A photovoltaic module containing TOPCon cells and a preparation method thereof
By introducing support and panel mechanisms into photovoltaic modules to achieve pitch angle adjustment, and increasing the thickness of the N+-Poly layer in the grid area on the back of the TOPCon cell, the problems of fixed angle and low light absorption efficiency after photovoltaic module installation are solved, thus improving photoelectric conversion efficiency.
Patent Information
- Application Number
- CN202410090464.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-23
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-01-23
AI Technical Summary
The tilt angle of photovoltaic modules is fixed after installation and cannot be adjusted according to the actual use scenario. In addition, the Poly Si structure on the back of the TOPCon cell affects the light absorption efficiency, resulting in a loss of conversion efficiency.
A photovoltaic module containing TOPCon cells was designed, employing a support mechanism and a panel mechanism to allow for pitch angle adjustment. The thickness of the N+-Poly layer is increased in the grid area on the back of the cell to improve passivation and contact performance. At the same time, the photoelectric conversion efficiency is improved by locally thinning the N+-Poly layer thickness in the non-grid area.
This technology enables photovoltaic modules to adjust their pitch angle according to the actual scene after installation, and improves photoelectric conversion efficiency by locally thinning the Poly layer in the non-grid area, thereby reducing the overall cost of the modules.
Smart Images

Figure CN117913164B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of photovoltaic modules, and in particular to a photovoltaic module containing a TOPCon cell and a preparation method thereof. Background Art
[0002] The manufacturing of photovoltaic modules is to first connect the cells in series to obtain high voltage, then connect them in parallel to obtain high current, and then encapsulate them in the frame to form photovoltaic modules. A photovoltaic module is composed of dozens of cells. The conversion efficiency of the cells directly affects the power generation efficiency of the photovoltaic module, and the production process of the cells directly affects the service life of the photovoltaic module.
[0003] Solar cells, also known as photovoltaic cells or photovoltaic cells or cells, are devices that use the photovoltaic effect to convert light energy into electrical energy. The two development directions of crystalline silicon solar cells are to reduce costs and improve efficiency. The photovoltaic industry is highly competitive, and it is very difficult to continue to reduce costs, but there is still a lot of room for improving efficiency. Recombination loss is a key factor affecting cell efficiency. For the traditional cell structure of aluminum back surface field (Al-BSF) and the mainstream PERC cell, the metal / semiconductor interface defect density on the back of the cell is high, and interface recombination is an important cause of efficiency loss. In order to reduce interface recombination losses, the contact area needs to be further reduced. However, there is a lower limit for the proportion of contact area to the total cell area, otherwise the contact resistance will be too large, resulting in a decrease in the fill factor (FF) and a decrease in the cell conversion efficiency. Another way is to use the selective passage characteristics of paired carriers (effectively improving the transport of one carrier while hindering the passage of another carrier), which can greatly reduce the recombination of the metal / semiconductor interface.
[0004] This passivation contact is superior to other traditional battery structures in two aspects: (1) The recombination of the metal / semiconductor interface is reduced by the passivation layer between the crystalline silicon and the metal contact; (2) The majority carriers can move to the metal contact by the tunneling effect, but the minority carriers cannot move from the crystalline silicon to the metal contact due to carrier selectivity. This passivation contact can use intrinsic amorphous silicon or ultra-thin silicon oxide as the passivation layer. The passivation contact based on amorphous silicon is the heterojunction battery structure or HJT; the superposition structure of the passivation contact based on SiO2 and polycrystalline silicon is TOPCon technology.
[0005] For example, Chinese patent CN116864548A discloses a p-type back-junction TOPCon cell and a preparation method thereof. In this technical solution, p-type crystalline silicon is used as a substrate, and a local p-type doped layer, a doped passivation layer, a front anti-reflection layer, and a front metal electrode are sequentially arranged on the front side; a tunneling oxide layer, an n-type doped polysilicon layer, a back anti-reflection layer, and a back metal electrode are sequentially arranged on the back side; the front metal electrode penetrates the front anti-reflection layer and the doped passivation layer to form an ohmic contact with the local p-type doped layer; the local p-type doped layer is an Al and B co-doped layer; the front metal electrode is an Ag paste electrode formed by printing and sintering, and the Ag paste does not contain Al powder.
[0006] When installing photovoltaic modules, the angle of the photovoltaic panels needs to be adjusted according to the actual scene. At present, after the photovoltaic modules are installed, their pitch angle is basically fixed, which makes it inconvenient to adjust the pitch angle of the photovoltaic panels according to the actual use scene.
[0007] Moreover, the complete back Poly Si of TOPCon cells in current photovoltaic modules can block the passage of minority carriers and allow the majority carriers to pass through, forming an extremely high carrier concentration barrier and enhancing the passivation and contact effects. However, the presence of Poly Si in the back non-grid area affects the absorption of light in the long-wave band, resulting in a loss of photoelectric conversion efficiency, so the complete back Poly structure has obvious defects. Summary of the invention
[0008] In order to solve the above problems, the object of the present invention is to provide a photovoltaic module containing TOPCon cells and a preparation method thereof.
[0009] The technical solution provided by the present invention is:
[0010] In a first aspect, a photovoltaic module containing a TOPCon cell comprises a support mechanism and a panel mechanism;
[0011] The support mechanism comprises a base, on which an elevation adjustment mechanism is provided, and the elevation adjustment mechanism is used to adjust the elevation angle of the panel fixing mechanism; the panel fixing mechanism is used to fix the panel mechanism;
[0012] The panel mechanism includes a frame, which is used to fix the upper cover plate and the lower cover plate; packaging material is provided between the upper cover plate and the lower cover plate;
[0013] A plurality of TOPCon batteries are encapsulated in the encapsulation material, and the plurality of TOPCon batteries are connected in series through electrical connectors and connected to a junction box;
[0014] The back electrode of the TOPCon cell corresponds to the N gate line area + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness.
[0015] The number of TOPCon batteries is 54 to 78;
[0016] The weight power density of the photovoltaic module is greater than or equal to 17 W / kg and less than or equal to 18.5 W / kg.
[0017] In a second aspect, a method for preparing a photovoltaic module containing a TOPCon cell comprises the following steps:
[0018] Cell sorting: Match and combine TOPCon cells with consistent performance;
[0019] Welding: Use electrical connectors to connect multiple cells in series;
[0020] Lamination: stack EVA, battery string, EVA, and back sheet on the panel from bottom to bottom to form a laminate;
[0021] Lamination: Heat and pressurize the stacked parts to combine them into an integral laminated assembly;
[0022] EL test: detect whether the laminated components have hidden defects;
[0023] Framing: Place laminated components without hidden defects into frames filled with packaging materials, and then install the cover plate;
[0024] Install the junction box: Install the junction box on one side of the lower cover, and connect the electrical connectors from the battery cells to the junction box;
[0025] Cleaning: remove dirt from the surface of photovoltaic modules;
[0026] Photovoltaic performance test: Test the photovoltaic output power of photovoltaic modules and select qualified photovoltaic modules for finished product inspection.
[0027] The panel structure and the supporting structure that have passed the inspection are installed to produce a photovoltaic module containing TOPCon cells.
[0028] In a third aspect, a TOPCon cell comprises an N-type silicon wafer layer, wherein a boron diffusion layer, a passivation layer, a front anti-reflection layer and a front electrode are stacked on the front side of the N-type silicon wafer layer, and at least two groups of oxide layers and an N-type silicon wafer layer are stacked on the back side. + -Poly layer, back anti-reflection layer, back electrode;
[0029] The N of the gate line area corresponding to the back electrode + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness, and the thickness of the protruding part is N + -0.5-5 times the thickness of the Poly layer, and the outer N layer in the non-gate line area +-Poly layer thickness is 10-20nm.
[0030] In a fourth aspect, a method for processing the outer layer Poly of a TOPCon battery comprises:
[0031] A protective layer is formed in the gate line area of the silicon wafer, and the protective layer is used to protect the outer N layer corresponding to the gate line area. + -Poly layer is protected from removal;
[0032] Then remove the outer N layer without protection layer in the non-gate line area + -Poly layer, so that the N + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness, and the thickness of the protruding part is N + -H times the thickness of the Poly layer, H ≥ 0.5.
[0033] As an optional technical solution of the fourth aspect, the value range of H is 0.5-5.
[0034] As an optional technical solution of the fourth aspect, the outer layer N + -Poly layer is partially removed, and the outer N layer of non-gate line area + -The remaining thickness of the Poly layer is K, K≥10nm.
[0035] Furthermore, the value range of K is 10-20 nm.
[0036] As an optional technical solution of the fourth aspect, the outer N layer without protection layer in the non-grid line area is removed by alkaline solution. + -Poly layer.
[0037] As an optional technical solution of the fourth aspect, the protective layer is a mask layer that does not react with alkaline solution and can be removed by acid solution.
[0038] Furthermore, when making the mask layer, firstly, a layer of Si-containing slurry is coated on the gate line area on the back side of the silicon wafer, and then dried at high temperature to form a SiO2 mask layer in the gate line area of the silicon wafer.
[0039] Optionally, the Si-containing slurry is applied to a thickness of 100-1000 nm.
[0040] Furthermore, a hollow pattern corresponding to the position of the screen-printed back gate line pattern is made on the mask plate, and after being prepared with Si-containing slurry, the slurry is roller-coated onto the mask plate so that the slurry adheres to the back gate line area of the silicon wafer through the hollow pattern, and then dried in a chain heating furnace at a set temperature of 300-700°C.
[0041] In a fifth aspect, a method for preparing a TOPCon battery, comprising the method for treating the outer layer of a TOPCon battery in the fourth aspect or any one of the optional technical solutions of the fourth aspect;
[0042] Before forming the mask layer in the gate line area on the back side of the silicon wafer, the following steps are also included:
[0043] Choose silicon wafer as substrate and make double-sided texture;
[0044] Diffusion of boron is performed on the front side of the silicon wafer to form a boron diffusion layer;
[0045] Remove the BSG layer on the back and sides of the silicon wafer and perform alkaline polishing on the back of the silicon wafer;
[0046] Depositing at least two sets of oxide layers and polysilicon layers on the back side of the silicon wafer;
[0047] Phosphorus doping is performed on the back of the silicon wafer to form N + -Poly layer, and forming a PSG layer on the outer layer;
[0048] Remove the PSG layer on the front and side of the silicon wafer;
[0049] Remove the outer N layer on the back of the silicon wafer without mask protection + -After the Poly layer, the following steps are also included:
[0050] Remove the excess Poly layer on the front and side of the silicon wafer; then remove the PSG, back mask layer and PSG layer in the non-mask area on the back;
[0051] A passivation layer, a front anti-reflection layer, and a back anti-reflection layer are formed on the silicon wafer;
[0052] The front and back sides of the silicon wafer are screen printed and sintered to form front electrodes and back electrodes, and the position of the back electrode corresponds to the position of the patterned mask.
[0053] As an optional technical solution of the fifth aspect, the silicon wafer is an N-type single crystal silicon wafer with a thickness of 100-160 microns and a resistivity of 0.4-10Ω·cm.
[0054] As an optional technical solution of the fifth aspect, a low-pressure and high-temperature diffusion furnace is used to diffuse boron on the front side of the silicon wafer, with a diffusion temperature of 800-1100° C. and a diffusion time of 10-50 minutes.
[0055] Furthermore, after diffusion, the sheet resistance of the boron diffusion layer is 100-260Ω / sq, the junction depth is 0.1-0.4 micrometers, and the thickness of the BSG layer is 100-160 nanometers.
[0056] As an optional technical solution of the fifth aspect, at least two groups of oxide layers and polysilicon layers are deposited on the back side of an N-type single crystal silicon wafer using LPCVD equipment.
[0057] Furthermore, there are two groups of oxide layers and polysilicon layers, including a first SiO2 layer, a first Poly layer, a second SiO2 layer, and a second Poly layer which are sequentially stacked from the inner layer to the outer layer.
[0058] Furthermore, the thickness of the first SiO2 layer is 1-2 nm, the thickness of the first Poly layer is 20-40 nm, the thickness of the second SiO2 layer is 0.5-2 nm, and the thickness of the second Poly layer is 30-150 nm.
[0059] As an optional technical solution of the fifth aspect, the phosphorus doping concentration range is 0.1-2E 21 .
[0060] As an optional technical solution of the fifth aspect, HF is used to remove the PSG layer on the front and side surfaces of the silicon wafer;
[0061] Use alkaline solution to remove the excess Poly layer on the front and sides of the silicon wafer, and the outer N layer on the back without mask layer protection + -Poly layer; use acid to remove the PSG in the non-mask area on the back, the back mask layer and the PSG layer here.
[0062] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:
[0063] After the photovoltaic assembly of the present invention is installed, when it is necessary to adjust the pitch angle of the panel, the height of the vertical sliding support can be adjusted first, and then the positions of the first slide and the second slide can be adjusted, and finally the first slide and the second slide of the vertical sliding support can be fixed. Therefore, after the photovoltaic assembly is installed, the pitch angle of the panel fixing mechanism can also be adjusted according to the actual usage scenario.
[0064] At the same time, the present invention forms N + -Poly, and after the PSG layer is formed on the outer layer, a layer of Si-containing slurry is applied to the gate contact area on the back of the silicon wafer, and then dried at high temperature, so that a SiO2 mask layer can be formed in the gate contact area on the back of the silicon wafer. Using Si-containing slurry, on the one hand, Si will not bring the risk of reducing battery performance, and secondly, the formed SiO2 mask layer is difficult to react with alkali at room temperature. Therefore, alkali is used to remove the excess Poly layer on the front and side of the silicon wafer, and the outer N layer on the back without mask layer protection. + -Poly layer, this mask layer can protect the N gate line area of the mask layer. + -Poly layer forms protection, so that only the outer N layer of the non-gate line area is thinned +After removing the PSG in the non-mask area of the back side with acid, the back mask layer and the PSG layer here, the passivation layer, anti-reflection layer and electrode can be produced, thereby obtaining the N-type layer in the gate line area corresponding to the back electrode. + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness TOPCon cells, thereby improving the shortcomings of current TOPCon cells and further improving the photoelectric conversion efficiency of photovoltaic modules. BRIEF DESCRIPTION OF THE DRAWINGS
[0065] Figure 1 This is a schematic diagram of the supporting structure of a photovoltaic module in one embodiment of the present application;
[0066] Figure 2 This is a schematic diagram of the connection between a column and a vertical sliding support in one embodiment of the present application;
[0067] Figure 3 for Figure 1 Enlarged view of point A in the middle;
[0068] Figure 4 This is a schematic diagram of the connection between the first slide seat and the slide table in one embodiment of the present application;
[0069] Figure 5 This is an exploded schematic diagram of a panel structure of a photovoltaic module in one embodiment of the present application;
[0070] Figure 6 This is a schematic diagram of the panel structure of a photovoltaic module in one embodiment of the present application;
[0071] Figure 7 In one embodiment of the present application, the second N + -Schematic diagram of the structure when the Poly layer is partially removed;
[0072] Figure 8 In one embodiment of the present application, the second N + -Schematic diagram of the structure when the Poly layer is completely removed.
[0073] Explanation of the symbols in the schematic diagram:
[0074] TOPCon cell 100, N-type silicon wafer layer 101, boron diffusion layer 102, passivation layer 103, front anti-reflection layer 104, front electrode 105, first SiO2 layer 106, first N + -Poly layer 107, second SiO2 layer 108, second N + -Poly layer 109, back anti-reflection layer 110, back electrode 111;
[0075] Upper cover plate 201, frame 202, lower cover plate 203, electrical connector 204, junction box 205, packaging material 206;
[0076] Base 301, column 302, vertical sliding support 303, first through hole 304, second bolt 305, supporting base 306, lower protrusion 307, pressure block 308, first bolt 309, upper protrusion 310, first vertical slide groove 311, slide table 312, third through hole 313, first slide seat 314, second slide seat 315, second support rod 316, first support rod 317, third bolt 318, horizontal slide groove 319. DETAILED DESCRIPTION
[0077] In order to further understand the content of the present invention, the present invention is described in detail in conjunction with the accompanying drawings and embodiments.
[0078] The structures, proportions, sizes, etc. illustrated in the drawings of this specification are only used to match the contents disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the limiting conditions for the implementation of the present invention, so they have no substantial technical significance. Any modification of the structure, change of the proportion relationship or adjustment of the size, without affecting the effects and purposes that can be achieved by the present invention, should still fall within the scope of the technical content disclosed by the present invention. At the same time, the terms such as "upper", "lower", "left", "right", "middle" and so on quoted in this specification are only for the convenience of description, and are not used to limit the scope of implementation. The change or adjustment of their relative relationship should also be regarded as the scope of implementation of the present invention without substantially changing the technical content.
[0079] Embodiment 1
[0080] The present application proposes a photovoltaic module containing TOPCon cells, including a supporting mechanism and a panel mechanism.
[0081] like Figure 1-4 As shown, the support mechanism includes a base 301, and an elevation adjustment mechanism is provided on the base 301, through which the elevation adjustment mechanism can be used to adjust the elevation angle of the panel fixing mechanism. When a panel mechanism is mounted on the panel fixing mechanism, the elevation angle of the panel mechanism can be adjusted together by adjusting the elevation angle of the panel fixing mechanism, so that the panel mechanism has a better light receiving angle.
[0082] In this embodiment, the panel fixing mechanism includes a support frame 306, a plurality of first vertical slide grooves 311 are provided on the support frame 306, a pressing block 308 is installed in the first vertical slide groove 311, an upper convex edge 310 is installed on the support frame 306 located on the upper side of the pressing block 308, and a lower convex edge 307 is installed on the support frame 306 located on the lower side of the pressing block 308. A threaded hole is provided on the upper convex edge 310, and a first bolt 309 is installed in the threaded hole.
[0083] The edge of the panel mechanism is placed on the lower convex edge 307, and then the first bolt 309 is tightened. The first bolt 309 pushes the pressing block 308, so that the pressing block 308 is tightly pressed against the panel mechanism, thereby fixing the panel mechanism.
[0084] In this embodiment, the elevation adjustment mechanism includes a column 302 vertically mounted on a base 301, the column 302 is provided with a second vertical slide groove, a vertical sliding support 303 is installed in the second vertical slide groove, and the upper end of the vertical sliding support 303 is hinged to the lower end of the supporting base 306. A plurality of first through holes 304 are evenly distributed on the vertical sliding support 303, and a second through hole is provided on the column 302. After the vertical sliding support 303 is adjusted to a suitable height, the second bolt 305 is passed through the second through hole and the first through hole 304, and then tightened with a nut, so that the vertical sliding support 303 can be fixed so that its height remains unchanged.
[0085] In this embodiment, the elevation adjustment mechanism further includes a slide 312 mounted on the base 301, and a transverse slide groove 319 is provided on the slide 312, and a first slide 314 and a second slide 315 are installed in the transverse slide groove 319. The first slide 314 is hinged with a first support rod 317, one end of the first support rod 317 is hinged with the first slide 314, and the other end is hinged with the support base 306. The second slide 315 is hinged with a second support rod 316, one end of the second support rod 316 is hinged with the second slide 315, and the other end is hinged with the first support rod 317.
[0086] The slide 312 is provided with a plurality of third through holes 313, and the first slide 314 and the second slide 315 are provided with fourth through holes. When the first slide 314 and the second slide 315 are adjusted to a suitable position, the third bolt 318 can be passed through the third through hole 313 and the fourth through hole, and then the nut is tightened, so that the first slide 314 and the second slide 315 can be fixed.
[0087] First, the height of the vertical sliding support 303 is adjusted, and then the positions of the first slide 314 and the second slide 315 are adjusted. Finally, the vertical sliding support 303, the first slide 314 and the second slide 315 are fixed, and the pitch angle of the panel fixing mechanism can be adjusted.
[0088] like Figure 5-6 As shown, the panel mechanism includes a frame 202, and the frame 202 is used to fix the upper cover plate 201 and the lower cover plate 203; a packaging material 206 is provided between the upper cover plate 201 and the lower cover plate 203.
[0089] A plurality of TOPCon batteries 100 are encapsulated in the encapsulation material. The plurality of TOPCon batteries 100 are connected in series through electrical connectors 204 and connected to a junction box 205 .
[0090] The N of the gate line area corresponding to the back electrode of the TOPCon battery 100 + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness. The number of TOPCon cells 100 is 54 to 78, such as 72.
[0091] The weight power density of photovoltaic modules is greater than or equal to 17 W / kg and less than or equal to 18.5 W / kg. If the photovoltaic module is too heavy, the lightness of the supporting material will be high, and the transportation cost will increase, thereby increasing the overall installation cost of the photovoltaic system. The higher the power of the photovoltaic module, the higher the photoelectric conversion efficiency of the solar cell will be required, making the manufacturing cost of the photovoltaic module higher. The weight power density of photovoltaic modules is in the range of 17 W / kg to 18.5 W / kg, which can not only meet the bearing capacity of common profiles on the market, but also control the cost of photovoltaic modules within the profit range of power generation.
[0092] In this application, the weight range of a single photovoltaic module is 27kg-33kg, and the size requirements of a single photovoltaic module are: length 2278mm or 1762mm or 2333mm or 2384mm or 2465mm, width 1134mm, thickness 30mm or 35mm. In this application, the output power of a single photovoltaic module is 565-585W. The overall photoelectric conversion efficiency of a single photovoltaic module is 21.9-22.6%. The size range of a single cell is 182*182mm or 210*210mm or 182*199mm.
[0093] The electrical connector 204, also known as a photovoltaic welding ribbon or welding ribbon, is used to electrically connect to the electrodes of the battery cell to collect the current converted by the battery cell. It is a component that realizes the electrical performance connection between the battery cells inside the photovoltaic module and is the core electrical connection component in the photovoltaic module. The quality of the electrical connector 204 directly affects the efficiency of the photovoltaic module in collecting electricity. In some embodiments, the electrical connector 204 includes an interconnection ribbon and a bus ribbon. The interconnection ribbon is used to connect the battery cells in series. An interconnection ribbon is welded on the back of each battery cell, so that several battery cells are welded together in series to form a battery string. The bus ribbon is a carrier for connecting the battery string. The bus ribbon connects the battery strings connected in series together, and finally leads to the positive and negative electrodes and connects to the junction box 205. In some embodiments, the interconnection ribbon and the bus ribbon are both tin-coated copper ribbons.
[0094] The cover plate includes an upper cover plate 201 and a lower cover plate 203. Generally, the side of the photovoltaic module directly facing the light source (such as sunlight) is called the front side, and the side away from the light source is called the back side. The upper cover plate 201 is located on the front side of the photovoltaic module and is also called the panel. The upper cover plate 201 is made of transparent material, and the light transmittance in the spectral wavelength range of 320nm-1100nm is more than 91%. It is generally tempered glass, also known as photovoltaic glass. Photovoltaic glass is a special glass that can utilize solar radiation and draw out current. It is also the outermost light-transmitting packaging panel of the photovoltaic module. It mainly plays a role of light transmission and protection. Its quality directly affects the power generation efficiency and service life of the photovoltaic module. Tempered glass is divided into coated glass and ordinary glass. Tempered glass uses low-iron ultra-white velvet tempered glass, with a light transmittance of more than 90%, and can also withstand solar ultraviolet radiation. The lower cover plate 203 is located on the back of the photovoltaic module and is also called the back plate. The back plate is a packaging component on the back of the photovoltaic module, which has heat resistance, insulation and protection. Commonly used backplane materials include TPT, i.e. polyvinyl fluoride composite film (Tedlar / PET / Tedl, a three-layer composite film), which has good resistance to environmental corrosion, insulation properties and good bonding properties with packaging materials.
[0095] The packaging material 206 includes a photovoltaic packaging film, which is the bonding material between the panel, battery and backboard in the photovoltaic module, and plays the role of bonding, light transmission, protection and insulation. The photovoltaic packaging film is generally an EVA (Ethylene-Vinyl-Acetate-Copolymer) film or a POE (Polyolefin elastomer) film. EVA film is a thermosetting film that has advantages in adhesion, durability, optical properties, etc., and is widely used in current components and optical products. At the same time, EVA film is not sticky at room temperature and is easy to operate. The water vapor isolation performance and anti-PI (Potential Induced Degradation) characteristics of POE film are stronger than those of EVA film, and are particularly suitable for photovoltaic modules encapsulated by double-sided glass.
[0096] The frame 202 is the outermost packaging structure of the photovoltaic module, and is lightweight and can meet the characteristics of the photovoltaic module. The frame 202 can improve the overall mechanical strength of the module and facilitate the installation and transportation of the module. The frame 202 is generally an aluminum alloy frame, which is used to protect the edge of the cover plate and cooperate with the silicone edging to enhance the sealing performance of the photovoltaic module.
[0097] The junction box 205 can transmit the current generated in the photovoltaic module to the external circuit. The junction box 205 includes positive and negative lead wires and an electrical box connected to the outside. The junction box 205 includes a bypass diode that forms a bypass path to maintain normal operation when the module fails, and a blocking diode that prevents current backflow when the light is low.
[0098] The present application also proposes a method for preparing a photovoltaic module containing a TOPCon cell, comprising the following steps:
[0099] Cell sorting: Match and combine TOPCon cells 100 with the same performance; in order to improve the conversion efficiency of photovoltaic modules, cells with the same or similar performance must be matched and combined before packaging. The sorting step is to test and sort the cells according to the electrical performance and size required by the customer.
[0100] Welding: Connect multiple cells in series using electrical connectors 204;
[0101] Lamination: stack EVA, battery string, EVA, and back sheet on the panel from bottom to bottom to form a laminate;
[0102] Lamination: Heat and pressurize the stacked parts to combine them into an integral laminated assembly;
[0103] EL test: detects hidden defects in laminated components. Based on the principle of electroluminescence, the near-infrared detection method is used to detect hidden defects in photovoltaic cells and their components.
[0104] Frame installation: The laminated components without hidden defects are installed in the frame 202 filled with the packaging material 206, and then the cover plate 201 is installed. The frames are connected with angle keys to enhance the strength and sealing performance of the components.
[0105] Install the junction box 205: Install the junction box 205 on one side of the lower cover plate 203, and connect the electrical connector 204 led out from the battery cell to the junction box 205;
[0106] Cleaning: remove dirt from the surface of photovoltaic modules;
[0107] Photovoltaic performance test: Inspect the photovoltaic output power of photovoltaic modules, select qualified photovoltaic modules for finished product inspection, install the qualified panel structure and support structure to make photovoltaic modules containing TOPCon cells.
[0108] The outer layer Poly processing method of the TOPCon battery 100 includes the following steps:
[0109] A protective layer is formed in the gate line area of the silicon wafer, and the protective layer is used to protect the outer N layer corresponding to the gate line area. + -Poly layer is protected from removal;
[0110] Then remove the outer N layer without protection layer in the non-gate line area + -Poly layer, so that the N + -Poly layer thickness is greater than N in non-gate line area +-Poly layer thickness, and the thickness of the protruding part is N + -H times the thickness of the Poly layer, H ≥ 0.5.
[0111] Embodiment 2
[0112] In this embodiment, the present application proposes a TOPCon cell, including an N-type silicon wafer layer 101, wherein a boron diffusion layer 102, a passivation layer 103, a front anti-reflection layer 104 and a front electrode 105 are stacked on the front side of the N-type silicon wafer layer 101, and at least two groups of oxide layers and an N-type silicon wafer layer 101 are stacked on the back side. + -Poly layer, back anti-reflection layer 110, back electrode 111. Among them, the oxide layer and N + -Poly layer has two groups, including the first SiO2 layer 106, the first N + -Poly layer 107, second SiO2 layer 108, second N + -Poly layer 109.
[0113] Here, the distance from the N-type silicon layer 101 is defined as from inner to outer. + -Poly layer 107 is the inner layer, the second N + -Poly layer 109 is the outer layer.
[0114] The front electrode 105 penetrates the front anti-reflection layer 104 and the passivation layer 103 to form an ohmic contact with the boron diffusion layer 102, and the back electrode 111 penetrates the back anti-reflection layer 110 to form an ohmic contact with the second N + -Poly layer 109 (ie outer layer) forms an ohmic contact.
[0115] The front electrode 105 is an Ag paste electrode formed by printing and sintering. The Ag paste does not contain Al powder. The front electrode 105 is prepared by pure Ag paste, in which the Al content is zero. Compared with the conventional Ag-Al paste electrode, the pure Ag paste electrode has a lower resistivity; the elimination of Al powder in the paste composition leads to a decrease in the metal diffusion penetration depth, a decrease in the composite current density in the metal area, and an increase in Voc; the elimination of Al powder and the change of glass material improve the corrosion resistance of the front metal electrode to carboxylic acid, reduce DH attenuation, and improve battery reliability.
[0116] As an optional implementation, Figure 8 As shown, the outer layer N of the non-gate line area + -The Poly layer is completely removed, that is, only the N layer of the gate line area corresponding to the back electrode is + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness, and the thickness of the protruding part is N +-0.5-5 times the thickness of the Poly layer. + -Poly layer thickness is less than N in the gate line area + -Poly layer thickness, that is, local thinning is achieved, so as to solve the problem that after the overall thinning of Poly Si, the doping amount of impurity atoms in the printing area becomes lower, and the passivation and contact effects will also be reduced.
[0117] As another optional implementation, Figure 7 As shown, the outer layer N of the non-gate line area + - Only part of the Poly layer is removed, that is, only the N layer of the gate line area corresponding to the back electrode is removed. + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness, and the thickness of the protruding part is N + -Poly layer thickness is 0.5-5 times, and the thickness of the outer N+-Poly layer in the non-gate line area is 10-20nm.
[0118] When the outer layer N + -When only part of the Poly layer is removed, that is, if the outer N layer is retained + - If there is still 10-20nm of the Poly layer left, the outer oxide layer between the inner and outer sides is still retained. + -The Poly layer has a different refractive index for light, so there will be better light absorption, which will significantly contribute to the improvement of Isc (short-circuit current). At the same time, the existence of the outer oxide layer will also cause the doping concentration to form an internal and external gradient, thereby greatly improving the passivation ability and ultimately greatly improving the conversion efficiency of the battery.
[0119] This embodiment also provides a TOPCon battery outer layer Poly processing method, including: forming a protective layer in the silicon wafer gate line area, the protective layer is used to protect the outer layer N corresponding to the gate line area + -Poly layer is not removed; then remove the outer N layer without protection layer in non-gate line area + -Poly layer, so that the N + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness, and the thickness of the protruding part is N + -H times the thickness of the Poly layer, H≥0.5. The value range of H can be 0.5-5.
[0120] The outer layer N without protection layer in non-gate line area + -Poly layer is partially removed, and the outer N layer of non-gate line area + -The remaining thickness of the Poly layer is K, K≥10nm. The value range of K can be 10-20nm.
[0121] Embodiment 3
[0122] In this application, a method for preparing a TOPCon battery is also proposed, comprising the following steps:
[0123] S1. Select an N-type single crystal silicon wafer as a substrate and perform double-sided texturing to form an anti-reflection structure. The N-type single crystal silicon wafer has a thickness of 100-160 microns and a resistivity of 0.4-10Ω·cm.
[0124] S2. Use a low-pressure and high-temperature diffusion furnace to diffuse boron on the front side of the N-type single crystal silicon wafer to form a boron diffusion layer.
[0125] S3, first remove the BSG layer on the back and side of the silicon wafer, and then perform alkali polishing on the back of the silicon wafer. Since the alkali solution does not react with BSG, removing the BSG layer first is conducive to the subsequent alkali polishing.
[0126] S4. Use LPCVD equipment to deposit at least two groups of oxide layers and polysilicon layers on the back side of the N-type single crystal silicon wafer to form an intrinsic Poly tunneling passivation structure.
[0127] S5, doping the back of the silicon wafer with phosphorus to form N + -Poly layer, and a PSG layer is formed on the outer layer.
[0128] S6. Use HF solution to remove the PSG layer on the front and side of the silicon wafer. When phosphorus diffuses, an excess PSG layer will also be deposited on the front. After it is removed, it will be beneficial for subsequent alkaline etching and Poly plating. Since the alkaline solution does not react with PSG, HF solution is used here.
[0129] S7. Form a mask layer in the gate line region on the back side of the silicon wafer. The mask layer is used to protect the polysilicon layer corresponding to the gate line region from being removed.
[0130] S8, remove the excess Poly layer on the front and sides of the silicon wafer, and the outer N layer on the back without mask layer protection + -Poly layer, so that the N + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness, and the thickness of the protruding part is N + -0.5-5 times the thickness of the Poly layer, and the outer N layer in the non-gate line area + -Poly layer thickness is 10-20nm; then remove the PSG in the non-mask area on the back, the back mask layer and the PSG layer here.
[0131] S9. Form a passivation layer, a front anti-reflection layer, and a back anti-reflection layer on the silicon wafer, such as an AlOx passivation layer or a SiNx anti-reflection layer.
[0132] S10, screen printing and sintering are performed on the front and back sides of the silicon wafer to form a front electrode and a back electrode, and the position of the back electrode corresponds to the position of the patterned mask, thereby manufacturing the TOPCon battery in the above embodiment.
[0133] Embodiment 4
[0134] In this application, a method for preparing a TOPCon battery is also proposed, comprising the following steps:
[0135] S1. Select an N-type single crystal silicon wafer as a substrate and perform double-sided texturing treatment to form an anti-reflection structure.
[0136] S2. Use a low-pressure and high-temperature diffusion furnace to diffuse boron on the front side of the N-type single crystal silicon wafer to form a boron diffusion layer. Perform boron doping to form a PN junction.
[0137] It should be noted that when using a low-pressure and high-temperature diffusion furnace to diffuse boron on the front side of the silicon wafer, the diffusion temperature is 800-1100°C and the diffusion time is 10-50 minutes.
[0138] S3, first remove the BSG layer on the back and side of the silicon wafer, and then perform alkali polishing on the back of the silicon wafer. Since the alkali solution does not react with BSG, removing the BSG layer first is conducive to the subsequent alkali polishing.
[0139] S4. Use LPCVD equipment to deposit at least two groups of oxide layers and polysilicon layers on the back side of the N-type single crystal silicon wafer to form an intrinsic Poly tunneling passivation structure.
[0140] S5, doping the back of the silicon wafer with phosphorus to form N + -Poly layer, and a PSG layer is formed on the outer layer.
[0141] S6. Use HF solution to remove the PSG layer on the front and side of the silicon wafer. When phosphorus diffuses, an excess PSG layer will also be deposited on the front. After it is removed, it will be beneficial for subsequent alkaline etching and Poly plating. Since the alkaline solution does not react with PSG, HF solution is used here.
[0142] S7. Form a mask layer in the gate line region on the back side of the silicon wafer. The mask layer is used to protect the polysilicon layer corresponding to the gate line region from being removed.
[0143] S8, remove the excess Poly layer on the front and sides of the silicon wafer, and the outer N layer on the back without mask layer protection + -Poly layer, so that the N + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness, and the thickness of the protruding part is N +-0.5-5 times the thickness of the Poly layer, and the outer N layer in the non-gate line area + -Poly layer thickness is 10-20nm; then remove the PSG in the non-mask area on the back, the back mask layer and the PSG layer here.
[0144] S9. Form a passivation layer, a front anti-reflection layer, and a back anti-reflection layer on the silicon wafer, such as an AlOx passivation layer or a SiNx anti-reflection layer.
[0145] S10, screen printing and sintering are performed on the front and back sides of the silicon wafer to form a front electrode and a back electrode, and the position of the back electrode corresponds to the position of the patterned mask, thereby manufacturing the TOPCon battery in the above embodiment.
[0146] Embodiment 5
[0147] In this application, a method for preparing a TOPCon battery is also proposed, comprising the following steps:
[0148] S1. Select an N-type single crystal silicon wafer as a substrate and perform double-sided texturing treatment to form an anti-reflection structure.
[0149] S2. Use a low-pressure, high-temperature diffusion furnace to diffuse boron on the front side of the N-type single crystal silicon wafer to form a boron diffusion layer. Perform boron doping to form a PN junction. It should be noted that the sheet resistance of the boron diffusion layer after diffusion is 100-260Ω / sq, the junction depth is 0.1-0.4 microns, and the BSG layer thickness is 100-160 nanometers.
[0150] S3, first remove the BSG layer on the back and side of the silicon wafer, and then perform alkali polishing on the back of the silicon wafer. Since the alkali solution does not react with BSG, removing the BSG layer first is conducive to the subsequent alkali polishing.
[0151] S4. Use LPCVD equipment to deposit at least two groups of oxide layers and polysilicon layers on the back side of the N-type single crystal silicon wafer to form an intrinsic Poly tunneling passivation structure.
[0152] S5, doping the back of the silicon wafer with phosphorus to form N + -Poly layer, and a PSG layer is formed on the outer layer.
[0153] S6. Use HF solution to remove the PSG layer on the front and side of the silicon wafer. When phosphorus diffuses, an excess PSG layer will also be deposited on the front. After it is removed, it will be beneficial for subsequent alkaline etching and Poly plating. Since the alkaline solution does not react with PSG, HF solution is used here.
[0154] S7. Form a mask layer in the gate line region on the back side of the silicon wafer. The mask layer is used to protect the polysilicon layer corresponding to the gate line region from being removed.
[0155] S8, remove the excess Poly layer on the front and sides of the silicon wafer, and the outer N layer on the back without mask layer protection + -Poly layer, so that the N + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness, and the thickness of the protruding part is N + -0.5-5 times the thickness of the Poly layer, and the outer N layer in the non-gate line area + -Poly layer thickness is 10-20nm; then remove the PSG in the non-mask area on the back, the back mask layer and the PSG layer here.
[0156] S9. Form a passivation layer, a front anti-reflection layer, and a back anti-reflection layer on the silicon wafer, such as an AlOx passivation layer or a SiNx anti-reflection layer.
[0157] S10, screen printing and sintering are performed on the front and back sides of the silicon wafer to form a front electrode and a back electrode, and the position of the back electrode corresponds to the position of the patterned mask, thereby manufacturing the TOPCon battery in the above embodiment.
[0158] Embodiment 6
[0159] In this application, a method for preparing a TOPCon battery is also proposed, comprising the following steps:
[0160] S1. Select an N-type single crystal silicon wafer as a substrate and perform double-sided texturing treatment to form an anti-reflection structure.
[0161] S2. Use a low-pressure and high-temperature diffusion furnace to diffuse boron on the front side of the N-type single crystal silicon wafer to form a boron diffusion layer. Perform boron doping to form a PN junction.
[0162] S3, first remove the BSG layer on the back and side of the silicon wafer, and then perform alkali polishing on the back of the silicon wafer. Since the alkali solution does not react with BSG, removing the BSG layer first is conducive to the subsequent alkali polishing.
[0163] S4. Use LPCVD equipment to deposit at least two groups of oxide layers and polysilicon layers on the back side of the N-type single crystal silicon wafer to form an intrinsic Poly tunneling passivation structure.
[0164] LPCVD equipment can complete the preparation of tunneling SiO2 layer and Poly layer in one stop. The two-in-one process of thermal oxidation and deposition of Poly layer can greatly increase production capacity and reduce equipment cost, which has great advantages over other equipment. After the thermal oxidation process is completed, the Poly layer is deposited under low pressure. In addition to saving time, more importantly, it can protect the ultra-thin silicon oxide layer. On the one hand, the oxide layer will not be further oxidized during the process of leaving the boat and lose the tunneling effect; on the other hand, the oxide layer will not be contaminated in the air.
[0165] In step S4, there are two groups of oxide layers and polysilicon layers, including a first SiO2 layer, a first Poly layer, a second SiO2 layer, and a second Poly layer which are sequentially stacked from the inner layer to the outer layer.
[0166] S5, doping the back of the silicon wafer with phosphorus to form N + -Poly layer, and a PSG layer is formed on the outer layer.
[0167] S6. Use HF solution to remove the PSG layer on the front and side of the silicon wafer. When phosphorus diffuses, an excess PSG layer will also be deposited on the front. After it is removed, it will be beneficial for subsequent alkaline etching and Poly plating. Since the alkaline solution does not react with PSG, HF solution is used here.
[0168] S7. Form a mask layer in the gate line region on the back side of the silicon wafer. The mask layer is used to protect the polysilicon layer corresponding to the gate line region from being removed.
[0169] S8, remove the excess Poly layer on the front and sides of the silicon wafer, and the outer N layer on the back without mask layer protection + -Poly layer, so that the N + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness, and the thickness of the protruding part is N + -0.5-5 times the thickness of the Poly layer, and the outer N layer in the non-gate line area + -Poly layer thickness is 10-20nm; then remove the PSG in the non-mask area on the back, the back mask layer and the PSG layer here.
[0170] S9, make a passivation layer, a front anti-reflection layer, and a back anti-reflection layer on the silicon wafer, such as AlO x Passivation layer or SiN x Anti-reflection layer.
[0171] S10, screen printing and sintering are performed on the front and back sides of the silicon wafer to form a front electrode and a back electrode, and the position of the back electrode corresponds to the position of the patterned mask, thereby manufacturing the TOPCon battery in the above embodiment.
[0172] Embodiment 7
[0173] In this application, a method for preparing a TOPCon battery is also proposed, comprising the following steps:
[0174] S1. Select an N-type single crystal silicon wafer as a substrate and perform double-sided texturing treatment to form an anti-reflection structure.
[0175] S2. Use a low-pressure and high-temperature diffusion furnace to diffuse boron on the front side of the N-type single crystal silicon wafer to form a boron diffusion layer. Perform boron doping to form a PN junction.
[0176] S3, first remove the BSG layer on the back and side of the silicon wafer, and then perform alkali polishing on the back of the silicon wafer. Since the alkali solution does not react with BSG, removing the BSG layer first is conducive to the subsequent alkali polishing.
[0177] S4. Use LPCVD equipment to deposit at least two groups of oxide layers and polysilicon layers on the back side of the N-type single crystal silicon wafer to form an intrinsic Poly tunneling passivation structure.
[0178] LPCVD equipment can complete the preparation of tunneling SiO2 layer and Poly layer in one stop. The two-in-one process of thermal oxidation and deposition of Poly layer can greatly increase production capacity and reduce equipment cost, which has great advantages over other equipment. After the thermal oxidation process is completed, the Poly layer is deposited under low pressure. In addition to saving time, more importantly, it can protect the ultra-thin silicon oxide layer. On the one hand, the oxide layer will not be further oxidized during the process of leaving the boat and lose the tunneling effect; on the other hand, the oxide layer will not be contaminated in the air.
[0179] In step S4, there are two groups of oxide layers and polysilicon layers, including a first SiO2 layer, a first Poly layer, a second SiO2 layer, and a second Poly layer which are sequentially stacked from the inner layer to the outer layer.
[0180] The thickness of the first SiO2 layer is 1-2 nm, the thickness of the first Poly layer is 20-40 nm, the thickness of the second SiO2 layer is 0.5-2 nm, and the thickness of the second Poly layer is 30-150 nm.
[0181] S5, doping the back of the silicon wafer with phosphorus to form N + -Poly layer, and a PSG layer is formed on the outer layer.
[0182] S6. Use HF solution to remove the PSG layer on the front and side of the silicon wafer. When phosphorus diffuses, an excess PSG layer will also be deposited on the front. After it is removed, it will be beneficial for subsequent alkaline etching and Poly plating. Since the alkaline solution does not react with PSG, HF solution is used here.
[0183] S7. Form a mask layer in the gate line region on the back side of the silicon wafer. The mask layer is used to protect the polysilicon layer corresponding to the gate line region from being removed.
[0184] S8, remove the excess Poly layer on the front and sides of the silicon wafer, and the outer N layer on the back without mask layer protection + -Poly layer, so that the N + -Poly layer thickness is greater than N in non-gate line area +-Poly layer thickness, and the thickness of the protruding part is N + -0.5-5 times the thickness of the Poly layer, and the outer N layer in the non-gate line area + -Poly layer thickness is 10-20nm; then remove the PSG in the non-mask area on the back, the back mask layer and the PSG layer here.
[0185] S9. Form a passivation layer, a front anti-reflection layer, and a back anti-reflection layer on the silicon wafer, such as an AlOx passivation layer or a SiNx anti-reflection layer.
[0186] S10, screen printing and sintering are performed on the front and back sides of the silicon wafer to form a front electrode and a back electrode, and the position of the back electrode corresponds to the position of the patterned mask, thereby manufacturing the TOPCon battery in the above embodiment.
[0187] Embodiment 8
[0188] In this application, a method for preparing a TOPCon battery is also proposed, comprising the following steps:
[0189] S1. Select an N-type single crystal silicon wafer as a substrate and perform double-sided texturing treatment to form an anti-reflection structure.
[0190] S2. Use a low-pressure and high-temperature diffusion furnace to diffuse boron on the front side of the N-type single crystal silicon wafer to form a boron diffusion layer. Perform boron doping to form a PN junction.
[0191] S3, first remove the BSG layer on the back and side of the silicon wafer, and then perform alkali polishing on the back of the silicon wafer. Since the alkali solution does not react with BSG, removing the BSG layer first is conducive to the subsequent alkali polishing.
[0192] S4. Use LPCVD equipment to deposit at least two groups of oxide layers and polysilicon layers on the back side of the N-type single crystal silicon wafer to form an intrinsic Poly tunneling passivation structure.
[0193] LPCVD equipment can complete the preparation of tunneling SiO2 layer and Poly layer in one stop. The two-in-one process of thermal oxidation and deposition of Poly layer can greatly increase production capacity and reduce equipment cost, which has great advantages over other equipment. After the thermal oxidation process is completed, the Poly layer is deposited under low pressure. In addition to saving time, more importantly, it can protect the ultra-thin silicon oxide layer. On the one hand, the oxide layer will not be further oxidized during the process of leaving the boat and lose the tunneling effect; on the other hand, the oxide layer will not be contaminated in the air.
[0194] S5, doping the back of the silicon wafer with phosphorus to form N + -Poly layer, and a PSG layer is formed on the outer layer, at this time, the first SiO2 layer 106 and the first N +-Poly layer 107, second SiO2 layer 108, second N + -Poly layer 109 structure, it should be noted that the distance from the N-type silicon layer 101 is defined as from inner to outer, then the first N + -Poly layer 107 is the inner layer, the second N + -Poly layer 109 is the outer layer.
[0195] In step S5, the phosphorus doping concentration range of the inner and outer layers of Poly is 0.1-2E 21 .
[0196] S6. Use HF solution to remove the PSG layer on the front and side of the silicon wafer. When phosphorus diffuses, an excess PSG layer will also be deposited on the front. After it is removed, it will be beneficial for subsequent alkaline etching and Poly plating. Since the alkaline solution does not react with PSG, HF solution is used here.
[0197] S7. Form a mask layer in the gate line region on the back side of the silicon wafer. The mask layer is used to protect the polysilicon layer corresponding to the gate line region from being removed.
[0198] S8, remove the excess Poly layer on the front and sides of the silicon wafer, and the outer N layer on the back without mask layer protection + -Poly layer, so that the N + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness, and the thickness of the protruding part is N + -0.5-5 times the thickness of the Poly layer, and the outer N layer in the non-gate line area + -Poly layer thickness is 10-20nm; then remove the PSG in the non-mask area on the back, the back mask layer and the PSG layer here.
[0199] S9. Form a passivation layer, a front anti-reflection layer, and a back anti-reflection layer on the silicon wafer, such as an AlOx passivation layer or a SiNx anti-reflection layer.
[0200] S10, screen printing and sintering are performed on the front and back sides of the silicon wafer to form a front electrode and a back electrode, and the position of the back electrode corresponds to the position of the patterned mask, thereby manufacturing the TOPCon battery in the above embodiment.
[0201] Embodiment 9
[0202] In this application, a method for preparing a TOPCon battery is also proposed, comprising the following steps:
[0203] S1. Select an N-type single crystal silicon wafer as a substrate and perform double-sided texturing treatment to form an anti-reflection structure.
[0204] S2. Use a low-pressure and high-temperature diffusion furnace to diffuse boron on the front side of the N-type single crystal silicon wafer to form a boron diffusion layer. Perform boron doping to form a PN junction.
[0205] S3, first remove the BSG layer on the back and side of the silicon wafer, and then perform alkali polishing on the back of the silicon wafer. Since the alkali solution does not react with BSG, removing the BSG layer first is conducive to the subsequent alkali polishing.
[0206] S4. Use LPCVD equipment to deposit at least two groups of oxide layers and polysilicon layers on the back side of the N-type single crystal silicon wafer to form an intrinsic Poly tunneling passivation structure.
[0207] LPCVD equipment can complete the preparation of tunneling SiO2 layer and Poly layer in one stop. The two-in-one process of thermal oxidation and deposition of Poly layer can greatly increase production capacity and reduce equipment cost, which has great advantages over other equipment. After the thermal oxidation process is completed, the Poly layer is deposited under low pressure. In addition to saving time, more importantly, it can protect the ultra-thin silicon oxide layer. On the one hand, the oxide layer will not be further oxidized during the process of leaving the boat and lose the tunneling effect; on the other hand, the oxide layer will not be contaminated in the air.
[0208] S5, doping the back of the silicon wafer with phosphorus to form N + -Poly layer, and a PSG layer is formed on the outer layer, at this time, the first SiO2 layer 106 and the first N + -Poly layer 107, second SiO2 layer 108, second N + -Poly layer 109 structure, it should be noted that the distance from the N-type silicon layer 101 is defined as from inner to outer, then the first N + -Poly layer 107 is the inner layer, the second N + -Poly layer 109 is the outer layer.
[0209] In step S5, the phosphorus doping concentration range of the inner and outer layers of Poly is 0.1-2E 21 .
[0210] S6. Use HF solution to remove the PSG layer on the front and side of the silicon wafer. When phosphorus diffuses, an excess PSG layer will also be deposited on the front. After it is removed, it will be beneficial for subsequent alkaline etching and Poly plating. Since the alkaline solution does not react with PSG, HF solution is used here.
[0211] S7, a mask layer is formed in the gate line area on the back of the silicon wafer, and the mask layer is used to protect the polysilicon layer corresponding to the gate line area from being removed. In this step, a patterned masking technology is used, and a layer of Si-containing slurry is first applied to the gate line area on the back of the silicon wafer, and then dried at high temperature to form a SiO2 mask layer in the gate line area of the silicon wafer, thereby playing a protective role during the subsequent alkali solution treatment. Among them, the thickness of the Si-containing slurry applied is 100-1000nm. Since the mask layer is only difficult to react with the alkali solution but not completely non-reactive with the alkali solution, the slurry should not be too thin at this time to avoid losing the protective effect.
[0212] S8, remove the excess Poly layer on the front and sides of the silicon wafer, and the outer N layer on the back without mask layer protection + -Poly layer, so that the N + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness, and the thickness of the protruding part is N + -0.5-5 times the thickness of the Poly layer, and the outer N layer in the non-gate line area + -Poly layer thickness is 10-20nm; then remove the PSG in the non-mask area on the back, the back mask layer and the PSG layer here.
[0213] S9. Form a passivation layer, a front anti-reflection layer, and a back anti-reflection layer on the silicon wafer, such as an AlOx passivation layer or a SiNx anti-reflection layer.
[0214] S10, screen printing and sintering are performed on the front and back sides of the silicon wafer to form a front electrode and a back electrode, and the position of the back electrode corresponds to the position of the patterned mask, thereby manufacturing the TOPCon battery in the above embodiment.
[0215] Embodiment 10
[0216] In this application, a method for preparing a TOPCon battery is also proposed, comprising the following steps:
[0217] S1. Select an N-type single crystal silicon wafer as a substrate and perform double-sided texturing treatment to form an anti-reflection structure.
[0218] S2. Use a low-pressure and high-temperature diffusion furnace to diffuse boron on the front side of the N-type single crystal silicon wafer to form a boron diffusion layer. Perform boron doping to form a PN junction.
[0219] S3, first remove the BSG layer on the back and side of the silicon wafer, and then perform alkali polishing on the back of the silicon wafer. Since the alkali solution does not react with BSG, removing the BSG layer first is conducive to the subsequent alkali polishing.
[0220] S4. Use LPCVD equipment to deposit at least two groups of oxide layers and polysilicon layers on the back side of the N-type single crystal silicon wafer to form an intrinsic Poly tunneling passivation structure.
[0221] LPCVD equipment can complete the preparation of tunneling SiO2 layer and Poly layer in one stop. The two-in-one process of thermal oxidation and deposition of Poly layer can greatly increase production capacity and reduce equipment cost, which has great advantages over other equipment. After the thermal oxidation process is completed, the Poly layer is deposited under low pressure. In addition to saving time, more importantly, it can protect the ultra-thin silicon oxide layer. On the one hand, the oxide layer will not be further oxidized during the process of leaving the boat and lose the tunneling effect; on the other hand, the oxide layer will not be contaminated in the air.
[0222] S5, doping the back of the silicon wafer with phosphorus to form N + -Poly layer, and a PSG layer is formed on the outer layer, at this time, the first SiO2 layer 106 and the first N + -Poly layer 107, second SiO2 layer 108, second N + -Poly layer 109 structure, it should be noted that the distance from the N-type silicon layer 101 is defined as from inner to outer, then the first N + -Poly layer 107 is the inner layer, the second N + -Poly layer 109 is the outer layer.
[0223] S6. Use HF solution to remove the PSG layer on the front and side of the silicon wafer. When phosphorus diffuses, an excess PSG layer will also be deposited on the front. After it is removed, it will be beneficial for subsequent alkaline etching and Poly plating. Since the alkaline solution does not react with PSG, HF solution is used here.
[0224] S7, a mask layer is formed in the gate line area on the back of the silicon wafer, and the mask layer is used to protect the polysilicon layer corresponding to the gate line area from being removed. In this step, a patterned masking technology is used, and a layer of Si-containing slurry is first applied to the gate line area on the back of the silicon wafer, and then dried at high temperature to form a SiO2 mask layer in the gate line area of the silicon wafer, thereby playing a protective role during the subsequent alkali solution treatment. Among them, the thickness of the Si-containing slurry applied is 100-1000nm. Since the mask layer is only difficult to react with the alkali solution but not completely non-reactive with the alkali solution, the slurry should not be too thin at this time to avoid losing the protective effect.
[0225] The graphic mask technology in step S7 specifically includes the following steps: first, a mask plate is made of metal, non-metal, alloy, composite material and the like, and then a hollow pattern corresponding to the position of the screen-printed back grid line pattern is made on the mask plate, and after using inorganic Si and organic solvent to prepare a Si-containing slurry that maintains rheological properties and wettability, a roller is used to immerse the slurry, and an outer layer similar to a sponge that can absorb the slurry can be set on the roller, and then the slurry is roller-coated onto the mask plate, so that the slurry is attached to the back grid line area of the silicon wafer through the hollow pattern, and then the temperature is set to 300-700°C in a chain heating furnace for drying.
[0226] When using Si-containing slurry, Si will not bring the risk of reducing battery performance. Secondly, the SiO2 mask layer formed is difficult to react with alkali solution at room temperature. Therefore, alkali solution is used to remove the excess Poly layer on the front and side of the silicon wafer and the outer N layer on the back without mask layer protection. + -Poly layer, this mask layer can protect the gate line area of the mask layer. + -Poly layer forms protection, so that only the outer N layer of the non-gate line area is thinned + After removing the PSG in the non-mask area of the back side with acid, the back mask layer and the PSG layer here, the passivation layer, anti-reflection layer and electrode can be produced, thereby obtaining the N-type layer in the gate line area corresponding to the back electrode. + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness TOPCon battery, thereby improving the shortcomings of the current TOPCon battery and further improving the photoelectric conversion efficiency.
[0227] S8, remove the excess Poly layer on the front and sides of the silicon wafer, and the outer N layer on the back without mask layer protection + -Poly layer, so that the N + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness, and the thickness of the protruding part is N + -0.5-5 times the thickness of the Poly layer, and the outer N layer in the non-gate line area + -Poly layer thickness is 10-20nm; then remove the PSG in the non-mask area on the back, the back mask layer and the PSG layer here.
[0228] S9. Form a passivation layer, a front anti-reflection layer, and a back anti-reflection layer on the silicon wafer, such as an AlOx passivation layer or a SiNx anti-reflection layer.
[0229] S10, screen printing and sintering are performed on the front and back sides of the silicon wafer to form a front electrode and a back electrode, and the position of the back electrode corresponds to the position of the patterned mask, thereby manufacturing the TOPCon battery in the above embodiment.
[0230] Embodiment 11
[0231] In this application, a method for preparing a TOPCon battery is also proposed, comprising the following steps:
[0232] S1. Select an N-type single crystal silicon wafer as a substrate and perform double-sided texturing treatment to form an anti-reflection structure.
[0233] S2. Use a low-pressure and high-temperature diffusion furnace to diffuse boron on the front side of the N-type single crystal silicon wafer to form a boron diffusion layer. Perform boron doping to form a PN junction.
[0234] S3, first remove the BSG layer on the back and side of the silicon wafer, and then perform alkali polishing on the back of the silicon wafer. Since the alkali solution does not react with BSG, removing the BSG layer first is conducive to the subsequent alkali polishing.
[0235] S4. Use LPCVD equipment to deposit at least two groups of oxide layers and polysilicon layers on the back side of the N-type single crystal silicon wafer to form an intrinsic Poly tunneling passivation structure.
[0236] LPCVD equipment can complete the preparation of tunneling SiO2 layer and Poly layer in one stop. The two-in-one process of thermal oxidation and deposition of Poly layer can greatly increase production capacity and reduce equipment cost, which has great advantages over other equipment. After the thermal oxidation process is completed, the Poly layer is deposited under low pressure. In addition to saving time, more importantly, it can protect the ultra-thin silicon oxide layer. On the one hand, the oxide layer will not be further oxidized during the process of leaving the boat and lose the tunneling effect; on the other hand, the oxide layer will not be contaminated in the air.
[0237] S5, doping the back of the silicon wafer with phosphorus to form N + -Poly layer, and a PSG layer is formed on the outer layer, at this time, the first SiO2 layer 106 and the first N + -Poly layer 107, second SiO2 layer 108, second N + -Poly layer 109 structure, it should be noted that the distance from the N-type silicon layer 101 is defined as from inner to outer, then the first N + -Poly layer 107 is the inner layer, the second N + -Poly layer 109 is the outer layer.
[0238] S6. Use HF solution to remove the PSG layer on the front and side of the silicon wafer. When phosphorus diffuses, an excess PSG layer will also be deposited on the front. After it is removed, it will be beneficial for subsequent alkaline etching and Poly plating. Since the alkaline solution does not react with PSG, HF solution is used here.
[0239] S7, a mask layer is formed in the gate line area on the back of the silicon wafer, and the mask layer is used to protect the polysilicon layer corresponding to the gate line area from being removed. In this step, a patterned masking technology is used, and a layer of Si-containing slurry is first applied to the gate line area on the back of the silicon wafer, and then dried at high temperature to form a SiO2 mask layer in the gate line area of the silicon wafer, thereby playing a protective role during the subsequent alkali solution treatment. Among them, the thickness of the Si-containing slurry applied is 100-1000nm. Since the mask layer is only difficult to react with the alkali solution but not completely non-reactive with the alkali solution, the slurry should not be too thin at this time to avoid losing the protective effect.
[0240] S8, remove the excess Poly layer on the front and sides of the silicon wafer, and the outer N layer on the back without mask layer protection + -Poly layer, so that the N + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness, and the thickness of the protruding part is N + -0.5-5 times the thickness of the Poly layer, and the outer N layer in the non-gate line area + -Poly layer thickness is 10-20nm; then remove the PSG in the non-mask area on the back, the back mask layer and the PSG layer here.
[0241] Specifically, an alkali solution is used to remove the excess Poly layer on the front and sides of the silicon wafer, and the outer N layer on the back without mask layer protection. + -Poly layer; use acid to remove the PSG in the non-mask area on the back, the back mask layer and the PSG layer here.
[0242] S9. Form a passivation layer, a front anti-reflection layer, and a back anti-reflection layer on the silicon wafer, such as an AlOx passivation layer or a SiNx anti-reflection layer.
[0243] S10, screen printing and sintering are performed on the front and back sides of the silicon wafer to form a front electrode and a back electrode, and the position of the back electrode corresponds to the position of the patterned mask, thereby manufacturing the TOPCon battery in the above embodiment.
[0244] Embodiment 12
[0245] In this application, a method for preparing a TOPCon battery is also proposed, comprising the following steps:
[0246] S1. Select an N-type single crystal silicon wafer as a substrate and perform double-sided texturing to form an anti-reflection structure. The N-type single crystal silicon wafer has a thickness of 100-160 microns and a resistivity of 0.4-10Ω·cm.
[0247] S2. Use a low-pressure and high-temperature diffusion furnace to diffuse boron on the front side of the N-type single crystal silicon wafer to form a boron diffusion layer. Perform boron doping to form a PN junction.
[0248] It should be noted that when using a low-pressure high-temperature diffusion furnace to diffuse boron on the front side of the silicon wafer, the diffusion temperature is 800-1100°C and the diffusion time is 10-50 minutes. The sheet resistance of the boron diffusion layer after diffusion is 100-260Ω / sq, the junction depth is 0.1-0.4 microns, and the BSG layer thickness is 100-160 nanometers.
[0249] S3, first remove the BSG layer on the back and side of the silicon wafer, and then perform alkali polishing on the back of the silicon wafer. Since the alkali solution does not react with BSG, removing the BSG layer first is conducive to the subsequent alkali polishing.
[0250] S4. Use LPCVD equipment to deposit at least two groups of oxide layers and polysilicon layers on the back side of the N-type single crystal silicon wafer to form an intrinsic Poly tunneling passivation structure.
[0251] LPCVD equipment can complete the preparation of tunneling SiO2 layer and Poly layer in one stop. The two-in-one process of thermal oxidation and deposition of Poly layer can greatly increase production capacity and reduce equipment cost, which has great advantages over other equipment. After the thermal oxidation process is completed, the Poly layer is deposited under low pressure. In addition to saving time, more importantly, it can protect the ultra-thin silicon oxide layer. On the one hand, the oxide layer will not be further oxidized during the process of leaving the boat and lose the tunneling effect; on the other hand, the oxide layer will not be contaminated in the air.
[0252] In step S4, there are two groups of oxide layers and polysilicon layers, including a first SiO2 layer, a first Poly layer, a second SiO2 layer, and a second Poly layer which are sequentially stacked from the inner layer to the outer layer.
[0253] The thickness of the first SiO2 layer is 1-2 nm, the thickness of the first Poly layer is 20-40 nm, the thickness of the second SiO2 layer is 0.5-2 nm, and the thickness of the second Poly layer is 30-150 nm.
[0254] S5, doping the back of the silicon wafer with phosphorus to form N + -Poly layer, and a PSG layer is formed on the outer layer, at this time, the first SiO2 layer 106 and the first N + -Poly layer 107, second SiO2 layer 108, second N + -Poly layer 109 structure, it should be noted that the distance from the N-type silicon layer 101 is defined as from inner to outer, then the first N + -Poly layer 107 is the inner layer, the second N + -Poly layer 109 is the outer layer.
[0255] In step S5, the phosphorus doping concentration range of the inner and outer layers of Poly is 0.1-2E21 .
[0256] S6. Use HF solution to remove the PSG layer on the front and side of the silicon wafer. When phosphorus diffuses, an excess PSG layer will also be deposited on the front. After it is removed, it will be beneficial for subsequent alkaline etching and Poly plating. Since the alkaline solution does not react with PSG, HF solution is used here.
[0257] S7, a mask layer is formed in the gate line area on the back of the silicon wafer, and the mask layer is used to protect the polysilicon layer corresponding to the gate line area from being removed. In this step, a patterned masking technology is used, and a layer of Si-containing slurry is first applied to the gate line area on the back of the silicon wafer, and then dried at high temperature to form a SiO2 mask layer in the gate line area of the silicon wafer, thereby playing a protective role during the subsequent alkali solution treatment. Among them, the thickness of the Si-containing slurry applied is 100-1000nm. Since the mask layer is only difficult to react with the alkali solution but not completely non-reactive with the alkali solution, the slurry should not be too thin at this time to avoid losing the protective effect.
[0258] The graphic mask technology in step S7 specifically includes the following steps: first, a mask plate is made of metal, non-metal, alloy, composite material and the like, and then a hollow pattern corresponding to the position of the screen-printed back grid line pattern is made on the mask plate, and after using inorganic Si and organic solvent to prepare a Si-containing slurry that maintains rheological properties and wettability, a roller is used to immerse the slurry, and an outer layer similar to a sponge that can absorb the slurry can be set on the roller, and then the slurry is roller-coated onto the mask plate, so that the slurry is attached to the back grid line area of the silicon wafer through the hollow pattern, and then the temperature is set to 300-700°C in a chain heating furnace for drying.
[0259] When using Si-containing slurry, Si will not bring the risk of reducing battery performance. Secondly, the SiO2 mask layer formed is difficult to react with alkali solution at room temperature. Therefore, alkali solution is used to remove the excess Poly layer on the front and side of the silicon wafer and the outer N layer on the back without mask layer protection. + -Poly layer, this mask layer can protect the N gate line area of the mask layer. + -Poly layer forms protection, so that only the outer N layer of the non-gate line area is thinned + After removing the PSG in the non-mask area of the back side with acid, the back mask layer and the PSG layer here, the passivation layer, anti-reflection layer and electrode can be produced, thereby obtaining the N-type layer in the gate line area corresponding to the back electrode. + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness TOPCon battery, thereby improving the shortcomings of the current TOPCon battery and further improving the photoelectric conversion efficiency.
[0260] S8, remove the excess Poly layer on the front and sides of the silicon wafer, and the outer N layer on the back without mask layer protection +-Poly layer, so that the N + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness, and the thickness of the protruding part is N + -0.5-5 times the thickness of the Poly layer, and the outer N layer in the non-gate line area + -Poly layer thickness is 10-20nm; then remove the PSG in the non-mask area on the back, the back mask layer and the PSG layer here.
[0261] Specifically, an alkali solution is used to remove the excess Poly layer on the front and sides of the silicon wafer, and the outer N layer on the back without mask layer protection. + -Poly layer; use acid to remove the PSG in the non-mask area on the back, the back mask layer and the PSG layer here.
[0262] S9, make a passivation layer, a front anti-reflection layer, and a back anti-reflection layer on the silicon wafer, such as AlO x Passivation layer or SiN x Anti-reflection layer.
[0263] S10, screen printing and sintering are performed on the front and back sides of the silicon wafer to form a front electrode and a back electrode, and the position of the back electrode corresponds to the position of the patterned mask, thereby manufacturing the TOPCon battery in the above embodiment.
[0264] The performance of the TOPCon battery proposed in this application is verified by specific experiments. The remaining preparation processes of the comparative example and experimental examples 1-8 are the same, except that the outer layer Poly of the comparative example is thinned overall, while the outer layer Poly of the experimental example is only thinned locally in the non-gridline area.
[0265] The outer layer N in the non-gate line area in Experimental Example 1-3 + - Poly is completely removed, and only the N + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness, and the thickness of the protruding part is N + -0.5-5 times the thickness of the Poly layer. Specifically, the remaining preparation processes of Experimental Examples 1-3 are the same, except that the outer N layer in the non-gate line area + -Poly before being thinned, the first SiO2 layer 106 in Experimental Example 1 is 1.5nm, the first N + -Poly layer 107 is 20nm, second SiO2 layer 108 is 1.7nm, second N + -Poly layer 109 is 100nm; in Experimental Example 2, the first SiO2 layer 106 is 1.5nm, the first N +-Poly layer 107 is 25nm, second SiO2 layer 108 is 1.7nm, second N + -Poly layer 109 is 120nm; in Experimental Example 3, the first SiO2 layer 106 is 1.5nm, the first N + -Poly layer 107 is 30nm, second SiO2 layer 108 is 1.7nm, second N + -Poly layer 109 is 130nm.
[0266] In Experimental Example 4, the outer layer N in the non-gate line area + -Poly still retains 10-20nm, and other step parameters are consistent with Experimental Example 3. In Experimental Example 5, the outer N + -Poly thickness is less than 10nm, and other step parameters are consistent with those in Experimental Example 3. + -Poly thickness is greater than 20nm, and other step parameters are consistent with those of Experimental Example 3. + -Poly thickness is N in non-gate line area + -Poly layer thickness is less than 0.5 times, and other step parameters are consistent with those of Experimental Example 3. + -Poly thickness is N in non-gate line area + -Poly layer thickness is more than 5 times, and other step parameters are consistent with Experimental Example 3.
[0267] The specific verification data is as follows:
[0268]
[0269] As can be seen from the above table, from a comprehensive comparison, the performance of Experimental Examples 1-3 is better than that of the comparative example. The performance of Experimental Example 4 is better than that of other Experimental Examples, and the performance of Experimental Example 3 is better than that of Experimental Examples 7-8.
[0270] According to the above data, let N of the gate line area corresponding to the back electrode + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness, and the thickness of the protruding part is N + -When the thickness of the Poly layer is 0.5-5 times, the photoelectric conversion efficiency of the TOPCon cell can be improved.
[0271] When the N of the gate line area corresponding to the back electrode is + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness, and the thickness of the protruding part is N + -0.5-5 times the thickness of the Poly layer, and the outer N layer in the non-grid area+ -When Poly is still 10-20nm, the photoelectric conversion efficiency of TOPCon cells can be further improved.
[0272] The present application achieves local thinning by removing the outer layer of Poly Si in the non-gridline area on the back side while leaving the outer layer of Poly Si in the gridline area unaffected, thereby improving the disadvantages of the current TOPCon cells and further improving the photoelectric conversion efficiency of the TOPCon cells of the photovoltaic module.
[0273] The present invention and its embodiments are described schematically above, and the description is not restrictive. The drawings show only one embodiment of the present invention, and the actual structure is not limited thereto. Therefore, if a person skilled in the art is inspired by it and designs a structural method and an embodiment similar to the technical solution without creativity without departing from the purpose of the invention, they shall all fall within the protection scope of the present invention.
Claims
1. A photovoltaic module containing a TOPCon cell, comprising a support mechanism and a panel mechanism; The support mechanism comprises a base (301), and an elevation adjustment mechanism is provided on the base (301), and the elevation adjustment mechanism is used to adjust the elevation angle of the panel fixing mechanism; the panel fixing mechanism is used to fix the panel mechanism; The panel mechanism comprises a frame (202), and the frame (202) is used to fix the upper cover plate (201) and the lower cover plate (203); a packaging material is provided between the upper cover plate (201) and the lower cover plate (203); Features: A plurality of TOPCon batteries (100) are encapsulated in the encapsulation material, and the plurality of TOPCon batteries (100) are connected in series through an electrical connector (204) and connected to a junction box (205); A method for preparing a photovoltaic module containing a TOPCon cell comprises the following steps: Cell sorting: Match and combine TOPCon cells with consistent performance; Welding: connecting multiple battery cells in series using an electrical connector (204); Lamination: stack EVA, battery string, EVA, and back sheet on the panel from bottom to bottom to form a laminate; Lamination: Heat and pressurize the stacked parts to combine them into an integral laminated assembly; EL test: detect whether the laminated components have hidden defects; Framing: placing the laminated components without hidden defects into a frame (202) filled with packaging material, and then installing the cover plate (201); Installing the junction box (205): installing the junction box (205) on one side of the lower cover plate (203), and connecting the electrical connector (204) led out from the battery cell to the junction box (205) to form a panel structure; Install the qualified panel structure and support structure to make a photovoltaic module containing TOPCon cells; The preparation method of TOPCon battery comprises the following steps: Choose silicon wafer as substrate and make double-sided texture; Diffusion of boron is performed on the front side of the silicon wafer to form a boron diffusion layer; Remove the BSG layer on the back and sides of the silicon wafer and perform alkaline polishing on the back of the silicon wafer; Depositing at least two sets of oxide layers and polysilicon layers on the back side of the silicon wafer; Phosphorus doping is performed on the back of the silicon wafer to form N + -Poly layer, and forming a PSG layer on the outer layer; Remove the PSG layer on the front and side of the silicon wafer; A mask layer is formed in the gate line region on the back side of the silicon wafer; Remove the outer N layer on the back of the silicon wafer without mask protection + -Poly layer, remove the excess Poly layer on the front and side of the silicon wafer; then remove the PSG, back mask layer and PSG layer in the non-mask area on the back; A passivation layer, a front anti-reflection layer, and a back anti-reflection layer are formed on the silicon wafer; Screen printing and sintering are performed on the front and back sides of the silicon wafer to form a front electrode and a back electrode, wherein the position of the back electrode corresponds to the position of the patterned mask; The outer layer Poly processing method of TOPCon battery includes the following steps: A protective layer is formed in the gate line area of the silicon wafer, and the protective layer is used to protect the outer N layer corresponding to the gate line area. + -Poly layer is protected from removal; Then remove the outer N layer without protection layer in the non-gate line area + -Poly layer, so that the N of the gate line area corresponding to the back electrode of the TOPCon battery (100) + -Poly layer thickness is greater than N in non-gate line area + -Poly layer thickness; Among them, the N of the gate line area corresponding to the back electrode + -The thickness of the protruding part of the Poly layer is N + -0.5-5 times the thickness of the Poly layer, and the outer N layer in the non-gate line area + -Poly layer thickness is 10-20nm; Use a low-pressure high-temperature diffusion furnace to diffuse boron on the front side of the silicon wafer. The diffusion temperature is 800-1100°C and the diffusion time is 10-50 minutes. After diffusion, the square resistance of the boron diffusion layer is 100-260Ω / sq, the junction depth is 0.1-0.4 microns, and the thickness of the BSG layer is 100-160 nanometers. Phosphorus doping concentration ranges from 0.1-2E21cm -3 .
2. The photovoltaic module containing TOPCon cells according to claim 1, characterized in that: Remove the outer N layer without protection layer in the non-gate line area by alkali solution + -Poly layer.
3. The photovoltaic module containing TOPCon cells according to claim 1, characterized in that: The protective layer is a mask layer which does not react with alkali solution and can be removed by acid solution.
4. The photovoltaic module containing TOPCon cells according to claim 3, characterized in that: When making the mask layer, first apply a layer of Si-containing slurry on the gate line area on the back of the silicon wafer, and then dry it at high temperature to form a SiO2 mask layer in the gate line area of the silicon wafer.
5. The method for preparing a photovoltaic module containing TOPCon cells according to claim 4, characterized in that: The thickness of the Si-containing slurry applied is 100-1000 nm.
6. The photovoltaic module containing TOPCon cells according to claim 4, characterized in that: A hollow pattern corresponding to the position of the screen-printed back gate line pattern is made on the mask plate. After preparing the Si-containing slurry, the slurry is roller-coated onto the mask plate so that the slurry adheres to the back gate line area of the silicon wafer through the hollow pattern. Then, the temperature is set at 300-700℃ in a chain heating furnace for drying.
7. The photovoltaic module containing TOPCon cells according to claim 1, characterized in that: The silicon wafer used as the substrate is an N-type single crystal silicon wafer with a thickness of 100-160 microns and a resistivity of 0.4-10Ω·cm.
8. The photovoltaic module containing TOPCon cells according to claim 1, characterized in that: The method for preparing a photovoltaic module containing TOPCon cells according to claim 1 is characterized in that at least two groups of oxide layers and polysilicon layers are deposited on the back of an N-type single crystal silicon wafer using LPCVD equipment.
9. The photovoltaic module containing TOPCon cells according to claim 8, characterized in that: There are two groups of oxide layers and polysilicon layers, including a first SiO2 layer, a first Poly layer, a second SiO2 layer, and a second Poly layer which are stacked in sequence from the inner layer to the outer layer.
10. The photovoltaic module containing TOPCon cells according to claim 9, characterized in that: The thickness of the first SiO2 layer is 1-2 nm, the thickness of the first Poly layer is 20-40 nm, the thickness of the second SiO2 layer is 0.5-2 nm, and the thickness of the second Poly layer is 30-150 nm.
11. The photovoltaic module containing TOPCon cells according to claim 1, characterized in that: Use HF to remove the PSG layer on the front and side of the silicon wafer; Use alkaline solution to remove the excess Poly layer on the front and sides of the silicon wafer, and the outer N layer on the back without mask layer protection + -Poly layer; use acid to remove the PSG in the non-mask area on the back, the back mask layer and the PSG layer here.