A kind of amorphous wire material with high soft magnetic properties and its preparation method and application

By applying DC current annealing treatment to the as-cast amorphous wire in a vacuum environment, the coercive force problem caused by residual internal stress in the preparation of cobalt-based amorphous wire is solved, and its soft magnetic properties are improved, making it suitable for precision electronic devices. and high-sensitivity sensors.

CN117904561BActive Publication Date: 2024-10-22DONGGUAN YUMAO NANO TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410079714.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-19
Publication Date
2024-10-22
Estimated Expiration
2044-01-19

AI Technical Summary

Technical Problem

Cobalt-based amorphous wire has large residual internal stress during the preparation process, resulting in a large coercive force Hc, which affects its application as a core material for sensors.

Method used

In the first vacuum environment, DC current is applied to the cast amorphous wire for annealing heat treatment. The residual internal stress is eliminated and the magnetic properties are improved by controlling the current size (30-130mA) and the power-on time (2.5-12.5min).

Benefits of technology

It achieves high saturation magnetic induction intensity, low coercivity, high magnetic permeability and high GMI change rate, improves the soft magnetic properties of amorphous wire, and is suitable for weak magnetic sensors and high-sensitivity detectors.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117904561B_ABST
    Figure CN117904561B_ABST
Patent Text Reader

Abstract

The present invention provides an amorphous wire with high soft magnetic properties and a preparation method and application thereof, belonging to the technical field of amorphous alloy materials. The present invention provides a method for obtaining an amorphous wire with high soft magnetic properties, comprising the following steps: applying a direct current to a cast amorphous wire under a first vacuum environment to obtain an amorphous wire with high soft magnetic properties; the direct current has a magnitude of 30 to 130 mA and a power-on time of 2.5 to 12.5 minutes; the composition of the cast amorphous wire is Co a Fe b Si c B d M e , wherein M is at least two of Nb, V, Zr, Mn, Cu and Ni, and a+b+c+d+e=100; a, b, c, d and e are the atomic percentages of the corresponding elements. The high soft magnetic property amorphous wire material provided by the present invention has high saturation magnetic induction and stress strength, low coercive force, high magnetic permeability, high GMI change rate and high sensitivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of amorphous alloy materials, and in particular relates to an amorphous wire material with high soft magnetic properties and a preparation method and application thereof. Background Art

[0002] Amorphous alloys have metastable structural characteristics and atomic arrangements with short-range order and long-range disorder. Soft magnetic amorphous alloys represented by cobalt-based alloys show the remarkable characteristics of no grains, no crystal defects, and no magnetic anisotropy. Compared with commonly used soft magnetic materials such as silicon steel, NiFe alloy, MnZn alloy, etc., cobalt-based amorphous alloys have the characteristics of high saturation magnetic induction intensity, low coercive force, high magnetic permeability, high GMI change rate and high magnetic field sensitivity.

[0003] Cobalt-based amorphous wire has a special magnetic domain structure, namely bamboo-shaped magnetic domain and core-shell structure. It exhibits many excellent magnetic soft properties, such as high magnetic permeability, high saturation magnetic induction intensity and significant GMI effect, and is widely used in important fields such as weak magnetic sensors and high-sensitivity detectors.

[0004] The Taylor method was first proposed by British scientist Taylor in 1924. The specific operation is to place the alloy ingot in a glass tube with a diameter of about 3 mm, heat it at high temperature until the metal melts, and produce metal wires with a diameter of 1 to 5 mm by pulling and quenching. Ulitovsky improved the Taylor method on the original basis and invented the Taylor-Ulitovsky method. The specific improvement is to add a winding wire collection device on the original basis to achieve automated mass production. This method adjusts the speed of the wire collection motor, and the speed is inversely proportional to the wire diameter. The faster the speed, the thinner the wire. Circular cross-section wires of different thicknesses can be obtained as required, and the diameter can be controlled within the range of 20 to 200 μm. However, the cast samples prepared by the Taylor-Ulitovsky method usually have large residual internal stress, which leads to a large coercive force Hc, affecting its application as a core material for sensors. Summary of the invention

[0005] In view of this, the object of the present invention is to provide an amorphous wire with high soft magnetic properties and a preparation method and application thereof. The amorphous wire with high soft magnetic properties provided by the present invention has high saturation magnetic induction intensity, low coercive force, high magnetic permeability, high GMI change rate and high sensitivity.

[0006] In order to achieve the above object, the present invention provides the following technical solutions:

[0007] The present invention provides a method for obtaining an amorphous wire material with high soft magnetic properties, comprising the following steps:

[0008] Under a first vacuum environment, applying a direct current to the as-cast amorphous wire to obtain an amorphous wire with high soft magnetic properties;

[0009] The magnitude of the direct current is 30-130 mA, and the power-on time is 2.5-12.5 min;

[0010] The composition of the cast amorphous wire is Co a Fe b Si c B d M e , wherein M is at least two of Nb, V, Zr, Mn, Cu and Ni, and a+b+c+d+e=100; a, b, c, d and e are the atomic percentages of the corresponding elements.

[0011] Preferably, the composition of the cast amorphous wire includes Co 68.15 Fe 4.35 Si 11.48 B 14.02 Cu1Nb1, Co 68 Fe 4.5 Si 11.48 B 14.02 Cu1V1 or Co 68 Fe 4.5 Si 11.48 B 14.02 VxV 0.5 Nb 0.5 .

[0012] Preferably, the vacuum degree of the first vacuum environment is 0-10Pa.

[0013] Preferably, the cast amorphous wire is a wire with a circular cross-section.

[0014] Preferably, the diameter of the metal core of the cast amorphous wire is 20-60 μm.

[0015] Preferably, the direct current is a unidirectional constant current.

[0016] Preferably, the method for preparing the cast amorphous wire comprises the following steps:

[0017] Under the conditions of a second vacuum and argon protection, metal raw materials Co, Fe, Si, B and M are melted corresponding to the composition of the cast amorphous wire to obtain a cobalt-based amorphous alloy;

[0018] The cobalt-based amorphous alloy is made into glass-coated amorphous wire by a glass-coating method;

[0019] The glass-coated amorphous wire is placed in a corrosive solution to remove the surface glass layer to obtain the cast amorphous wire material.

[0020] Preferably, the vacuum degree of the second vacuum is ≤10 -3 Pa.

[0021] The present invention provides a high soft magnetic property amorphous wire obtained by the method described in the above scheme, which is composed of Co a Fe b Si c B d M e , wherein M is at least two of Nb, V, Zr, Mn, Cu and Ni, and a+b+c+d+e=100; a, b, c, d and e are the atomic percentages of the corresponding elements; the high soft magnetic property amorphous wire has an effective magnetic permeability μe of 13000-16000 at 1kHz, a saturation magnetic induction intensity Bs of 0.70-0.80T, a coercive force Hc<0.5A / m, and a giant magneto-impedance effect GMI% of 400-450%.

[0022] The present invention provides the application of the amorphous wire material with high soft magnetic properties described in the above scheme in precision electronic devices or high-sensitivity weak magnetic sensors.

[0023] The present invention provides a method for obtaining an amorphous wire with high soft magnetic properties, comprising the following steps: applying a direct current to a cast amorphous wire under a first vacuum environment to obtain an amorphous wire with high soft magnetic properties; the direct current has a magnitude of 30 to 130 mA and a power-on time of 2.5 to 12.5 min; the composition of the cast amorphous wire is Co a Fe b Si c B d M e , wherein M is at least two of Nb, V, Zr, Mn, Cu and Ni, and a+b+c+d+e=100; a, b, c, d and e are the atomic percentages of the corresponding elements.

[0024] In the present invention, Cu has good ductility, and trace doping can improve the continuity and uniformity of the cast wire; large atoms of Nb, V and Zr are helpful to improve the amorphous forming ability of the component (Inoue's three principles: the atomic size difference between the main elements is relatively large, at least more than 12%); by adding Nb and V, the interaction between atoms is mainly changed, the amorphous forming ability can be improved and the magnetostriction coefficient can be changed, so that the negative magnetostriction coefficient is converted into a positive one, thereby improving the soft magnetic properties.

[0025] The present invention uses a direct current of 30 to 130 mA to perform annealing heat treatment on the amorphous wire, which belongs to small-amplitude current annealing. When the current is greater than 130 mA, the amorphous wire is easily burned by the large current, and the Joule heat generated by the large current is sufficient to crystallize the amorphous alloy, thereby causing the coercive force Hc to be high. Similarly, the Joule heat depends on the combined effect of the current size and the power-on time. The longer the power-on time, the more accumulated heat is generated, which is also not conducive to the heat treatment effect. The present invention uses a power-on time of 2.5 to 12.5 minutes. The generated heat can meet the relaxation enthalpy of the amorphous material, improve the magnetic properties by using structural relaxation, and is not enough to crystallize the amorphous wire.

[0026] The heat treatment method provided by the present invention can further improve the soft magnetic properties of amorphous wires, so that they have high saturation magnetic induction intensity, low coercive force, high magnetic permeability, high GMI change rate and high sensitivity, and can be widely used in important fields such as weak magnetic sensors and high-sensitivity detectors.

[0027] Compared with the commonly used heating annealing method, the heat treatment method provided by the present invention has more precise control of heat by current annealing, is simple to operate, and has high preparation efficiency; more importantly, the current Joule heat can better eliminate residual internal stress and realize circumferential excitation of amorphous wire, induce circumferential magnetic field, optimize circumferential magnetic domains, and effectively improve the soft magnetic properties of amorphous wire. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.

[0029] Figure 1 This is a SEM photo of the cast amorphous wire obtained in Comparative Example 1;

[0030] Figure 2 This is a schematic diagram of the direct current annealing principle of amorphous wire in the present invention;

[0031] Figure 3 1 is the XRD diagram of the amorphous wire obtained in Comparative Example 1 and Example 1;

[0032] Figure 4 The differential scanning calorimetry (DSC) spectra of the amorphous wires obtained in Comparative Example 1 and Example 1 are shown;

[0033] Figure 5 The magnetic permeability test spectra of the amorphous wire obtained in Comparative Example 1 and Example 1;

[0034] Figure 6The VSM test spectra of the amorphous wire sample vibrating magnetometer obtained in Comparative Example 1 and Example 1;

[0035] Figure 7 The impedance change rate GMI test graph of the amorphous wire obtained in Comparative Example 1 and Example 1;

[0036] Figure 8 This is a schematic diagram of preparing cast amorphous wire according to the present invention. DETAILED DESCRIPTION

[0037] The present invention provides a method for obtaining an amorphous wire material with high soft magnetic properties, comprising the following steps:

[0038] Under a first vacuum environment, applying a direct current to the as-cast amorphous wire to obtain an amorphous wire with high soft magnetic properties;

[0039] The magnitude of the direct current is 30-130 mA, and the power-on time is 2.5-12.5 min;

[0040] The composition of the cast amorphous wire is Co a Fe b Si c B d M e , wherein M is at least two of Nb, V, Zr, Mn, Cu and Ni, and a+b+c+d+e=100; a, b, c, d and e are the atomic percentages of the corresponding elements.

[0041] In the present invention, the vacuum degree of the first vacuum environment is preferably 0-10Pa, more preferably 10Pa. In the present invention, the cast amorphous wire is preferably a round cross-section wire; the diameter of the metal core of the cast amorphous wire is preferably 20-60μm, more preferably 30-50μm, and more preferably 35-42μm. In the present invention, the composition of the cast amorphous wire preferably includes Co 68.15 Fe 4.35 Si 11.48 B 14.02 Cu1Nb1, Co 68 Fe 4.5 Si 11.48 B 14.02 Cu1V1 or Co 68 Fe 4.5 Si 11.4 8B 14.02 VxV 0.5 Nb 0.5 .

[0042] In the present invention, the magnitude of the direct current is 30-130 mA, specifically 30 mA, 60 mA, 90 mA or 130 mA; the power-on time of the direct current is 2.5-12.5 min, specifically 2.5 min, 5 min, 7.5 min, 10 min or 12.5 min. In the present invention, the direct current is preferably a unidirectional constant current; the error fluctuation range of the direct current is preferably within 3 mA.

[0043] The present invention uses a direct current of 30 to 130 mA to perform annealing heat treatment on the cast amorphous wire, which belongs to small-amplitude current annealing. When the current is greater than 130 mA, the amorphous wire is easily burned by the large current, and the Joule heat generated by the large current is sufficient to crystallize the amorphous alloy, thereby causing the coercive force Hc to be high. Similarly, the Joule heat depends on the combined effect of the current size and the power-on time. The longer the power-on time, the more accumulated heat is generated, which is also not conducive to the heat treatment effect. The present invention uses a power-on time of 2.5 to 12.5 minutes. The generated heat can meet the relaxation enthalpy of the amorphous material, improve the magnetic properties by using structural relaxation, and is not enough to crystallize the amorphous wire.

[0044] The amorphous wire heat treatment principle used in the present invention is as follows Figure 2 As shown, in the first vacuum environment, the two ends of the cast amorphous wire are fixed with current clamps, and a direct current is applied to the amorphous wire through a current source. The current passes through the wire to generate Joule heat and annular magnetizing magnetic field, which can release the residual internal stress of the cast amorphous wire, induce annular magnetic field, improve the distribution of annular magnetic domains, and optimize the soft magnetic properties of the amorphous wire.

[0045] In the present invention, the method for preparing the cast amorphous wire preferably comprises the following steps:

[0046] Under the conditions of a second vacuum and argon protection, metal raw materials Co, Fe, Si, B and M are melted corresponding to the composition of the cast amorphous wire to obtain a cobalt-based amorphous alloy;

[0047] The cobalt-based amorphous alloy is made into glass-coated amorphous wire by a glass-coating method;

[0048] The glass-coated amorphous wire is placed in a corrosive solution to remove the surface glass layer to obtain the cast amorphous wire material.

[0049] In the present invention, under the conditions of a second vacuum and argon protection, metal raw materials Co, Fe, Si, B and M are smelted corresponding to the composition of the cast amorphous wire material to obtain a cobalt-based amorphous alloy.

[0050] In the present invention, the vacuum degree of the second vacuum is preferably ≤10 -3 Pa, more preferably 10 -3Pa; the purity of the metal raw materials Co, Fe, Si, B and M is preferably greater than 99.9wt.%. The present invention has no special requirements for the smelting method, and a smelting method known in the art can be used. In the present invention, the metal raw materials with a purity greater than 99.9wt.% are selected to avoid the introduction of impurities that affect the soft magnetic properties of the alloy. When smelting the alloy, the temperature is ≤10 -3 Pa vacuum environment and argon protection can prevent alloy oxidation from affecting the soft magnetic properties.

[0051] After the smelting is completed, the present invention preferably cuts the obtained cobalt-based amorphous alloy into small cylindrical blocks of 1 to 2 mm.

[0052] After obtaining the cobalt-based amorphous alloy, the present invention adopts a glass coating method to make the cobalt-based amorphous alloy into a glass-coated amorphous wire.

[0053] The present invention has no special requirements for the glass coating method, and any method known in the art may be used.

[0054] After obtaining the glass-coated amorphous wire, the present invention places the glass-coated amorphous wire in a corrosive solution to remove the surface glass layer to obtain the cast amorphous wire material.

[0055] In the present invention, the mass content of hydrofluoric acid in the etching solution is preferably 40%, the mass content of sodium thiocyanate is preferably 0.2%, and the mass content of hexamine is preferably 0.8%. The time for which the glass-coated amorphous wire is placed in the etching solution is preferably 100 to 150 seconds, more preferably 110 to 140 seconds, and more preferably 120 to 130 seconds. The present invention has no special requirements for the amount of etching solution, and it only needs to be able to immerse the glass-coated amorphous wire. The present invention has no special requirements for the preparation of the etching solution, and it can be prepared in a manner well known in the art.

[0056] After removing the surface glass layer, the present invention preferably takes the obtained amorphous wire out of the etching solution and puts it into anhydrous ethanol for ultrasonic cleaning for 3 to 5 times, then air-dries it and then puts it into a vacuum drying oven for storage for later use.

[0057] In the present invention, the ultrasonic frequency is preferably 40,000 to 50,000 Hz, more preferably 45,000 to 47,000 Hz; the ultrasonic power is preferably 15 to 40 W, more preferably 20 to 35 W; the ultrasonic time is preferably 10 to 20 s, more preferably 12 to 15 s.

[0058] The method for preparing the cast amorphous wire provided by the present invention has the advantages of simple operation and short preparation cycle.

[0059] Figure 8This is a schematic diagram of the preparation of cast amorphous wires in the present invention. As shown in the figure, firstly, a mother alloy rod with a diameter of Φ2-4 mm is obtained by suction casting in a vacuum arc furnace, the rod is cut into small cylinders with a length of 1-2 mm by a low-speed cutter, and then the rod is placed in a glass test tube of a wire drawing machine and heated to 950-1050°C by an induction coil, and a continuous and uniform amorphous wire with a length of hundreds of meters can be produced by the wire drawing machine's own wire collecting device.

[0060] The present invention provides a high soft magnetic property amorphous wire material prepared by the method described in the above scheme, which is composed of Co a Fe b Si c B d M e , wherein M is at least two of Nb, V, Zr, Mn, Cu and Ni, and a+b+c+d+e=100; a, b, c, d and e are the atomic percentages of the corresponding elements; the high soft magnetic property amorphous wire has an effective magnetic permeability μe of 13000-16000 at 1kHz, a saturation magnetic induction intensity Bs of 0.70-0.80T, a coercive force Hc<0.5A / m, and a giant magneto-impedance effect GMI% of 400-450%.

[0061] The present invention provides the application of the amorphous wire material with high soft magnetic properties described in the above scheme in precision electronic devices or high-sensitivity weak magnetic sensors.

[0062] The amorphous wire material of the present invention after current heat treatment has excellent soft magnetic properties, high saturation magnetic induction intensity, low coercive force, high magnetic permeability, high GMI change rate and high sensitivity. As a new generation of cobalt-based amorphous microwire material, it can be applied to important fields such as weak magnetic sensors and high-sensitivity detectors.

[0063] In order to further illustrate the present invention, a high soft magnetic property amorphous wire material provided by the present invention and its preparation method and application are described in detail below in combination with the accompanying drawings and embodiments, but they should not be understood as limiting the protection scope of the present invention.

[0064] Example 1

[0065] In 10 -3 Pa and under the condition of argon protection, metal raw materials Co, Fe, Si, B, Cu and Nb with purity greater than 99.9wt.% are smelted to obtain Co 68.15 Fe 4.35 Si 11.48 B 14.02 The cobalt-based amorphous alloy of Cu1Nb1 is then cut into small cylindrical blocks of 1 to 2 mm;

[0066] The cut cobalt-based amorphous alloy small cylindrical blocks are prepared into glass-coated amorphous wires by using a glass coating method, and the glass coating method is shown in Example 1 of the patent publication number CN114015957B;

[0067] The glass-coated amorphous wire was placed in an etching solution containing 40% hydrofluoric acid, 0.2% sodium thiocyanate and 0.8% hexamethylenetetramine for 120 seconds to remove the glass layer on the surface. The amorphous wire was then taken out of the etching solution, ultrasonically cleaned in a beaker containing anhydrous ethanol for 5 times, and dried to obtain Co 68.15 Fe 4.35 Si 11.4 8B 14.02 The Cu1Nb1 cast amorphous wire is placed in a vacuum drying oven for future use;

[0068] The Co 68.15 Fe 4.35 Si 11.48 B 14.02 Take 10 cm length of Cu1Nb1 cast amorphous wire and perform current annealing heat treatment: clamp the two ends of the wire with current clamps, connect the wire between the constant current source and the current clamp, set the current output parameter to 30 mA, the power-on time to 2.5 min, and reduce the ambient vacuum to 10 Pa.

[0069] Comparative Example 1

[0070] According to the preparation steps of Example 1, Co 68.15 Fe 4.35 Si 11.48 B 14.02 Cu1Nb1 as-cast amorphous wire.

[0071] Example 2

[0072] In 10 -3 Pa and under the condition of argon protection, metal raw materials Co, Fe, Si, B, Cu and V with purity greater than 99.9wt.% are melted to obtain a composition of Co 68 Fe 4.5 Si 11.48 B 14.02 The cobalt-based amorphous alloy of Cu1V1 is then cut into small cylindrical blocks of 1 to 2 mm;

[0073] The cut cobalt-based amorphous alloy small cylindrical blocks are prepared into glass-coated amorphous wires by using a glass coating method, and the glass coating method is shown in Example 1 of the patent publication number CN114015957B;

[0074] The glass-coated amorphous wire was placed in an etching solution containing 40% hydrofluoric acid, 0.2% sodium thiocyanate and 0.8% hexamethylenetetramine for 120 seconds to remove the glass layer on the surface. The amorphous wire was then taken out of the etching solution, ultrasonically cleaned in a beaker containing anhydrous ethanol for 5 times, and dried to obtain Co 68 Fe 4.5 Si 11.48 B 14.02 The Cu1V1 cast amorphous wire is placed in a vacuum drying oven for future use;

[0075] The Co 68 Fe 4.5 Si 11.48 B 14.02 Take 10 cm length of Cu1V1 cast amorphous wire and perform current annealing heat treatment: clamp the two ends of the wire with current clamps, connect the wire between the constant current source and the current clamp, set the current output parameter to 30 mA, the power-on time to 2.5 min, and reduce the ambient vacuum to 10 Pa.

[0076] Comparative Example 2

[0077] According to the preparation steps of Example 2, Co 68 Fe 4.5 Si 11.48 B 14.02 Cu1V1 cast amorphous wire.

[0078] Example 3

[0079] In 10 -3 Pa and under the condition of argon protection, metal raw materials Co, Fe, Si, B, Cu, V and Nb with purity greater than 99.9wt.% are melted to obtain Co 68 Fe 4.5 Si 11.48 B 14.02 VxV 0.5 Nb 0.5 The cobalt-based amorphous alloy is then cut into small cylindrical blocks of 1 to 2 mm;

[0080] The cut cobalt-based amorphous alloy small cylindrical blocks are prepared into glass-coated amorphous wires by using a glass coating method, and the glass coating method is shown in Example 1 of the patent publication number CN114015957B;

[0081] The glass-coated amorphous wire was placed in an etching solution containing 40% hydrofluoric acid, 0.2% sodium thiocyanate and 0.8% hexamethylenetetramine for 120 seconds to remove the glass layer on the surface. The amorphous wire was then taken out of the etching solution, ultrasonically cleaned in a beaker containing anhydrous ethanol for 5 times, and dried to obtain Co 68 Fe 4.5 Si 11.48 B 14.0 2Cu1V 0.5 Nb 0.5 The cast amorphous wire is placed in a vacuum drying oven for future use;

[0082] The Co 68 Fe 4.5 Si 11.48 B 14.02 VxV 0.5 Nb 0.5 The cast amorphous wire was taken in a length of 10 cm and subjected to current annealing heat treatment. The specific operation method was to clamp the two ends of the wire with a current clamp, connect the wire between the constant current source and the current clamp, set the current output parameter to 30 mA, the power-on time to 2.5 min, and reduce the environmental vacuum to 10 Pa.

[0083] Comparative Example 3

[0084] According to the preparation steps of Example 3, Co 68 Fe 4.5 Si 11.48 B 14.02 VxV 0.5 Nb 0.5 As-cast amorphous wire.

[0085] Comparative Example 4

[0086] In 10 -3 Pa and under the condition of argon protection, metal raw materials Co, Fe, Si and B with purity greater than 99.9wt.% are smelted to obtain a composition of Co 68.65 Fe 4.85 Si 11.98 B 14.52 The cobalt-based amorphous alloy is then cut into small cylindrical blocks of 1 to 2 mm;

[0087] The cut cobalt-based amorphous alloy small cylindrical blocks are prepared into glass-coated amorphous wires by using a glass coating method, and the glass coating method is shown in Example 1 of the patent publication number CN114015957B;

[0088] The glass-coated amorphous wire was placed in an etching solution containing 40% hydrofluoric acid, 0.2% sodium thiocyanate and 0.8% hexamethylenetetramine for 120 seconds to remove the glass layer on the surface. The amorphous wire was then taken out of the etching solution, ultrasonically cleaned in a beaker containing anhydrous ethanol for 5 times, and dried to obtain Co 68.65 Fe 4.85 Si 11.98 B 14.52 The cast amorphous wire is placed in a vacuum drying oven for future use;

[0089] The Co 68.65 Fe 4.85 Si 11.98 B 14.52 Take 10 cm length of the cast amorphous wire and perform current annealing heat treatment: clamp the two ends of the wire with current clamps, connect the wire between the constant current source and the current clamp, set the current output parameter to 30 mA, the power-on time to 2.5 min, and reduce the environmental vacuum to 10 Pa.

[0090] Structural and performance standards

[0091] The amorphous wires of Examples 1 to 3 and Comparative Examples 1 to 4 were subjected to structural characterization, thermodynamic characterization, static magnetic property test and impedance change rate test.

[0092] Figure 1 This is a SEM photograph of the diameter of the cast amorphous wire after removing the glass coating in Comparative Example 1. The surface of the amorphous wire is smooth and neat, and the diameter is 30 to 40 μm.

[0093] Crystalline phase characterization

[0094] The amorphous wires obtained in Example 1 and Comparative Example 1 were analyzed by X-ray diffraction. Figure 3 The XRD results of the two are diffuse broad diffraction peaks (As-prepared represents the amorphous wire that has not been heat treated, that is, the cast amorphous wire; DC-annealing represents the amorphous wire after current annealing), indicating that the amorphous wire obtained in Example 1 and the cast amorphous wire obtained in Comparative Example 1 are both amorphous phases.

[0095] The amorphous wires in Example 2 and Comparative Example 2 were analyzed by X-ray diffraction. The XRD results were consistent with Figure 3 Similarly, it is a diffuse broad diffraction peak, indicating that the amorphous wire obtained in Example 2 and the cast amorphous wire obtained in Comparative Example 2 are both in the amorphous phase.

[0096] The amorphous wires in Example 3 and Comparative Example 3 were analyzed by X-ray diffraction. The XRD results were consistent with Figure 3Similarly, it is a diffuse broad diffraction peak, indicating that the amorphous wire obtained in Example 3 and the cast amorphous wire obtained in Comparative Example 3 are both in the amorphous phase.

[0097] Thermodynamic characterization

[0098] In order to compare the changes in thermodynamic parameters and relaxation enthalpy of the as-cast and annealed amorphous wires, differential scanning calorimetry (DSC) was used to perform thermodynamic characterization on Examples 1 to 3 and Comparative Examples 1 to 3.

[0099] The differential scanning calorimetry (DSC) test steps are as follows: weigh 12 mg of amorphous wire, put it into a crucible, compact it, and put it into the DSC equipment for testing. In an argon atmosphere, perform temperature scanning at a heating rate of 20 K / min and a cooling rate of 50 K / min to test its heat change.

[0100] DSC curves and relaxation enthalpy data can be found at Figure 4 , indicating that the amorphous wire material of Example 1 after annealing is still amorphous, because the glass transition point Tg and crystallization temperature Tx of the material have not changed compared with the cast state, and the size and location of the exothermic peak have not changed significantly. The conclusion of thermodynamic characterization that it is amorphous is also consistent with the conclusion of XRD experiment. Moreover, by comparing the relaxation enthalpy of the two, it is found that the relaxation enthalpy of the amorphous wire material after annealing is significantly reduced, indicating that it absorbs Joule heat during the annealing process, undergoes structural relaxation, and rises to a high energy state, thereby causing its enthalpy change value to decrease.

[0101] Differential scanning calorimetry (DSC) was used to characterize the thermodynamics of Example 2 and Comparative Example 2. Figure 4 Similarly, it shows that the amorphous wire material of Example 2 after annealing is still amorphous, because the glass transition point Tg and crystallization temperature Tx of the material have not changed compared with the cast state, and the size and location of the exothermic peak have not changed significantly. The conclusion that the thermodynamic characterization is amorphous is also consistent with the conclusion of the XRD experiment. Moreover, by comparing the relaxation enthalpy of the two, it is found that the relaxation enthalpy of the amorphous wire material after annealing is significantly reduced, indicating that it absorbs Joule heat during the annealing process, undergoes structural relaxation, and rises to a high energy state, thereby causing its enthalpy change value to decrease.

[0102] Differential scanning calorimetry (DSC) was used to characterize the thermodynamics of Example 3 and Comparative Example 3. Figure 4Similarly, it is shown that the amorphous wire material of Example 3 after annealing is still amorphous, because the glass transition point Tg and crystallization temperature Tx of the material have not changed compared with the cast state, and the size and location of the exothermic peak have not changed significantly. The conclusion that the thermodynamic characterization is amorphous is also consistent with the conclusion of the XRD experiment. Moreover, by comparing the relaxation enthalpy of the two, it is found that the relaxation enthalpy of the amorphous wire material after annealing is significantly reduced, indicating that it absorbs Joule heat during the annealing process, undergoes structural relaxation, and rises to a high energy state, thereby causing its enthalpy change value to decrease.

[0103] Soft magnetic properties test

[0104] The amorphous wire in the present invention is a high-performance soft magnetic material. In order to measure the specific values ​​of the soft magnetic performance parameters and compare and analyze the changes in the soft magnetic properties of the amorphous wire after current annealing, soft magnetic properties tests were performed on Examples 1 to 3 and Comparative Examples 1 to 3:

[0105] 1. Use the E4094A impedance analyzer produced by Keysight to measure the magnetic permeability of the wire. The frequency test range is set to 500-1500Hz. The test vehicle is a small excitation copper coil with a diameter of 3mm. Take 20 wires of 10cm long and put them into the coil for magnetic permeability test.

[0106] The magnetic permeability test results of Example 1 and Comparative Example 1 are shown in Figure 5 The effective magnetic permeability μe of the amorphous wire in Example 1 after annealing is generally significantly higher than that in the cast state in Comparative Example 1, indicating that the current annealing method in the present invention is very helpful in improving the magnetic permeability. Taking the frequency of 1 kHz as an example, the effective magnetic permeability μe of the cast wire is 9500, while after annealing, μe can reach 14000, an increase of 47%.

[0107] The magnetic permeability test results of Example 2 and Comparative Example 2 are Figure 5 Similarly, the effective magnetic permeability μe of the amorphous wire after annealing in Example 2 is generally significantly higher than that of the cast wire in Comparative Example 2, indicating that the current annealing method in the present invention is very helpful in improving the magnetic permeability. Taking the frequency of 1 kHz as an example, the effective magnetic permeability μe of the cast wire is 8900, while after annealing, μe can reach 15000, an increase of 68%.

[0108] The magnetic permeability test results of Example 3 and Comparative Example 3 are Figure 5 Similarly, the effective magnetic permeability μe of the amorphous wire after annealing in Example 3 is generally significantly higher than that of the cast wire in Comparative Example 2, indicating that the current annealing method in the present invention is very helpful in improving the magnetic permeability. Taking the frequency of 1 kHz as an example, the effective magnetic permeability μe of the cast wire is 9300, while after annealing, μe can reach 15800, an increase of 69%.

[0109] Comparative Example 4 adopts the same current annealing process as Example 1, and after annealing, μe reaches 12100 at 1kHz, which is 33% higher than the as-cast μe value of 9100. This shows that the cobalt-based amorphous wire provided by the present invention has the characteristic of high magnetic permeability.

[0110] 2. The static magnetic properties of the wire were measured using a Lake Shore 7404 vibrating sample magnetometer (VSM). The magnetic field test range of the instrument was set to ±10,000 Oe. The wire was fixed on a 4 mm2 silicon wafer and the wire was neatly arranged in the horizontal direction. The VSM test was performed at room temperature.

[0111] The VSM test results of Example 1 and Comparative Example 1 are as follows: Figure 6 As shown, the cobalt-based amorphous wire of Example 1 after current annealing has the characteristics of high saturation magnetic flux density Bs and low coercive force Hc, and is a typical soft magnetic material from the line shape of the hysteresis loop. Obviously, current annealing greatly improves the saturation magnetic flux density of the amorphous wire. Bs is 0.55T in the cast state, and Bs reaches 0.72T after annealing. At the same time, the coercive force Hc is kept in a relatively small value range, almost close to 0 (<0.5A / m).

[0112] The test results of Example 2 and Comparative Example 2 are Figure 6 Similarly, the cobalt-based amorphous wire material of Example 2 after current annealing has the characteristics of high saturation magnetic flux density Bs and low coercive force Hc, and is a typical soft magnetic material from the line shape of the hysteresis loop. Obviously, current annealing greatly improves the saturation magnetic flux density of the amorphous wire material, Bs is 0.50T in the cast state, and Bs reaches 0.73T after annealing, while the coercive force Hc is kept in a relatively small value range, almost close to 0 (<0.5A / m).

[0113] The test results of Example 3 and Comparative Example 3 are Figure 6 Similarly, the cobalt-based amorphous wire material of Example 3 after current annealing has the characteristics of high saturation magnetic flux density Bs and low coercive force Hc, and is a typical soft magnetic material from the line shape of the hysteresis loop. Obviously, current annealing greatly improves the saturation magnetic flux density of the amorphous wire material, Bs is 0.52T in the cast state, and Bs reaches 0.76T after annealing, while the coercive force Hc is kept in a relatively small value range, almost close to 0 (<0.5A / m).

[0114] Comparative Example 4 adopts the same current annealing process as Example 1, and the Bs in the cast state is 0.49T, and after annealing, the Bs reaches 0.65T, and the coercive force is 0.5A / m. It shows that the cobalt-based amorphous wire provided by the present invention has the characteristics of high saturation magnetic induction intensity Bs and low coercive force Hc.

[0115] 3. The impedance change rate of the wire was tested using an impedance analyzer produced by Keysight and a Helmholtz coil. The magnetic field range provided by the Helmholtz coil was 0 to 100 Oe. Both ends of the wire were welded and fixed on a circuit board. The circuit board was placed in the center area of ​​the coil and connected to a test circuit. Examples 1 to 3 and Comparative Examples 1 to 3 were tested for the GMI effect.

[0116] The GMI curves of Example 1 and Comparative Example 1 are as follows: Figure 7 As shown in the figure, the maximum GMI of both wires corresponds to a 5Oe magnetic field, and when the field strength reaches 100Oe, the GMI change rate tends to 0. The maximum GMI% of the annealed amorphous wire is 405%, while that of the cast wire under the same conditions is only 70%. Obviously, this is also a good effect achieved through structural relaxation.

[0117] The GMI curves of Example 2 and Comparative Example 2 are Figure 7 Similarly, the maximum GMI of both corresponds to a 5Oe magnetic field, and when the field strength reaches 100Oe, the GMI change rate tends to 0. The maximum GMI% of the annealed amorphous wire is 420%, while that of the cast wire under the same conditions is only 68%. Obviously, this is also a good effect achieved through structural relaxation.

[0118] The GMI curves of Example 3 and Comparative Example 3 are Figure 7 Similarly, the maximum GMI of both corresponds to a 5Oe magnetic field, and when the field strength reaches 100Oe, the GMI change rate tends to 0. The maximum GMI% of the amorphous wire after annealing is 445%, while that of the cast wire under the same conditions is only 69%. Obviously, this is also a good effect achieved through structural relaxation. Therefore, whether from the perspective of the prepared state properties of the material or the annealing effect, the present invention is indeed an effective method.

[0119] Comparative Example 4 adopts the same current annealing process as Example 1, and the as-cast GMI is only 65%, and the maximum GMI after current annealing is 320%. It shows that the cobalt-based amorphous wire provided by the present invention has the characteristics of high GMI change rate and high sensitivity.

[0120] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for obtaining amorphous wire with high soft magnetic properties, characterized in that: The following steps are involved: Under a first vacuum environment, applying a direct current to the as-cast amorphous wire to obtain an amorphous wire with high soft magnetic properties; The magnitude of the direct current is 30-130 mA, and the power-on time is 2.5 min; The composition of the cast amorphous wire is Co 68.15 Fe 4.35 Si 11.48 B 14.02 Cu1Nb1, Co 68 Fe 4.5 Si 11.48 B 14.02 Cu1V1 or Co 68 Fe 4.5 Si 11.48 B 14.02 VxV 0.5 Nb 0.5 ; The high soft magnetic property amorphous wire has an effective magnetic permeability μe of 13000-16000 at 1kHz, a saturation magnetic induction intensity Bs of 0.70-0.80T, a coercive force Hc<0.5A / m, and a giant magneto-impedance effect GMI% of 400-450%.

2. The method according to claim 1, characterized in that The vacuum degree of the first vacuum environment is 0-10Pa.

3. The method according to claim 1, characterized in that The as-cast amorphous wire is a wire with a circular cross-section.

4. The method according to claim 3, characterized in that The diameter of the metal core of the cast amorphous wire is 20-60 μm.

5. The method according to claim 1, characterized in that The direct current is a unidirectional constant current.

6. The method according to claim 1 or 4, characterized in that: The method for preparing the cast amorphous wire comprises the following steps: Under the conditions of a second vacuum and argon protection, metal raw materials Co, Fe, Si, B and M are melted corresponding to the composition of the cast amorphous wire to obtain a cobalt-based amorphous alloy; The M is Cu and Nb or Cu and V or Cu, V and Nb; The cobalt-based amorphous alloy is made into glass-coated amorphous wire by a glass-coating method; The glass-coated amorphous wire is placed in a corrosive solution to remove the surface glass layer to obtain the cast amorphous wire material.

7. The method according to claim 6, characterized in that The vacuum degree of the second vacuum is ≤10 -3 Pa.

8. The high soft magnetic property amorphous wire obtained by the method according to any one of claims 1 to 7, characterized in that: The high soft magnetic property amorphous wire has an effective magnetic permeability μe of 13000-16000 at 1kHz, a saturation magnetic induction intensity Bs of 0.70-0.80T, a coercive force Hc<0.5A / m, and a giant magneto-impedance effect GMI% of 400-450%.

9. Application of the amorphous wire with high soft magnetic properties as claimed in claim 8 in precision electronic devices or high-sensitivity weak magnetic sensors.