Under a nitrogen protective atmosphere, a porous aromatic framework material (PAF-68) was polymerized from 5,10,15,20-tetratetra(4-ethynylphenyl)porphyrin (TEPP) and tri(4-bromophenyl)amine (BPA) in the presence of a catalyst. The synthetic route is as follows: .

[0053] The specific synthesis method is as follows: Weigh 250 mg (0.352 mmol) of 5,10,15,20-tetra(4-ethynylphenyl)porphyrin and 226 mg (0.469 mmol) of tri(4-bromophenyl)amine into a 100 mL double-necked flask, add 15 mL of N,N-dimethylformamide and 15 mL of triethylamine, and add 45 mg of tetra(triphenylphosphine)palladium and 15 mg of cuprous iodide under nitrogen protection. Sonicate the mixture for 5 minutes.

[0054] The reaction mixture was subjected to freeze-drying under nitrogen protection and liquid nitrogen, undergoing three cycles of freezing, vacuuming, and thawing. It was then placed in an oil bath at 100 °C for two days. The product was filtered, washed with ethanol, dichloromethane, tetrahydrofuran, ethanol, and water, respectively, and dried under vacuum at 80 °C overnight to obtain a porous aromatic framework material with a yield of 95.9%.

[0055] Fourier transform infrared (IR) spectroscopy analysis was performed on the porous aromatic framework material (PAF-68) prepared in Example 6. Specifically, the values ​​at 564 and 515 cm⁻¹ were... -1 The peak at 3281 cm⁻¹ is related to the stretching vibration of C-Br on the monomer TBPP, while the peak at 3281 cm⁻¹ is related to the stretching vibration of C-Br on the monomer TBPP. -1 The peak at 2204 cm⁻¹ is attributed to the characteristic vibration of the terminal alkynyl C≡H bond in EPA. The disappearance of these characteristic peaks in the product indicates that the monomer has reacted sufficiently, and a new, low-intensity peak at 2204 cm⁻¹ appears. -1 The peaks are attributed to the stretching vibrations of the newly formed alkyne bonds in PAF-68. These findings confirm the successful synthesis of PAF-68.

[0056] Below, we characterize the properties of the porous aromatic framework material prepared in the above embodiments.

[0057] Porous aromatic framework material (PAF-68) was prepared using the methods in Examples 1-6. We used PAF-68 prepared in Example 1 as an example for nitrogen adsorption isotherm analysis, such as... Figure 2 As shown.

[0058] Figure 2 Nitrogen adsorption isotherm at 77 K for the porous aromatic framework material (PAF-68) prepared in Example 1.

[0059] Depend on Figure 2 As can be seen, the N2 adsorption-desorption isotherm of PAF-68 exhibits a typical Type I curve. The hysteresis in the isotherm may be attributed to the expansion of the fully organic framework with increasing pressure. Based on the Brunauer-Emmett-Teller model, the BET specific surface area of ​​PAF-68 is estimated to be 509.37 m². 2 g -1 The total pore volume of PAF-68 was predicted to be 0.28 cm³ using nonlocal density functional theory (NLDFT). 3 g -1 The main pore sizes are concentrated at 0.51 nm and 0.88 nm, which facilitates the diffusion of substrates through the pores and their arrival at reaction sites during catalytic conversion.

[0060] We also estimated the BET specific surface area and total pore volume of PAF-68 prepared in Examples 2-6, and the results are shown in Table 1.

[0061] Table 1. BET specific surface area and total pore volume of PAF-68 <![CDATA[BET specific surface area (m 2 g -1 )]]> <![CDATA[Total pore volume (cm 3 g -1 )]]> Example 1 509.37 0.28 Example 2 532.57 0.30 Example 3 578.79 0.33 Example 4 462.83 0.25 Example 5 452.85 0.25 Example 6 422.84 0.22 As shown in Table 1, the BET specific surface area of ​​PAF-68 prepared in the embodiments of the present invention ranges from 422.84 to 578.79 m². 2 g -1 The total pore volume ranges from 0.22 to 0.33 cm³. 3 g -1 The main pore sizes are concentrated at 0.51 nm and 0.88 nm, which facilitates the diffusion of substrates through the pores and their arrival at reaction sites during catalytic conversion.

[0062] Application Example 1 The porous aromatic framework material (PAF-68) prepared in Example 1 was used as a photocatalyst to oxidize mustard gas mimic (CEES) to a non-toxic oxidation product (CEESO) in an air atmosphere. The specific operation is as follows:

[0063] 1.3 mg of the porous aromatic framework material (PAF-68) sample prepared in Example 1 and 5 mL of deuterated methanol were placed in a 20 mL quartz reactor, and air was introduced into the reaction system to create an air atmosphere. Then, 15 μL of the substrate CEES was added, and the reactor was placed under a xenon lamp to simulate sunlight for photocatalytic reaction. The reaction was monitored using NMR.

[0064] Figure 3 This is an experimental diagram showing the photocatalytic degradation of mustard gas simulants by the porous aromatic framework material (PAF-68) prepared in Example 1. Figure 4 The NMR results show that, under air conditions, it takes 5.1 minutes for CEES to be completely converted to CEESO in PAF-68 material, with a half-life of t. 1 / 2 =2.3 minutes.

[0065] Application Example 2 The porous aromatic framework material (PAF-68) prepared in Example 1 was used as a photocatalyst to oxidize mustard gas mimic (CEES) to a non-toxic oxidation product (CEESO) in a humid air atmosphere. The specific operation is as follows:

[0066] 1.3 mg of the porous aromatic framework material (PAF-68) sample prepared in Example 1 and 5 mL of deuterated methanol were placed in a 20 mL quartz reactor. Moist air was introduced into the reaction system to maintain an atmosphere of 60% relative humidity. Then, 15 μL of the substrate CEES was added, and the reactor was placed under a xenon lamp to simulate sunlight for photocatalytic reaction. The reaction was monitored using NMR.

[0067] The NMR results show that, under 60% relative humidity air conditions, PAF-68 material completely converts CEES to CEESO via photocatalytic detoxification within 4.7 minutes. 1 / 2 It only took 1.9 minutes.

[0068] Application Example 3 The porous aromatic framework material (PAF-68) prepared in Example 1 was used as a photocatalyst to oxidize mustard gas analog (CEES) to a non-toxic oxidation product (CEESO) in an air atmosphere with a relative humidity of 60%.

[0069] Multiple cyclic catalytic tests were conducted according to the method in Application Example 2. The results showed that after 7 cycles, the photocatalytic degradation performance could still be maintained at over 95%.

[0070] In summary, the NMR results showed that the half-life t of the photocatalytic detoxification effect of PAF-68 material under 60% relative humidity air conditions was... 1 / 2 The shortest half-life is only 1.9 minutes. This demonstrates that the porous aromatic framework (PAF-68) material prepared in this embodiment of the invention, as a photocatalyst, has an ultra-fast rate of oxidizing the mustard gas mimic CEES to the non-toxic oxidation product CEESO in an air atmosphere. Especially in humid (60% relative humidity) air, the conversion half-life can reach as fast as 1.9 minutes, and it still maintains good photocatalytic degradation performance after multiple cycles, which is superior to all porous material photocatalysts reported to date.

[0071] The above are merely preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, and improvements made within the spirit and principles of the present invention should be included within the protection scope of the present invention.

Claims

1. A porous aromatic framework material, characterized in that, The structural formula of the porous aromatic framework material is shown below: ; Where n≥1.

2. A method for preparing a porous aromatic framework material, characterized in that, Includes the following steps: Under a protective atmosphere, porous aromatic framework materials were prepared by using 5,10,15,20-tetra(4-bromophenyl)porphyrin and tris(4-ethynylphenyl)amine as raw materials and then adding a catalyst to carry out a catalytic reaction. or, Porous aromatic framework materials were prepared by using 5,10,15,20-tetra(4-ethynylphenyl)porphyrin and tri(4-bromophenyl)amine as raw materials under a protective atmosphere and then adding a catalyst for catalytic reaction.

3. The method for preparing the porous aromatic framework material according to claim 2, characterized in that, The specific method includes the following steps: 5,10,15,20-tetra(4-bromophenyl)porphyrin and tris(4-ethynylphenyl)amine were mixed in a solvent, and triethylamine and a catalyst were added. After thorough mixing, the mixture was heated to 60–120 °C under a protective atmosphere. After the reaction was complete, the mixture was filtered to prepare a porous aromatic framework material; or… 5,10,15,20-tetra(4-ethynylphenyl)porphyrin and tri(4-bromophenyl)amine were mixed in a solvent, and triethylamine and a catalyst were added. After mixing evenly, the mixture was heated to 60–120 °C under a protective atmosphere. After the reaction was completed, the mixture was filtered to prepare a porous aromatic framework material.

4. The method for preparing the porous aromatic framework material according to claim 3, characterized in that, The mass ratio of 5,10,15,20-tetra(4-bromophenyl)porphyrin to tris(4-ethynylphenyl)amine is 250:113.6; The mass ratio of 5,10,15,20-tetra(4-ethynylphenyl)porphyrin to tris(4-bromophenyl)amine is 250:

226.

5. The method for preparing the porous aromatic framework material according to claim 3, characterized in that, The ratio of 5,10,15,20-tetra(4-bromophenyl)porphyrin to triethylamine is 250 mg: 15-18 mL; The ratio of 5,10,15,20-tetra(4-ethynylphenyl)porphyrin to triethylamine is 250 mg: 15-18 mL; The catalyst is tetra(triphenylphosphine)palladium and cuprous iodide; The mass ratio of tetra(triphenylphosphine)palladium to cuprous iodide is 45–59:15–19; The mass ratio of 5,10,15,20-tetra(4-bromophenyl)porphyrin to tetra(triphenylphosphine)palladium is 250:45-59; The mass ratio of 5,10,15,20-tetra(4-ethynylphenyl)porphyrin to tetra(triphenylphosphine)palladium is 250:45-59.

6. The method for preparing the porous aromatic framework material according to claim 3, characterized in that, The process of achieving uniform mixing involves ultrasonic mixing of the solution.

7. The method for preparing the porous aromatic framework material according to claim 3, characterized in that, The protective atmosphere is nitrogen; the heating reaction time is 2 to 4 days.

8. The method for preparing the porous aromatic framework material according to claim 3, characterized in that, The solvent is any one of toluene, mesitylene, o-dichlorobenzene, N,N-dimethylformamide, N,N-dimethylacetamide, tetrahydrofuran, and dichloromethane.

9. An application of the porous aromatic framework material according to claim 1, characterized in that, The porous aromatic framework material is used as a photocatalyst for the photocatalytic degradation of mustard gas simulants.