A method for preparing high-strength fiber-reinforced synthetic resin composite material

By adopting a multi-layer structure high-strength fiber-reinforced synthetic resin composite preparation method in polyamide-imide synthetic resin, using a skeleton sandwich structure and a specific slurry composition, the problem of polyamide-imide synthetic resin under impact and extrusion is solved. Solve the deformation problem, achieve high strength and high toughness material preparation, and improve the thermal stability and thermal conductivity of the material.

CN117887212BActive Publication Date: 2024-10-11深圳市深赛尔股份有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410059428.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-16
Publication Date
2024-10-11
Estimated Expiration
2044-01-16

AI Technical Summary

Technical Problem

Existing polyamide-imide synthetic resins have high costs during the production process, and their performance is difficult to accurately control. They are also prone to deformation and reduced toughness under conditions such as impact and extrusion, making it difficult to achieve the goal of high hardness and rigidity.

Method used

A multi-layer structure of high-strength fiber-reinforced synthetic resin composite material preparation method is adopted, using glass fiber and silicon carbide fiber skeleton, combined with a slurry of polyacrylate, calcium stearate, polyamide-imide copolymer and silicone defoamer The material is formed into a material with high strength and toughness through ultrasonic dispersion and roll solidification technology.

Benefits of technology

A high-strength fiber-reinforced synthetic resin composite material with a heat distortion temperature ≥294°C, a tensile strength ≥838MPa, a bending strength ≥283MPa and a compressive strength ≥286MPa has been achieved, which improves the thermal stability and thermal conductivity of the material and reduces the The effect of bubbles enhances the overall performance of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004665910900000121
    Figure BDA0004665910900000121
  • Figure BDA0004665910900000122
    Figure BDA0004665910900000122
  • Figure BDA0004665910900000131
    Figure BDA0004665910900000131
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-strength fiber-reinforced synthetic resin composite material. The preparation method comprises the following steps: synthesizing a slurry composed of a polyamide-imide copolymer solution, a polyacrylate with a siloxane structure, and an organosilicon defoamer, weaving a skeleton with glass fiber and a silicon carbide fiber bundle, wherein the lower surface of the skeleton is an aramid fiber layer, and the upper surface is slurry. After the air is exhausted, an aramid fiber layer is covered on the uppermost surface, the aramid fiber layer is sent into a rolling device, and epoxy resin is sprayed therein for rolling and pressing, and the high-strength fiber-reinforced synthetic resin composite material is obtained after curing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials, in particular to a method for preparing a high-strength fiber-reinforced synthetic resin composite material. Background Art

[0002] Polyamide-imide synthetic resin has the characteristics of high strength and high wear resistance, and is often used in aerospace, military, automobile and other industries, such as making aircraft parts, engine casings, etc. However, its production cost is too high, and the production process is difficult to accurately control. The performance of the generated polyamide-imide is often affected by the production conditions and the external environment, and the expected results of the researchers are often not obtained, and the performance of the polyamide-imide shear force is weakened. When it is hit and squeezed, the polyamide-imide is prone to deformation. In addition, when the researchers are pursuing the development of a polyamide-imide synthetic resin with high hardness and high rigidity, its toughness is easy to reduce, the resin becomes brittle, and the tensile capacity is reduced. Usually, epoxy resins are added for modification, but the amount of modified resins is difficult to control, which is easy to reduce the performance of the synthetic resin. The high-strength fiber-reinforced synthetic resin composite material prepared by the preparation method of a high-strength fiber-reinforced synthetic resin composite material of the present invention is modified by fillers, and different resins are added to expand the performance of polyamide-imide, and a structure containing a skeleton sandwich is designed to withstand the impact caused by impact and extrusion. Summary of the invention

[0003] The purpose of the present invention is to solve the above deficiencies in the prior art and to propose a method for preparing a high-strength fiber-reinforced synthetic resin composite material.

[0004] The invention provides a method for preparing a high-strength fiber-reinforced synthetic resin composite material. The high-strength fiber-reinforced synthetic resin composite material comprises a skeleton woven from intermediate glass fibers and silicon carbide fibers, a slurry on the skeleton, an aramid layer under the skeleton and an aramid layer on the slurry.

[0005] Furthermore, the raw materials for preparing the slurry include: polyacrylate, calcium stearate, polyamide-imide copolymer and silicone defoamer.

[0006] Furthermore, the slurry raw materials are prepared by weight, including 20 parts of polyacrylate, 5 parts of calcium stearate, 40 parts of polyamide-imide copolymer and 2 parts of silicone defoamer.

[0007] Furthermore, the raw materials for preparing the polyamide-imide copolymer include: N,N-dimethylacetamide, 2,2'-bis(trifluoromethyl)benzidine, 4,4'-(hexafluoroisopropyl)diphthalic anhydride, terephthaloyl chloride, N,N-dimethylacetamide, pyridine, acetic anhydride and propylene oxide.

[0008] Furthermore, the raw materials for preparing the polyamide-imide copolymer include, by weight, 45 to 55 parts of N,N-dimethylacetamide, 3 to 4 parts of 2,2′-bis(trifluoromethyl)benzidine, 1.5 to 2 parts of 4,4′-(hexafluoroisopropyl)diphthalic anhydride, 1.6 to 1.65 parts of terephthaloyl chloride, 3 to 8 parts of N,N-dimethylacetamide, 1 to 1.3 parts of pyridine, 0.2 to 0.6 parts of acetic anhydride and 1.7 to 1.8 parts of propylene oxide.

[0009] Furthermore, the raw materials for preparing the polyacrylate include: toluene, xylene, azobisisoheptanenitrile, methyl methacrylate, ethyl methacrylate, butyl acrylate, octyl acrylate and vinyltrimethoxysilane.

[0010] Furthermore, the raw materials for preparing the polyacrylate include, by weight, 80 to 120 parts of toluene, 30 to 50 parts of xylene, 1 to 2 parts of azobisisoheptanenitrile, 15 to 25 parts of methyl methacrylate, 15 to 25 parts of ethyl methacrylate, 50 to 70 parts of butyl acrylate, 70 to 90 parts of octyl acrylate and 4 to 8 parts of vinyltrimethoxysilane.

[0011] Furthermore, the skeleton is composed of glass fiber bundles and silicon carbide fiber bundles.

[0012] Furthermore, the high-strength fiber-reinforced synthetic resin composite material is prepared by weaving glass fiber bundles and silicon carbide fiber bundles as warp and weft respectively to form a skeleton structure after weaving; coating an aramid fiber layer on the lower surface of the skeleton structure, and spraying a slurry on the upper surface of the skeleton structure; the slurry is: ground polyacrylate and calcium stearate are placed in a polyamide-imide copolymer solution, an organosilicon defoamer is added, and then a suspension is prepared by ultrasonic dispersion; after spraying, drying is performed, and after drying, the air in the skeleton structure is discharged by ultrasonic oscillation, and after the discharge is completed, a layer of aramid fiber layer is coated on the upper surface to obtain a semi-finished product; the semi-finished product is sent to a rolling device, atomized epoxy resin is sprayed in at 160°C and in a vacuum state, and roller pressing is performed, and after pressing, it is cured at 240°C for 3 hours to obtain a high-strength fiber-reinforced synthetic resin composite material.

[0013] Furthermore, after the pressing, the material is cured at 240° C. for 3 hours to obtain a high-strength fiber-reinforced synthetic resin composite material.

[0014] The high-strength fiber-reinforced synthetic resin composite material proposed by the present invention has a heat deformation temperature of ≥294°C, a tensile strength of ≥838MPa, a bending strength of ≥283MPa and a compressive strength of ≥286MPa.

[0015] The present invention provides a method for preparing a high-strength fiber-reinforced synthetic resin composite material, which has the following beneficial effects:

[0016] 1. The present invention prepares a high-strength fiber-reinforced synthetic resin composite material with a four-layer structure, uses a variety of fibers: glass fiber, aramid fiber and silicon carbide fiber as fillers to form a structure with a skeleton sandwich; fills the skeleton with a slurry formed by polyacrylate, calcium stearate, polyamide-imide copolymer and silicone defoamer, and finally cures and cross-links the polyamide-imide copolymer with epoxy resin, and utilizes the modification of the rigidity and hardness of the physical structure of the filler and the modification of the toughness and flexibility of the polyamide-imide copolymer by polyacrylate, silicone defoamer and epoxy resin, so that a synthetic resin having high strength is prepared;

[0017] 2. The polyamide-imide copolymer produced by the present invention does not require additional filtering and purification processes;

[0018] 3. The polyacrylate and silicone defoamer in the formed slurry have a siloxane structure, which has high viscosity, high strength, high abrasion resistance, and excellent thermal conductivity and high temperature resistance. It can tightly bond calcium stearate and polyamide-imide, and enable the slurry to quickly transfer the high temperature of the aramid fiber layer to the skeleton and the bottom aramid fiber layer during the reaction, and quickly connect and diffuse the external force.

[0019] 4. The added epoxy resin is cross-linked and cured with polyamide-imide, while the silicone defoamer and ultrasonic vibration method successively reduce the influence of bubbles formed in the reaction on the resin properties, making the synthetic resin structure tighter. DETAILED DESCRIPTION

[0020] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0021] Unless otherwise specified, the examples and comparative examples are parallel tests with the same components, component contents, preparation steps and preparation parameters. The experimental methods in the following examples are conventional methods unless otherwise specified. The experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.

[0022] The sources of the materials mentioned in the present invention are as follows: the organosilicon defoamer is purchased from Dongguan Guozhong New Materials Research Institute Co., Ltd., with a content of 99%, model DU-159; the epoxy resin is bisphenol A type epoxy resin (product name NPEL-127L) purchased from Guangzhou Jingyi New Materials Co., Ltd.

[0023] Unless otherwise specified, all reagents were used as received without further purification. The flask was equipped with a mechanical stirrer, a nitrogen inlet, and a reflux condenser. The N,N-dimethylacetamide and γ-butyrolactone used were of chromatographic grade, and other reagents were of analytical grade unless otherwise specified. All 4,4′-(hexafluoroisopropylidene)diphthalic anhydride, 4,4′-(hexafluoroisopropylidene)diphthalic anhydride, and terephthaloyl chloride used were placed in the reaction vessel in a powdered state at one time in each step to avoid contact with air as much as possible.

[0024] The fineness of the aramid fiber is 1000D-2000D; in the aramid fiber layer, the gaps between the aramid fibers are all less than 50 μm.

[0025] In the preparation examples and embodiments of the present invention, the "parts" are parts by weight unless otherwise specified.

[0026] Example 1

[0027] Add 50 parts of N,N-dimethylacetamide, 3.6 parts of 2,2'-bis(trifluoromethyl)benzidine and 1.8 parts of 4,4'-(hexafluoroisopropyl)diphthalic anhydride to a flask under nitrogen flow at room temperature, and stir for 2 hours. After cooling the flask to 0°C in an ice bath, add 1.62 parts of terephthaloyl chloride and stir for 10 minutes. Add 6 parts of N,N-dimethylacetamide and stir for 3 hours while allowing the ambient temperature to rise to room temperature. Then add 1.18 parts of pyridine and 0.43 parts of acetic anhydride, stir at room temperature for 30 minutes, and stir for further 60 minutes at 70°C. After cooling to room temperature, add 1.74 parts of propylene oxide and stir for 12 hours to obtain a polyamide-imide copolymer solution.

[0028] Add 1 part of initiator azobisisoheptanenitrile to 100 parts of toluene and 40 parts of xylene, and then add 20 parts of methyl methacrylate, 20 parts of ethyl methacrylate, 60 parts of butyl acrylate, and 80 parts of octyl acrylate in sequence, react at 70°C for 10 hours, and then add 6 parts of vinyltrimethoxysilane to obtain a polyacrylate containing a siloxane structure.

[0029] 13 parts of glass fiber bundles and 15 parts of silicon carbide fiber bundles are woven as warp and weft respectively, and the surface density of the woven fiber is 140g / m 2, after weaving, a skeleton structure is formed; an aramid fiber layer is coated on the lower surface of the skeleton structure, and a slurry is sprayed on the upper surface of the skeleton structure; the slurry is: 20 parts of polyacrylate containing a siloxane structure are ground to 10-15μm, 5 parts of calcium stearate are ground to 10-15μm, placed in 40 parts of a polyamide-imide copolymer solution, and then prepared into a suspension by ultrasonic dispersion. After spraying, drying is carried out. After drying, the air in the skeleton structure is discharged by ultrasonic oscillation. After the discharge is completed, a layer of aramid fiber layer is coated on the upper surface to obtain a semi-finished product. 30 parts of the semi-finished product are sent to a rolling device, 60 parts of atomized epoxy resin are sprayed at 140°C and vacuum, and roller pressing is carried out. After pressing, it is cured at 240°C for 3h to obtain a high-strength fiber-reinforced synthetic resin composite material.

[0030] The rolling device includes: an encapsulated vacuum chamber, a pressing roller group, an infrared radiation temperature adjustment group, a temperature monitoring group, an epoxy resin heating tank, an epoxy resin pump, an insulating epoxy resin conduit, an epoxy resin atomizing nozzle, and a rolling process control processor; the encapsulated vacuum chamber is fully sealed and wrapped in the outer layer of the rolling device, and is evacuated by a vacuum pump. The encapsulated vacuum chamber is provided with a material inlet and outlet. When the material is in and out, the material inlet and outlet are opened. After the material is in and out, the material inlet and outlet are closed. Sealing strips are provided at the edges of the material inlet and outlet and at the edges in contact with the material; the infrared radiation temperature adjustment group includes: a semi-finished product preheating infrared radiation source and a curing heating infrared radiation source; the temperature monitoring group monitors the semi-finished product temperature, the epoxy resin temperature and the curing temperature after pressing through the first temperature sensor, the second temperature sensor and the third temperature sensor respectively; the temperature signal of the temperature monitoring group is reflected The heat-insulating epoxy resin conduit is connected to the epoxy resin atomizing nozzle through the heat-insulating epoxy resin conduit; the heat-insulating epoxy resin conduit includes: a conduit outer insulation layer, a conduit anti-folding protective layer and a conduit inner layer; the conduit outer insulation layer is a flexible insulation material, which is wrapped outside the conduit anti-folding protective layer; the conduit inner layer is an anti-oxidation surface passivated copper tube; the conduit anti-folding protective layer is a stainless steel wire braided mesh, which is wrapped outside the conduit inner wall; the flexible insulation material includes: diene foam, hydrocarbon foam elastomer or nitrile rubber foam;

[0031] More precise temperature control can be achieved; the vacuum degree of the rolling process is higher through the fully sealed encapsulation of the vacuum chamber; the epoxy resin atomization is more precise and the temperature is more accurate, which greatly reduces the temperature loss of the epoxy resin pipe transportation and the temperature difference of the atomization spraying process;

[0032] The vacuum pump is used to evacuate the entire sealed vacuum cavity wrapped in the outer layer of the rolling device into a vacuum state; the semi-finished product is preheated to the semi-finished product preheating set temperature through the first infrared radiation of the semi-finished product preheating infrared radiation source; the epoxy resin is heated to the first set temperature through the epoxy resin heating tank; the epoxy resin pump extracts and pumps the epoxy resin to the epoxy resin atomizing nozzle; the epoxy resin atomizing nozzle sprays a preset amount of atomized epoxy resin, and then sends it to the pressing roller group for roller pressing and laminating; after laminating, it is sent to the infrared radiation temperature adjustment group to the post-pressing curing infrared radiation area, the third temperature sensor monitors the curing temperature after pressing, and the pressed material is heated by the second infrared radiation of the curing heating infrared radiation source Heating to a set curing temperature; curing at the set curing temperature for a set curing time to obtain a high-strength fiber-reinforced synthetic resin composite material; the semi-finished product preheating set temperature includes: 140°C or 160°C; the first set temperature includes: 142°C or 162°C, wherein 142°C is a cooling compensation set temperature for the temperature of the epoxy resin after atomization due to the decrease in the external temperature when the semi-finished product preheating set temperature is 140°C, and the epoxy resin atomization temperature is kept accurately controlled to be not less than 140°C; 162°C is a cooling compensation set temperature for the temperature of the epoxy resin after atomization due to the decrease in the external temperature when the semi-finished product preheating set temperature is 160°C, and the epoxy resin atomization temperature is kept accurately controlled to be not less than 160°C;

[0033] The roller pressing process is more accurately controlled, which significantly improves the actual preheating temperature of the semi-finished product. Compared with the hot air heating or electric heating wire heating in the prior art, which is difficult to heat objects in a full vacuum state, the infrared radiation heating of the present invention is more suitable for precise heating in a full vacuum environment, which greatly improves the heating efficiency and heating accuracy in a vacuum environment, and greatly improves the temperature constancy of the curing process; the fully enclosed roller vacuum chamber allows the curing process to remain in a vacuum state, avoiding the influence of external air dust and impurities on the curing process, and significantly improving the cleanliness of the materials in the curing process.

[0034] Example 2

[0035] Add 45 parts of N,N-dimethylacetamide, 3 parts of 2,2'-bis(trifluoromethyl)benzidine and 1.5 parts of 4,4'-(hexafluoroisopropyl)diphthalic anhydride to a flask under nitrogen flow at room temperature, and stir for 2 hours. After cooling the flask to 0°C in an ice bath, add 1.6 parts of terephthaloyl chloride and stir for 8 minutes. Add 3 parts of N,N-dimethylacetamide and stir for 2 hours while allowing the ambient temperature to rise to room temperature. Then add 1 part of pyridine and 0.2 parts of acetic anhydride, stir at room temperature for 25 minutes, and stir for further 60 minutes at 55°C. After cooling to room temperature, add 1.7 parts of propylene oxide and stir for 12 hours to obtain a polyamide-imide copolymer solution.

[0036] Add 1 part of initiator azobisisoheptanenitrile to 80 parts of toluene and 30 parts of xylene, and then add 15 parts of methyl methacrylate, 15 parts of ethyl methacrylate, 15 parts of butyl acrylate, and 50 parts of octyl acrylate in sequence, react at 70°C for 9 hours, and then add 4 parts of vinyltrimethoxysilane to obtain a polyacrylate containing a siloxane structure.

[0037] 13 parts of glass fiber bundles and 15 parts of silicon carbide fiber bundles are woven as warp and weft respectively, and the surface density of the woven fiber is 140g / m 2 , after weaving, a skeleton structure is formed; an aramid fiber layer is coated on the lower surface of the skeleton structure, and a slurry is sprayed on the upper surface of the skeleton structure; the slurry is: 20 parts of polyacrylate containing a siloxane structure are ground to 10-15μm, 5 parts of calcium stearate are ground to 10-15μm, placed in 40 parts of a polyamide-imide copolymer solution, and then prepared into a suspension by ultrasonic dispersion. After spraying, drying is carried out. After drying, the air in the skeleton structure is discharged by ultrasonic oscillation. After the discharge is completed, a layer of aramid fiber layer is coated on the upper surface to obtain a semi-finished product. 30 parts of the semi-finished product are sent to a rolling device, 60 parts of atomized epoxy resin are sprayed at 160°C and vacuum, and roller pressing is carried out. After pressing, it is cured at 240°C for 3h to obtain a high-strength fiber-reinforced synthetic resin composite material.

[0038] Example 3

[0039] Add 55 parts of N,N-dimethylacetamide, 4 parts of 2,2'-bis(trifluoromethyl)benzidine and 2 parts of 4,4'-(hexafluoroisopropyl)diphthalic anhydride to a flask under nitrogen flow at room temperature, and stir for 2 hours. After cooling the flask to 0°C in an ice bath, add 1.65 parts of terephthaloyl chloride and stir for 12 minutes. Add 8 parts of N,N-dimethylacetamide and stir for 4 hours while allowing the ambient temperature to rise to room temperature. Then add 1.3 parts of pyridine and 0.6 parts of acetic anhydride, stir at room temperature for 40 minutes, and stir for further 70 minutes at 70°C. After cooling to room temperature, add 1.8 parts of propylene oxide and stir for 12 hours to obtain a polyamide-imide copolymer solution.

[0040] Add 2 parts of initiator azobisisoheptanenitrile to 120 parts of toluene and 50 parts of xylene, and then add 25 parts of methyl methacrylate, 25 parts of ethyl methacrylate, 70 parts of butyl acrylate, and 90 parts of octyl acrylate in sequence, react at 70°C for 10 hours, and then add 8 parts of vinyltrimethoxysilane to obtain a polyacrylate containing a siloxane structure.

[0041] 13 parts of glass fiber bundles and 15 parts of silicon carbide fiber bundles are woven as warp and weft respectively, and the surface density of the woven fiber is 140g / m 2, after weaving, a skeleton structure is formed; an aramid fiber layer is coated on the lower surface of the skeleton structure, and a slurry is sprayed on the upper surface of the skeleton structure; the slurry is: 20 parts of polyacrylate containing a siloxane structure are ground to 10-15μm, 5 parts of calcium stearate are ground to 10-15μm, placed in 40 parts of a polyamide-imide copolymer solution, and then prepared into a suspension by ultrasonic dispersion. After spraying, drying is carried out. After drying, the air in the skeleton structure is discharged by ultrasonic oscillation. After the discharge is completed, a layer of aramid fiber layer is coated on the upper surface to obtain a semi-finished product. 30 parts of the semi-finished product are sent to a rolling device, and 60 parts of atomized epoxy resin are sprayed in a vacuum state of 160°C and 0.05MPa, and roller pressing is carried out at a pressure of 0.05MPa. After pressing, it is cured at 240°C for 3h to obtain a high-strength fiber-reinforced synthetic resin composite material.

[0042] The difference between Comparative Example 1 and Example 1 is that no silicone oil defoamer is added.

[0043] The difference between Comparative Example 2 and Example 1 is that 20 parts of polyacrylate containing silicone structure are ground to 50-60 μm, and 5 parts of calcium stearate are ground to 50-60 μm.

[0044] The difference between Comparative Example 3 and Example 1 is that 10 parts of polyacrylate containing silicone structure are ground to 10-15 μm, and 5 parts of calcium stearate are ground to 10-15 μm.

[0045] The difference between Comparative Example 4 and Example 1 is that 30 parts of polyacrylate containing silicone structure are ground to 10-15 μm, and 5 parts of calcium stearate are ground to 10-15 μm.

[0046] The difference between Comparative Example 5 and Example 1 is that the polyacrylate containing a siloxane structure in Example 1 is replaced by an equal weight portion of polyacrylate without a siloxane structure.

[0047] Performance Testing

[0048] 1. Thermogravimetric analysis (TGA) test

[0049] The thermal weight loss of the cured products prepared in Examples 1 to 3 and Comparative Example 1 was tested under air and nitrogen conditions, respectively. The specific conditions of the experiment were: starting at 50°C, then heating to 800°C at a rate of 20°C / min, using nitrogen or air as the carrier gas, with a flow rate of 20 mL / min. The results are shown in Table 1.

[0050] Table 1

[0051]

[0052] It can be seen from Table 1 that the thermal stability of Examples 1-3 is better. Under the same test conditions, the higher the temperature result value, the better the thermal stability.

[0053] 2. Other performance tests

[0054] Other tests were performed on Examples 1 to 3 and Comparative Examples 1 to 5, and the results are shown in Table 2.

[0055] Table 2

[0056]

[0057]

[0058] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for preparing a high-strength fiber-reinforced synthetic resin composite material, characterized in that: The high-strength fiber-reinforced synthetic resin composite material is prepared by weaving a skeleton formed by intermediate glass fibers and silicon carbide fibers, a slurry on the skeleton, an aramid layer under the skeleton, and an aramid layer on the slurry; the slurry raw materials are prepared by weight, including 20 parts of polyacrylate, 5 parts of calcium stearate, 40 parts of polyamide-imide copolymer, and 2 parts of silicone defoaming agent; the high-strength fiber-reinforced synthetic resin composite material is prepared by weaving glass fiber bundles and silicon carbide fiber bundles as warp and weft respectively, and forming a skeleton structure after weaving; coating the aramid fiber layer on the lower surface of the skeleton structure, and spraying the slurry on the upper surface of the skeleton structure. The slurry is as follows: polyacrylate ground to 10-15 μm and calcium stearate ground to 10-15 μm are placed in a polyamide-imide copolymer solution, an organosilicon defoamer is added, and then a suspension is prepared by ultrasonic dispersion; after spraying, drying is performed, and after drying, the air in the skeleton structure is discharged by ultrasonic oscillation, and after the discharge is completed, a layer of aramid fiber layer is coated on the upper surface to obtain a semi-finished product; the semi-finished product is sent to a rolling device, atomized epoxy resin is sprayed at 160° C. and in a vacuum state, and rolling and pressing are performed, and after pressing, curing is performed to obtain a high-strength fiber-reinforced synthetic resin composite material.

2. The method for preparing a high-strength fiber-reinforced synthetic resin composite material according to claim 1, characterized in that: The raw materials for preparing the polyamide-imide copolymer include: N, N-dimethylacetamide, 2, 2'-bis(trifluoromethyl)benzidine, 4, 4'-(hexafluoroisopropylidene) diphthalic anhydride, terephthaloyl chloride, N, N-dimethylacetamide, pyridine, acetic anhydride and propylene oxide.

3. The method for preparing a high-strength fiber-reinforced synthetic resin composite material according to claim 1, characterized in that: The raw materials for preparing the polyamide-imide copolymer include, by weight, 45-55 parts of N,N-dimethylacetamide, 3-4 parts of 2,2'-bis(trifluoromethyl)benzidine, 1.5-2 parts of 4,4'-(hexafluoroisopropylidene)diphthalic anhydride, 1.6-1.65 parts of terephthaloyl chloride, 3-8 parts of N,N-dimethylacetamide, 1-1.3 parts of pyridine, 0.2-0.6 parts of acetic anhydride and 1.7-1.8 parts of propylene oxide.

4. The method for preparing a high-strength fiber-reinforced synthetic resin composite material according to claim 1, characterized in that: The raw materials for preparing the polyacrylate include: toluene, xylene, azobisisoheptanenitrile, methyl methacrylate, ethyl methacrylate, butyl acrylate, octyl acrylate and vinyl trimethoxysilane.

5. The method for preparing a high-strength fiber-reinforced synthetic resin composite material according to claim 1, characterized in that: The raw materials for preparing the polyacrylate include, by weight: 80-120 parts of toluene, 30-50 parts of xylene, 1-2 parts of azobisisoheptanenitrile, 15-25 parts of methyl methacrylate, 15-25 parts of ethyl methacrylate, 50-70 parts of butyl acrylate, 70-90 parts of octyl acrylate and 4-8 parts of vinyltrimethoxysilane.

6. The method for preparing a high-strength fiber-reinforced synthetic resin composite material according to claim 1, characterized in that: After the pressing, the composite material is cured at 240° C. for 3 hours to obtain a high-strength fiber-reinforced synthetic resin composite material.