Preparation method of water-dispersible photocurable polyimide nano resin

CN117866216BActive Publication Date: 2024-11-19SUMII TECH (SHENZHEN) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410042544.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-11
Publication Date
2024-11-19
Estimated Expiration
2044-01-11

Smart Images

  • Figure CN117866216B_ABST
    Figure CN117866216B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a water-dispersible photocurable polyimide nano resin, which specifically comprises the following steps: step 1, preparing a photopolymerizable linear polymer; step 2, preparing a photopolymerizable imide monomer; and step 3, preparing a water-dispersible photocurable polyimide nano resin according to the products obtained in step 1 and step 2. The nano resin material prepared by the invention solves the problem of poor dispersibility of existing nano materials in polyimide slurry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials and relates to a method for preparing water-dispersible photocurable polyimide nano resin. Background Art

[0002] Polyimide has unique mechanical, thermal, electrical and optical properties, and has been widely used in the fields of motor insulation materials, functional coatings, optoelectronic devices, etc. The synthesis conditions of polyimide are harsh, and the tape casting film forming process is complicated. People have begun to try new film-forming methods, such as preparing a new type of polyimide resin slurry, further spin coating and using ultraviolet light to cure the film. In order to improve the mechanical, thermal, electrical and optical properties of the resin, nanomaterials such as nano oxides, nano metals, nano carbon and other materials are added to the polyimide slurry. The disadvantage is that polyimide and nanomaterials are heterogeneous structures, and the dispersibility of nanomaterials in polyimide slurry is poor. In addition, during the use of resins, people have higher and higher requirements for environmental protection, and water as a dispersant is more environmentally friendly. Therefore, it is of great significance to prepare nanomaterials of water-dispersible photocurable polyimide. Summary of the invention

[0003] The purpose of the present invention is to provide a method for preparing a water-dispersible photocurable polyimide nano resin. The nano resin material prepared by the method solves the problem of poor dispersibility of existing nano materials in polyimide slurry.

[0004] The technical solution adopted by the present invention is a method for preparing a water-dispersible photocurable polyimide nano resin, which specifically comprises the following steps:

[0005] Step 1, preparing a photopolymerizable linear polymer;

[0006] Step 2, preparing a photopolymerizable imide monomer;

[0007] Step 3, preparing water-dispersible photocurable polyimide nano resin according to the products obtained in step 1 and step 2.

[0008] The present invention is also characterized in that:

[0009] The specific process of step 1 is:

[0010] Step 1.1, add 0.1mL-0.5mL of 4-vinylaniline, 1mL-1.5mL of methyl acrylate, and 2mL-10mL of N,N-dimethylformamide into a reaction bottle, introduce nitrogen to exclude air for 30min-60min, add 10mg-30mg of azobisisobutyronitrile, heat to 80℃~90℃ and react for 8h-16h. After the reaction is completed, pour the reaction solution into 50mL-100mL of industrial alcohol, collect the solid powder, and vacuum dry for 12h-36h to obtain a linear polymer precursor;

[0011] Step 1.2, take 0.5g of linear polymer precursor and 0.1-0.3g of cinnamoyl chloride and dissolve them in 5mL-15mL of N,N-dimethylformamide solution, then add 0.05mL-0.15mL of triethylamine, react for 4h-12h, pour the reaction solution into 50mL-100mL of industrial alcohol, collect the solid powder, and vacuum dry it for 12-36h to obtain a photopolymerizable linear polymer.

[0012] The specific process of step 2 is:

[0013] Step 2.1, dissolving 1.09 g to 2.18 g of pyromellitic anhydride in N, N-dimethylformamide to obtain a pyromellitic anhydride solution; dissolving 1.08 g to 2.16 g of 1,4-diaminobenzene in N, N-dimethylformamide to obtain a 1,4-diaminobenzene solution;

[0014] Step 2.2, adding the pyromellitic anhydride solution dropwise into the 1,4-diaminobenzene solution, stirring for 3h-6h after the addition is completed, heating to 80°C-150°C and continuing the reaction for 6h-18h, and separating and purifying by column to obtain an imide precursor;

[0015] Step 2.3, take 1g of imide precursor and 0.3g-0.6g of cinnamoyl chloride and dissolve them in 10mL-15mL of N,N-dimethylformamide solution, then add 0.1mL-0.3mL of triethylamine, react for 4h-12h, separate and purify by column to obtain photopolymerizable imide monomer.

[0016] The specific process of step 3 is:

[0017] Step 3.1, preparing polyimide nano resin;

[0018] Step 3.2, dissolving 1 g to 2 g of polyethylene glycol monomethyl ether in a mixed solution of 5 mL to 10 mL of N, N-dimethylformamide and deionized water, adding 24 mg to 48 mg of NaH, and stirring for 30 min to 60 min to obtain a mixed solution A;

[0019] Step 3.3, take 0.1g-0.2g of polyimide nano resin, add it to the mixed solution A obtained in step 3.2, stir at room temperature for 30min-60min, and dialyze after the reaction to obtain water-dispersible photocurable polyimide nano resin.

[0020] The specific process of step 3.1 is:

[0021] 0.5g-1.0g of a photopolymerizable linear polymer, 0.05g-0.1g of a photopolymerizable imide monomer and 0.05g-0.1g of vinyl cinnamate are respectively dissolved in 2mL-4mL of N,N-dimethylformamide to obtain a mixed solution B, and the mixed solution B is added dropwise into 20mL-40mL of deionized water while stirring, and irradiated with an ultraviolet curing lamp for 10s-60s. After the reaction is completed, freeze-drying is performed at -70°C to -30°C to obtain a polyimide nanoresin.

[0022] The beneficial effect of the present invention is that the preparation method of the water-dispersible photocurable polyimide nano resin provided by the present invention constructs a linear polymer and an imide monomer having a cinnamic acid structural unit, mixes and disperses the linear polymer and imide monomer with vinyl cinnamate, and prepares a nano material by ultraviolet light irradiation. By cleverly using the difference in activity between the cinnamic acid double bond and the vinyl ester double bond of vinyl cinnamate under ultraviolet light conditions, the prepared polyimide nano resin retains the vinyl ester double bond. At the same time, the water-dispersible nano resin is obtained by modifying the nano resin with polyethylene glycol monoether. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 It is a performance comparison chart of Example 1 and Comparative Examples 1 to 3 in the method for preparing water-dispersible photocurable polyimide nanoresin of the present invention. DETAILED DESCRIPTION

[0024] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0025] The preparation method of the water-dispersible photocurable polyimide nano resin of the present invention specifically comprises the following steps:

[0026] Step 1, add 0.1-0.5mL of 4-vinylaniline, 1-1.5mL of methyl acrylate, and 2-10mL of N,N-dimethylformamide to a 25mL reaction bottle, and introduce nitrogen to exclude air for 30-60min. Add 10-30mg of azobisisobutyronitrile, heat to 80℃~90℃ and react for 8-16h. After the reaction is completed, pour the reaction solution into 50-100mL of industrial alcohol, collect the solid powder, and vacuum dry at 45℃ for 12-36h to obtain a linear polymer precursor. Take 0.5g of linear polymer precursor and 0.1-0.3g of cinnamoyl chloride and dissolve them in 5-15mL of N,N-dimethylformamide solution, then add 0.05-0.15mL of triethylamine, react at 50℃ for 4-12h, further pour the reaction solution into 50-100mL of industrial alcohol, collect solid powder, and vacuum dry at 45℃ for 12-36h to obtain a photopolymerizable linear polymer. The synthesis route is as follows (m is related to the amount of methyl acrylate input during synthesis, and n is related to the amount of 4-vinylaniline input during synthesis):

[0027]

[0028] Step 2, dissolve 1.09g-2.18g of pyromellitic anhydride in 5mL of N,N-dimethylformamide; further dissolve 1.08-2.16g of 1,4-diaminobenzene in 5mL of N,N-dimethylformamide; add the pyromellitic anhydride solution dropwise to the 1,4-diaminobenzene solution (addition time is 0.5-1h). After the addition is completed, stir at room temperature for 3-6h; further heat to 80℃-150℃ and continue the reaction for 6-18h. Use column separation and purification (eluent v (ethyl acetate): v (petroleum ether) = 1:5) to obtain an imide precursor. Further, 1 g of the imide precursor and 0.3-0.6 g of cinnamoyl chloride were dissolved in 10-15 mL of N,N-dimethylformamide solution, and then 0.1 mL-0.3 mL of triethylamine was added, and the mixture was reacted at 50° C. for 4 h-12 h. The mixture was separated and purified by column (eluent v (ethyl acetate): v (petroleum ether) = 1:5) to obtain a photopolymerizable imide monomer, which was synthesized as follows:

[0029]

[0030] Step 3: Dissolve 0.5-1.0 g of a photopolymerizable linear polymer, 0.05-0.1 g of a photopolymerizable imide monomer, and 0.05-0.1 g of vinyl cinnamate in 2 mL-4 mL of N,N-dimethylformamide, and dropwise add the resulting solution into 20-40 mL of deionized water while rapidly stirring (300 r / min). Further, use an ultraviolet curing lamp (50-150 mW / cm 2After the reaction is completed, the polyimide nano resin is obtained by freeze drying at -70°C to -30°C.

[0031] 1g-2g of polyethylene glycol monomethyl ether (average molecular weight 1000-1900) is dissolved in 5mL-10mL of a mixed solution of N, N-dimethylformamide and deionized water (v:v=1:1), NaH (24-48mg) is added, and the mixture is stirred at room temperature for 30-60min to obtain a mixed solution A. 0.1-0.2g of polyimide nanoresin is added to the mixed solution A, and the mixture is stirred at room temperature for 30-60min. After the reaction is completed, the mixture is dialyzed in a 7000Da dialysis bag and an ethanol solution to obtain a water-dispersible photocurable polyimide nanoresin.

[0032] Example 1

[0033] Step 1, take 0.1mL of 4-vinylaniline, 1mL of methyl acrylate, and 2mL of N,N-dimethylformamide and add them to a 25mL reaction bottle, and introduce nitrogen to exclude air for 30min. Add 10mg of azobisisobutyronitrile and heat to 80℃ for 8h. After the reaction is completed, pour the reaction solution into 50mL of industrial alcohol, collect the solid powder, and vacuum dry it at 45℃ for 12h to obtain a linear polymer precursor. Take 0.5g of linear polymer precursor and 0.1g of cinnamoyl chloride and dissolve them in 5mL of N,N-dimethylformamide solution, then add 0.05mL of triethylamine, react at 50℃ for 4h, pour the reaction solution into 50mL of industrial alcohol, collect the solid powder, and vacuum dry it at 45℃ for 12h to obtain a photopolymerizable linear polymer.

[0034] Step 2, dissolve 1.09g of pyromellitic anhydride in 5mL of N,N-dimethylformamide, and dissolve 1.08g of 1,4-diaminobenzene in 5mL of N,N-dimethylformamide; add the pyromellitic anhydride solution drop by drop into the 1,4-diaminobenzene solution (the dropping time is 0.5h). After the dropping is completed, stir at room temperature for 3h, heat to 80°C and continue to react for 6h, and separate and purify by column (eluent v (ethyl acetate): v (petroleum ether) = 1:5) to obtain an imide precursor; take 1g of the imide precursor and 0.3g of cinnamoyl chloride and dissolve them in 10mL of N,N-dimethylformamide solution, 0.1mL of triethylamine, react at 50°C for 4h, separate and purify by column (eluent v (ethyl acetate): v (petroleum ether) = 1:5) to obtain a photopolymerizable imide monomer.

[0035] Step 3: Dissolve 0.5 g of photopolymerizable linear polymer, 0.05 g of photopolymerizable imide monomer and 0.05 g of vinyl cinnamate in 2 mL of N,N-dimethylformamide, and add the resulting solution dropwise into 20 mL of deionized water while stirring rapidly (300 r / min). Use a UV curing lamp (50 mW / cm 2 After the reaction, the polyimide nano resin was obtained by freeze drying at -30°C.

[0036] 1 g of polyethylene glycol monomethyl ether (average molecular weight 1000) was dissolved in 5 mL of a mixed solution of N, N-dimethylformamide and deionized water (v:v=1:1), and NaH (24 mg) was added. The mixture was stirred at room temperature for 30 min to obtain a mixed solution A. 0.1 g of polyimide nanoresin was added to the mixed solution A and stirred at room temperature for 30 min. After the reaction, the mixture was dialyzed in a 7000 Da dialysis bag and an ethanol solution to obtain a water-dispersible photocurable polyimide nanoresin.

[0037] Comparative Example 1 (Methyl acrylate was replaced by vinyl acetate, other conditions and steps remained unchanged, and the resulting nano resin could not be dispersed in water)

[0038] Step 1, add 0.1mL of 4-vinylaniline, 1mL of vinyl acetate, and 2mL of N,N-dimethylformamide to a 25mL reaction bottle, and introduce nitrogen to exclude air for 30min. Add 10mg of azobisisobutyronitrile, heat to 80℃ and react for 8h. After the reaction is completed, pour the reaction solution into 50mL of industrial alcohol, collect the solid powder, and vacuum dry it at 45℃ for 12h to obtain a linear polymer precursor; take 0.5g of the linear polymer precursor and 0.1g of cinnamoyl chloride and dissolve them in 5mL of N,N-dimethylformamide solution, then add 0.05mL of triethylamine, react at 50℃ for 4h-12h, pour the reaction solution into 50mL of industrial alcohol, collect the solid powder, and vacuum dry it at 45℃ for 12h to obtain a photopolymerizable linear polymer.

[0039] Step 2, dissolve 1.09g of pyromellitic anhydride in 5mL of N,N-dimethylformamide, and dissolve 1.08g of 1,4-diaminobenzene in 5mL of N,N-dimethylformamide; add the pyromellitic anhydride solution drop by drop into the 1,4-diaminobenzene solution (the dropping time is 0.5h). After the dropping is completed, stir at room temperature for 3h, heat to 80°C and continue to react for 6h, and separate and purify by column (eluent v (ethyl acetate): v (petroleum ether) = 1:5) to obtain an imide precursor; take 1g of the imide precursor and 0.3g of cinnamoyl chloride and dissolve them in 10mL of N,N-dimethylformamide solution, 0.1mL of triethylamine, react at 50°C for 4h, separate and purify by column (eluent v (ethyl acetate): v (petroleum ether) = 1:5) to obtain a photopolymerizable imide monomer.

[0040] Step 3: Dissolve 0.5 g of photopolymerizable linear polymer, 0.05 g of photopolymerizable imide monomer and 0.05 g of vinyl cinnamate in 2 mL of N,N-dimethylformamide, and add the resulting solution dropwise into 20 mL of deionized water while stirring rapidly (300 r / min). Use a UV curing lamp (50 mW / cm 2 After the reaction, the polyimide nano resin was obtained by freeze drying at -30°C.

[0041] 1 g of polyethylene glycol monomethyl ether (average molecular weight 1000) was dissolved in 5 mL of a mixed solution of N, N-dimethylformamide and deionized water (v:v=1:1), and NaH (24 mg) was added. The mixture was stirred at room temperature for 30 min to obtain a mixed solution A. 0.1 g of polyimide nanoresin was added to the mixed solution A and stirred at room temperature for 30 min. After the reaction, the mixture was dialyzed in a 7000 Da dialysis bag and an ethanol solution to obtain a water-dispersible photocurable polyimide nanoresin.

[0042] Comparative Example 2 (the deionized water in the mixed solution was removed, and other experimental steps and conditions remained unchanged, and the nano-resin finally obtained could not be dispersed in water)

[0043] Step 1, take 0.1mL of 4-vinylaniline, 1mL of methyl acrylate, and 2mL of N,N-dimethylformamide and add them to a 25mL reaction bottle, and introduce nitrogen to exclude air for 30min. Add 10mg of azobisisobutyronitrile and heat to 80℃ for 8h. After the reaction is completed, pour the reaction solution into 50mL of industrial alcohol, collect the solid powder, and vacuum dry it at 45℃ for 12h to obtain a linear polymer precursor. Take 0.5g of linear polymer precursor and 0.1g of cinnamoyl chloride and dissolve them in 5mL of N,N-dimethylformamide solution, then add 0.05mL of triethylamine, react at 50℃ for 4h, pour the reaction solution into 50mL of industrial alcohol, collect the solid powder, and vacuum dry it at 45℃ for 12h to obtain a photopolymerizable linear polymer.

[0044] Step 2, dissolve 1.09g of pyromellitic anhydride in 5mL of N,N-dimethylformamide, and dissolve 1.08g of 1,4-diaminobenzene in 5mL of N,N-dimethylformamide; add the pyromellitic anhydride solution drop by drop into the 1,4-diaminobenzene solution (the dropping time is 0.5h). After the dropping is completed, stir at room temperature for 3h, heat to 80°C and continue to react for 6h, and separate and purify by column (eluent v (ethyl acetate): v (petroleum ether) = 1:5) to obtain an imide precursor; take 1g of the imide precursor and 0.3g of cinnamoyl chloride and dissolve them in 10mL of N,N-dimethylformamide solution, 0.1mL of triethylamine, react at 50°C for 4h, separate and purify by column (eluent v (ethyl acetate): v (petroleum ether) = 1:5) to obtain a photopolymerizable imide monomer.

[0045] Step 3: Dissolve 0.5 g of photopolymerizable linear polymer, 0.05 g of photopolymerizable imide monomer and 0.05 g of vinyl cinnamate in 2 mL of N,N-dimethylformamide, and add the resulting solution dropwise into 20 mL of deionized water while stirring rapidly (300 r / min). Use a UV curing lamp (50 mW / cm 2 After the reaction, the polyimide nano resin was obtained by freeze drying at -30°C.

[0046] Dissolve 1 g of polyethylene glycol monomethyl ether (average molecular weight 1000) in 5-10 mL of a mixed solution of N,N-dimethylformamide and deionized water (v:v=1:1), add NaH (24 mg), and stir at room temperature for 30 min to obtain a mixed solution A. Take 0.1 g of polyimide nanoresin, add it to the mixed solution A and stir at room temperature for 30 min. After the reaction, dialyze in a 7000Da dialysis bag and ethanol solution to obtain a water-dispersible photocurable polyimide nanoresin.

[0047] Comparative Example 3 (vinyl cinnamate was replaced by vinyl acrylate, other experimental steps and reaction conditions remained unchanged, and nano resin could not be obtained)

[0048] Step 1, add 0.1mL of 4-vinylaniline, 1mL of vinyl acetate, and 2mL of N,N-dimethylformamide to a 25mL reaction bottle, and introduce nitrogen to exclude air for 30min. Add 10mg of azobisisobutyronitrile, heat to 80℃ and react for 8h. After the reaction is completed, pour the reaction solution into 50mL of industrial alcohol, collect the solid powder, and vacuum dry it at 45℃ for 12h to obtain a linear polymer precursor; take 0.5g of the linear polymer precursor and 0.1g of cinnamoyl chloride and dissolve them in 5mL of N,N-dimethylformamide solution, then add 0.05mL of triethylamine, react at 50℃ for 4h-12h, pour the reaction solution into 50mL of industrial alcohol, collect the solid powder, and vacuum dry it at 45℃ for 12h to obtain a photopolymerizable linear polymer.

[0049] Step 2, dissolve 1.09g of pyromellitic anhydride in 5mL of N,N-dimethylformamide, and dissolve 1.08g of 1,4-diaminobenzene in 5mL of N,N-dimethylformamide; add the pyromellitic anhydride solution drop by drop into the 1,4-diaminobenzene solution (the dropping time is 0.5h). After the dropping is completed, stir at room temperature for 3h, heat to 80°C and continue to react for 6h, and separate and purify by column (eluent v (ethyl acetate): v (petroleum ether) = 1:5) to obtain an imide precursor; take 1g of the imide precursor and 0.3g of cinnamoyl chloride and dissolve them in 10mL of N,N-dimethylformamide solution, 0.1mL of triethylamine, react at 50°C for 4h, separate and purify by column (eluent v (ethyl acetate): v (petroleum ether) = 1:5) to obtain a photopolymerizable imide monomer.

[0050] Step 3: Dissolve 0.5 g of photopolymerizable linear polymer, 0.05 g of photopolymerizable imide monomer and 0.05 g of vinyl acrylate in 2 mL of N,N-dimethylformamide. Add the resulting solution dropwise into 20 mL of deionized water while stirring rapidly (300 r / min). Use a UV curing lamp (50 mW / cm 2 ) was irradiated for 10 seconds. After the reaction was completed, the polyimide nanoresin was obtained by freeze-drying at -30°C.

[0051] Dissolve 1g of polyethylene glycol monomethyl ether (average molecular weight 1000) in 5-10mL of a mixed solution of N,N-dimethylformamide and deionized water (v:v=1:1), add NaH (24mg), and stir at room temperature for 30min. Take 0.1g of polyimide nano resin, add it to the mixed solution, and stir at room temperature for 30min. After the reaction, dialyze in a 7000Da dialysis bag and ethanol solution to obtain a water-dispersible light-curable polyimide resin.

[0052] Results and Discussion

[0053] Table 1 Performance comparison of embodiments and comparative examples

[0054] Example 1 Comparative Example 1 Comparative Example 2 Comparative Example 3 Hydraulic radius (nm) 26 22 24 50 Water dispersibility dispersion Reunion Reunion dispersion <![CDATA[Coefficient of thermal expansion (K -1 )]]> <![CDATA[3.8x10 -5 ]]> <![CDATA[3.5x10 -5 ]]> <![CDATA[3.2x10 -5 ]]> <![CDATA[7.0x10 -5 ]]>

[0055] like Figure 1 ( Figure 1 The horizontal axis represents the normalized intensity, and the vertical axis represents the hydraulic radius) and as shown in Table 1, the hydraulic radius of Comparative Example 3 is much higher than that of Example 1 and Comparative Examples 1-2; due to the cyclization and cross-linking of the double bonds in cinnamic acid, a nano material can be formed. However, after vinyl cinnamate in Comparative Example 3 was replaced with vinyl acrylate, no reaction occurred. Therefore, when measured by a laser particle size analyzer, the physical mixed system formed by the photopolymerizable linear polymer, the photopolymerizable imide monomer and the vinyl acrylate, the mixed system is easily dispersed in the solvent, and at the same time, the molecular chain of the linear polymer stretches out, and the measured hydraulic radius value is larger than 50nm. The hydraulic radius of Example 1 is larger than that of Comparative Examples 1 and 2. The main reason is that in Example 1, the polyethylene glycol monomethyl ether polymer chain is grafted to the methyl acrylate unit in the linear polymer, which increases the molecular weight of the nano resin.

[0056] Comparative Example 1 cannot be dispersed in aqueous solution because after methyl acrylate is replaced by vinyl acetate, polyethylene glycol monomethyl ether cannot be grafted to the methyl acrylate unit in the linear polymer through transesterification. In Comparative Example 2, no deionized water is added during the reaction, and the methyl acrylate unit in the linear polymer cannot be hydrolyzed, resulting in the inability of polyethylene glycol monomethyl ether to complete grafting through transesterification.

[0057] Comparative Example 3 is a non-nano material with a high thermal expansion coefficient. However, after cyclization and cross-linking, Example 1 and Comparative Examples 1-2 form a nano material structure with better thermal stability.

[0058] Example 2

[0059] Step 1, take 0.3mL of 4-vinylaniline, 1.2mL of methyl acrylate, and 8mL of N,N-dimethylformamide and add them to a 25mL reaction bottle, and introduce nitrogen to exclude air for 50min. Add 20mg of azobisisobutyronitrile and heat to 85℃ for reaction for 12h. After the reaction is completed, pour the reaction solution into 70mL of industrial alcohol, collect the solid powder, and vacuum dry it at 45℃ for 24h to obtain a linear polymer precursor. Take 0.5g of linear polymer precursor and 0.2g of cinnamoyl chloride and dissolve them in 10mL of N,N-dimethylformamide solution, then add 0.12mL of triethylamine, react at 50℃ for 10h, pour the reaction solution into 80mL of industrial alcohol, collect the solid powder, and vacuum dry it at 45℃ for 24h to obtain a photopolymerizable linear polymer.

[0060] Step 2, dissolving 1.84g of pyromellitic anhydride in 5mL of N,N-dimethylformamide, dissolving 1.24g of 1,4-diaminobenzene in 5mL of N,N-dimethylformamide; adding the pyromellitic anhydride solution dropwise into the 1,4-diaminobenzene solution (addition time is 0.8h), stirring at room temperature for 4h after the addition is completed, heating to 100°C and continuing the reaction for 12h, and separating and purifying by column (eluent v (ethyl acetate): v (petroleum ether) = 1:5) to obtain an imide precursor; taking 1g of the imide precursor and 0.4g of cinnamoyl chloride and dissolving them in 12mL of N,N-dimethylformamide solution, adding 0.2mL of triethylamine, reacting at 50°C for 8h, separating and purifying by column (eluent v (ethyl acetate): v (petroleum ether) = 1:5) to obtain a photopolymerizable imide monomer.

[0061] Step 3: Dissolve 0.8 g of photopolymerizable linear polymer, 0.08 g of photopolymerizable imide monomer and 0.08 g of vinyl cinnamate in 3 mL of N,N-dimethylformamide, and add the resulting solution dropwise into 30 mL of deionized water while stirring rapidly (300 r / min). Use a UV curing lamp (100 mW / cm 2 After the reaction, the polyimide nano resin was obtained by freeze drying at -50°C.

[0062] 1.5 g of polyethylene glycol monomethyl ether (average molecular weight 1500) was dissolved in 8 mL of a mixed solution of N, N-dimethylformamide and deionized water (v:v=1:1), and NaH (36 mg) was added. The mixture was stirred at room temperature for 40 min to obtain a mixed solution A. 0.1 g of polyimide nanoresin was added to the mixed solution A and stirred at room temperature for 40 min. After the reaction, the mixture was dialyzed in a 7000 Da dialysis bag and an ethanol solution to obtain a water-dispersible photocurable polyimide nanoresin.

[0063] Example 3

[0064] Step 1, take 0.5mL of 4-vinylaniline, 1.5mL of methyl acrylate, and 10mL of N, N-dimethylformamide and add them to a 25mL reaction bottle, and introduce nitrogen to exclude air for 60min. Add 30mg of azobisisobutyronitrile and heat to 90℃ for reaction for 16h. After the reaction is completed, pour the reaction solution into 100mL of industrial alcohol, collect the solid powder, and vacuum dry it at 45℃ for 36h to obtain a linear polymer precursor. Take 0.5g of linear polymer precursor and 0.3g of cinnamoyl chloride and dissolve them in 15mL of N, N-dimethylformamide solution, then add 0.15mL of triethylamine, react at 50℃ for 12h, pour the reaction solution into 100mL of industrial alcohol, collect the solid powder, and vacuum dry it at 45℃ for 36h to obtain a photopolymerizable linear polymer.

[0065] Step 2, dissolving 2.18g of pyromellitic anhydride in 5mL of N,N-dimethylformamide, dissolving 2.16g of 1,4-diaminobenzene in 5mL of N,N-dimethylformamide; adding the pyromellitic anhydride solution dropwise into the 1,4-diaminobenzene solution (addition time is 1h), stirring at room temperature for 6h after the addition is completed, heating to 150°C and continuing to react for 18h, and separating and purifying by column (eluent v (ethyl acetate): v (petroleum ether) = 1:5) to obtain an imide precursor; taking 1g of the imide precursor and 0.6g of cinnamoyl chloride and dissolving them in 15mL of N,N-dimethylformamide solution, adding 0.3mL of triethylamine, reacting at 50°C for 12h, and separating and purifying by column (eluent v (ethyl acetate): v (petroleum ether) = 1:5) to obtain a photopolymerizable imide monomer.

[0066] Step 3: Dissolve 1.0 g of photopolymerizable linear polymer, 0.1 g of photopolymerizable imide monomer and 0.1 g of vinyl cinnamate in 4 mL of N,N-dimethylformamide, and add the resulting solution dropwise into 40 mL of deionized water while stirring rapidly (300 r / min). Use a UV curing lamp (150 mW / cm 2 After the reaction, the polyimide nano resin was obtained by freeze drying at -70°C.

[0067] 2 g of polyethylene glycol monomethyl ether (average molecular weight 1900) was dissolved in 10 mL of a mixed solution of N, N-dimethylformamide and deionized water (v:v=1:1), NaH (48 mg) was added, and the mixture was stirred at room temperature for 60 min to obtain a mixed solution A. 0.2 g of polyimide nanoresin was added to the mixed solution A and stirred at room temperature for 60 min. After the reaction, the mixture was dialyzed in a 7000 Da dialysis bag and an ethanol solution to obtain a water-dispersible photocurable polyimide nanoresin.

[0068] The invention constructs a method for preparing a novel polyimide nano resin; mainly preparing a photopolymerizable linear polymer and a photopolymerizable imide monomer, and combining them with vinyl cinnamate (photopolymerizable and free radical polymerizable); cyclizing the double bonds of cinnamate under ultraviolet light to obtain a nano resin, which retains the double bonds of vinyl ester. The nano resin is further modified by polyethylene glycol monoether to obtain a water-dispersible nano resin.

Claims

1. A method for preparing water-dispersible photocurable polyimide nanoresin, Features: The specific steps include: Step 1, preparing a photopolymerizable linear polymer; The specific process of step 1 is as follows: Step 1.1, add 0.1mL-0.5mL of 4-vinylaniline, 1mL-1.5mL of methyl acrylate, and 2mL-10mL of N,N-dimethylformamide into a reaction bottle, introduce nitrogen to exclude air for 30min-60min, add 10mg-30mg of azobisisobutyronitrile, heat to 80℃~90℃ and react for 8h-16h. After the reaction is completed, pour the reaction solution into 50mL-100mL of industrial alcohol, collect the solid powder, and vacuum dry it for 12h-36h to obtain a linear polymer precursor; Step 1.2, take 0.5 g of linear polymer precursor and 0.1-0.3 g of cinnamoyl chloride and dissolve them in 5 mL-15 mL of N, N-dimethylformamide solution, then add 0.05 mL-0.15 mL of triethylamine, react for 4 h-12 h, pour the reaction solution into 50 mL-100 mL of industrial alcohol, collect the solid powder, and vacuum dry it for 12-36 h to obtain a photopolymerizable linear polymer; Step 2, preparing a photopolymerizable imide monomer; The specific process of step 2 is: Step 2.1, dissolving 1.09 g to 2.18 g of pyromellitic anhydride in N, N-dimethylformamide to obtain a pyromellitic anhydride solution; dissolving 1.08 g to 2.16 g of 1,4-diaminobenzene in N, N-dimethylformamide to obtain a 1,4-diaminobenzene solution; Step 2.2, adding the pyromellitic anhydride solution dropwise into the 1,4-diaminobenzene solution, stirring for 3h-6h after the addition is completed, heating to 80°C-150°C and continuing the reaction for 6h-18h, and separating and purifying by column to obtain an imide precursor; Step 2.3, take 1 g of the imide precursor and 0.3 g-0.6 g of cinnamoyl chloride and dissolve them in 10 mL-15 mL of N, N-dimethylformamide solution, then add 0.1 mL-0.3 mL of triethylamine, react for 4 h-12 h, separate and purify by column to obtain a photopolymerizable imide monomer; Step 3, preparing a water-dispersible photocurable polyimide nano resin according to the products obtained in step 1 and step 2; the specific process of step 3 is: Step 3.1, preparing polyimide nano resin; the specific process of step 3.1 is: 0.5 g to 1.0 g of a photopolymerizable linear polymer, 0.05 g to 0.1 g of a photopolymerizable imide monomer, and 0.05 g to 0.1 g of vinyl cinnamate are dissolved in 2 mL to 4 mL of N, N-dimethylformamide to obtain a mixed solution B, and the mixed solution B is added dropwise into 20 mL to 40 mL of deionized water while being added dropwise and stirred, and irradiated with an ultraviolet curing lamp for 10 s to 60 s. After the reaction is completed, freeze-drying is performed at -70°C to -30°C to obtain a polyimide nanoresin; Step 3.2, dissolving 1 g to 2 g of polyethylene glycol monomethyl ether in 5 mL to 10 mL of a mixed solution of N, N-dimethylformamide and deionized water, adding 24 mg to 48 mg of NaH, and stirring the mixture for 30 min to 60 min to obtain a mixed solution A; Step 3.3, take 0.1g-0.2g of polyimide nano resin, add it to the mixed solution A obtained in step 3.2, stir at room temperature for 30min-60min, and dialyze after the reaction to obtain water-dispersible photocurable polyimide nano resin.