A pure vegetable oil-based polyol and preparation method thereof

By using glycerin as a ring-opening agent and solid acid catalyst SO42-/ZrO2, the problems of low product hydroxyl value and waste liquid pollution in the preparation of vegetable oil-based polyols in the existing technology are solved, and efficient and environmentally friendly polyol preparation is achieved, which is suitable for As a raw material for polyurethane.

CN117946382BActive Publication Date: 2024-10-18LINYI SIKERUI POLYURETHANE MATERIALS CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202410097439.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-24
Publication Date
2024-10-18
Estimated Expiration
2044-01-24

AI Technical Summary

Technical Problem

In existing vegetable oil-based polyol preparation methods, water or small molecular alcohols are commonly used as ring-opening agents, resulting in a low hydroxyl value of the product, and the use of inorganic acid catalysts can easily produce a large amount of waste acid and waste liquid to pollute the environment.

Method used

Glycerol is used as a ring-opening agent, combined with the solid acid catalyst SO42-/ZrO2, and epoxy vegetable oil is prepared and dried to simplify catalyst separation and reduce waste liquid production.

Benefits of technology

The hydroxyl value and viscosity of the polyol are increased, making it suitable as a raw material for polyurethane, reducing production costs, avoiding waste acid and waste liquid pollution, and simplifying process treatment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117946382B_ABST
    Figure CN117946382B_ABST
Patent Text Reader

Abstract

The invention discloses a pure vegetable oil-based polyol and a preparation method thereof, and relates to the technical field of polyols. The polyol comprises the following raw materials in parts by weight: 20-40 parts by weight of vegetable oil, 25-40 parts by weight of hydrogen peroxide, 0.2-0.5 parts by weight of a strongly acidic ion exchange resin, 10-12 parts by weight of formic acid, 30-50 parts by weight of glycerol, 0.3-0.6 parts by weight of a catalyst, and 50-80 parts by weight of n-hexane. The invention adopts glycerol as a ring-opening agent, and glycerol is a byproduct of biodiesel, so that not only the raw material source is wide, but also the obtained polyol has a high hydroxyl value and a moderate viscosity, which is more conducive to being used as a raw material for synthesizing polyurethane in a one-step method, and by using a solid acid catalyst SO4 2‑ / ZrO2, during the preparation process, the catalyst is separated from the reaction product by simple filtration, which simplifies the product post-treatment process, reduces the production cost, and avoids the generation of a large amount of waste acid and waste liquid to pollute the environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyols, in particular to a pure vegetable oil-based polyol and a preparation method thereof. Background Art

[0002] Oligomer polyols are a very important chemical intermediate, especially widely used in polyurethane synthesis. At present, oligomer polyols are mainly derived from fossil resources such as petroleum. Fossil resources such as petroleum are limited and non-renewable. Using natural renewable resources as substitutes has become a mainstream trend. The unit structure of vegetable oil is triglycerides composed of various saturated and unsaturated fatty acids and glycerol. It contains rich functional groups and is easy to modify. The modified compounds are expected to become ideal raw materials to replace petroleum resources. In addition, vegetable oil chemical raw materials have the advantages of being naturally renewable, biodegradable, and more environmentally friendly, and are widely used.

[0003] However, in the prior art, the preparation of vegetable oil-based polyols usually adopts the epoxy ring-opening method, in which the commonly used ring-opening agent is water or a small molecule alcohol, such as methanol, and the hydroxyl value of the obtained product is relatively low. The commonly used catalyst is an inorganic acid. Although the ring-opening conversion rate is high, it is easy to produce a large amount of waste acid and waste liquid to pollute the environment. Summary of the invention

[0004] The purpose of the present invention is to provide a pure vegetable oil-based polyol and a preparation method thereof, so as to solve the problem that the preparation of vegetable oil-based polyols currently proposed in the above-mentioned background technology usually adopts the epoxy ring-opening method, wherein the commonly used ring-opening agent is water or a small molecule alcohol, such as methanol, and the hydroxyl value of the obtained product is low. The commonly used catalyst is an inorganic acid. Although the ring-opening conversion rate is high, it is easy to produce a large amount of waste acid and waste liquid to pollute the environment.

[0005] To achieve the above object, the present invention provides the following technical solution: a pure vegetable oil-based polyol, comprising the following raw materials in parts by weight: 20-40 parts by weight of vegetable oil, 25-40 parts by weight of hydrogen peroxide, 0.2-0.5 parts by weight of strongly acidic ion exchange resin, 10-12 parts by weight of formic acid, 30-50 parts by weight of glycerol, 0.3-0.6 parts by weight of a catalyst and 50-80 parts by weight of n-hexane.

[0006] Preferably, the vegetable oil is selected from one or more of soybean oil, linseed oil, castor oil, rice bran oil, rapeseed oil, olive oil, sesame oil, cottonseed oil and palm oil.

[0007] Preferably, the catalyst is a solid acid catalyst SO4 2- / ZrO2.

[0008] A method for preparing pure vegetable oil-based polyols comprises the following steps:

[0009] S1. preparing epoxidized vegetable oil using vegetable oil, hydrogen peroxide, strongly acidic ion exchange resin and formic acid;

[0010] S2, quantitatively weigh epoxidized vegetable oil, n-hexane, glycerol and catalyst into a reactor, heat to 100°C and continue stirring for reaction for 2 hours;

[0011] S3, after the reaction is completed, the catalyst is separated by filtration, and then deionized water is added to the reaction solution for repeated washing until no glycerol is detected in the lower layer solution, and then the solvent n-hexane is removed by vacuum rotary evaporation to obtain a mixed solution;

[0012] S4, drying the mixed solution in the previous step to obtain pure vegetable oil-based polyol;

[0013] S5. Collect and seal the prepared pure vegetable oil-based polyols for storage.

[0014] Preferably, in step S1, the preparation of epoxidized vegetable oil comprises the following steps:

[0015] S11, taking a certain amount of vegetable oil and a strong acid ion exchange resin and putting them into a reactor, then weighing a certain amount of hydrogen peroxide and formic acid and mixing them and adding them into the reactor, and mechanically stirring at 80° C. for 6 hours and then stopping the reaction;

[0016] S12, after separating the catalyst, washing the oil phase with a large amount of saturated sodium chloride solution until it becomes neutral;

[0017] S13, finally, the treated solution is subjected to vacuum rotary evaporation at 80° C. to obtain epoxidized vegetable oil;

[0018] S14, collecting the prepared epoxidized vegetable oil.

[0019] Preferably, the stirring is carried out by combining mechanical stirring with ultrasonic stirring.

[0020] Preferably, in step S3, the process of filtering and separating the catalyst is: cooling the post-reaction solution to room temperature, then filtering and separating the solution using a filter to remove the catalyst and solid impurities, and collecting the filtered solution.

[0021] Preferably, in step S3, the glycerol is detected using a copper sulfate solution, and the detection process is as follows: a certain amount of sample is taken from the repeatedly washed reaction solution, the sample is added to the copper sulfate solution and the color change is observed; if the sample contains glycerol, it reacts with the copper sulfate, causing the color of the solution to change to green or dark blue.

[0022] Preferably, in step S4, the drying is carried out under vacuum, using far-infrared radiation and near-infrared radiation to dry the mixed solution simultaneously;

[0023] The far-infrared radiation source and the near-infrared radiation source are respectively located on the upper and lower sides of the mixed product, and radiate alternately toward the mixed product at the same time:

[0024] The wavelength of the far-infrared radiation is 20-23 μm, the distance between the radiation source of the far-infrared radiation and the mixed product is 15-17 cm, and the temperature of the radiation source of the far-infrared radiation is 130-180° C.;

[0025] The wavelength of the near infrared radiation is 1.4-2.0 μm, the distance between the radiation source of the near infrared radiation and the mixed product is 12-14 cm, and the temperature of the radiation source of the near infrared radiation is 90-130° C.;

[0026] The alternating radiation refers to irradiating the mixed product by alternating far-infrared radiation and near-infrared radiation at an exchange frequency of 12 minutes per time, and the first radiation is far-infrared radiation.

[0027] Preferably, the drying treatment time is 100-130 minutes.

[0028] Compared with the prior art, the present invention has the following beneficial effects:

[0029] In the present invention, glycerol is used as a ring-opening agent. Glycerol is a byproduct of biodiesel. Not only is the raw material source extensive, but the obtained polyol has a high hydroxyl value and moderate viscosity, which is more conducive to being used as a raw material for the one-step synthesis of polyurethane. By using a solid acid catalyst SO4 2- / ZrO2, during the preparation process, the catalyst is separated from the reaction product by simple filtration, which simplifies the product post-treatment process, reduces the production cost, and avoids the generation of a large amount of waste acid and waste liquid to pollute the environment. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a flow chart of a method for preparing pure vegetable oil-based polyols according to the present invention;

[0031] Figure 2 It is a statistical diagram of the ring-opening conversion rate in the present invention. DETAILED DESCRIPTION

[0032] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the implementation regulations described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0033] The present invention will be further described below in conjunction with the embodiments.

[0034] Example 1

[0035] This embodiment provides a pure vegetable oil-based polyol, comprising the following raw materials in parts by weight: 20 parts by weight of vegetable oil, 25 parts by weight of hydrogen peroxide, 0.3 parts by weight of a strongly acidic ion exchange resin, 10 parts by weight of formic acid, 30 parts by weight of glycerol, 0.3 parts by weight of a catalyst, and 50 parts by weight of n-hexane;

[0036] Wherein, the vegetable oil is soybean oil;

[0037] The catalyst is a solid acid catalyst SO4 2- / ZrO2;

[0038] A method for preparing pure vegetable oil-based polyols comprises the following steps:

[0039] Ⅰ. Preparation of epoxidized vegetable oil using vegetable oil, hydrogen peroxide, strongly acidic ion exchange resin and formic acid;

[0040] Wherein, the preparation of epoxidized vegetable oil comprises the following steps:

[0041] 11) A certain amount of vegetable oil and a strong acid ion exchange resin are put into a reactor, and then a certain amount of hydrogen peroxide and formic acid are weighed and mixed and added into the reactor, and the reaction is stopped after mechanical stirring at 80° C. for 6 hours;

[0042] 12) After separating the catalyst, wash the oil phase with a large amount of saturated sodium chloride solution until it becomes neutral;

[0043] 13) finally, the treated solution is subjected to vacuum rotary evaporation at 80° C. to obtain epoxidized vegetable oil;

[0044] 14) Collecting the prepared epoxidized vegetable oil.

[0045] Ⅱ. Quantitatively weigh epoxidized vegetable oil, n-hexane, glycerin and catalyst into a reactor, heat to 100°C and continue stirring for 2 hours; wherein, the stirring method is a combination of mechanical stirring and ultrasonic stirring.

[0046] III. After the reaction is completed, the catalyst is separated by filtration, and then deionized water is added to the reaction solution for repeated washing until no glycerol is detected in the lower layer solution, and then the solvent n-hexane is removed by vacuum rotary evaporation to obtain a mixed solution;

[0047] The process of filtering and separating the catalyst is as follows: cooling the post-reaction solution to room temperature, then filtering and separating the solution using a filter to remove the catalyst and solid impurities, and collecting the filtered solution.

[0048] Among them, the detection of glycerol is carried out using copper sulfate solution, and the detection process is: take a certain amount of sample from the repeatedly washed reaction solution, add the obtained sample to the copper sulfate solution to observe the color change, if the sample contains glycerol, it will react with copper sulfate, causing the color of the solution to change to green or dark blue.

[0049] IV. Drying the mixed solution in the previous step to obtain pure vegetable oil-based polyol;

[0050] The drying process is carried out under vacuum, using far infrared radiation and near infrared radiation to dry the mixed solution; the drying process time is 110 minutes;

[0051] The far-infrared radiation source and the near-infrared radiation source are respectively located on the upper and lower sides of the mixed product, and radiate alternately toward the mixed product at the same time:

[0052] The wavelength of the far-infrared radiation is 20 μm, the distance between the radiation source of the far-infrared radiation and the mixed product is 15 cm, and the temperature of the radiation source of the far-infrared radiation is 130° C.;

[0053] The wavelength of the near-infrared radiation is 1.4 μm, the distance between the radiation source of the near-infrared radiation and the mixed product is 12 cm, and the temperature of the radiation source of the near-infrared radiation is 90° C.;

[0054] The alternating radiation refers to irradiating the mixed product by alternating far-infrared radiation and near-infrared radiation at an exchange frequency of 12 minutes per time, and the first radiation is far-infrared radiation.

[0055] V. Collect and seal the prepared pure vegetable oil-based polyol.

[0056] Example 2

[0057] This embodiment provides a pure vegetable oil-based polyol, comprising the following raw materials in parts by weight: 30 parts by weight of vegetable oil, 32 parts by weight of hydrogen peroxide, 0.5 parts by weight of a strongly acidic ion exchange resin, 11 parts by weight of formic acid, 40 parts by weight of glycerol, 0.4 parts by weight of a catalyst, and 65 parts by weight of n-hexane;

[0058] Wherein, the vegetable oil is soybean oil;

[0059] The catalyst is a solid acid catalyst SO4 2- / ZrO2;

[0060] A method for preparing pure vegetable oil-based polyols comprises the following steps:

[0061] Ⅰ. Preparation of epoxidized vegetable oil using vegetable oil, hydrogen peroxide, strongly acidic ion exchange resin and formic acid;

[0062] Wherein, the preparation of epoxidized vegetable oil comprises the following steps:

[0063] 11) A certain amount of vegetable oil and a strong acid ion exchange resin are put into a reactor, and then a certain amount of hydrogen peroxide and formic acid are weighed and mixed and added into the reactor, and the reaction is stopped after mechanical stirring at 80° C. for 6 hours;

[0064] 12) After separating the catalyst, wash the oil phase with a large amount of saturated sodium chloride solution until it becomes neutral;

[0065] 13) finally, the treated solution is subjected to vacuum rotary evaporation at 80° C. to obtain epoxidized vegetable oil;

[0066] 14) Collecting the prepared epoxidized vegetable oil.

[0067] Ⅱ. Quantitatively weigh epoxidized vegetable oil, n-hexane, glycerol and catalyst into a reactor, heat to 80°C and continue stirring for 2 hours; wherein, the stirring method is a combination of mechanical stirring and ultrasonic stirring.

[0068] III. After the reaction is completed, the catalyst is separated by filtration, and then deionized water is added to the reaction solution for repeated washing until no glycerol is detected in the lower layer solution, and then the solvent n-hexane is removed by vacuum rotary evaporation to obtain a mixed solution;

[0069] The process of filtering and separating the catalyst is as follows: cooling the post-reaction solution to room temperature, then filtering and separating the solution using a filter to remove the catalyst and solid impurities, and collecting the filtered solution.

[0070] Among them, the detection of glycerol is carried out using copper sulfate solution, and the detection process is: take a certain amount of sample from the repeatedly washed reaction solution, add the obtained sample to the copper sulfate solution to observe the color change, if the sample contains glycerol, it will react with copper sulfate, causing the color of the solution to change to green or dark blue.

[0071] IV. Drying the mixed solution in the previous step to obtain pure vegetable oil-based polyol;

[0072] The drying process is carried out under vacuum, using far infrared radiation and near infrared radiation to dry the mixed solution; the drying process time is 110 minutes;

[0073] The far-infrared radiation source and the near-infrared radiation source are respectively located on the upper and lower sides of the mixed product, and radiate alternately toward the mixed product at the same time:

[0074] The wavelength of the far-infrared radiation is 20 μm, the distance between the radiation source of the far-infrared radiation and the mixed product is 15 cm, and the temperature of the radiation source of the far-infrared radiation is 130° C.;

[0075] The wavelength of the near-infrared radiation is 1.4 μm, the distance between the radiation source of the near-infrared radiation and the mixed product is 12 cm, and the temperature of the radiation source of the near-infrared radiation is 90° C.;

[0076] The alternating radiation refers to irradiating the mixed product by alternating far-infrared radiation and near-infrared radiation at an exchange frequency of 12 minutes per time, and the first radiation is far-infrared radiation.

[0077] V. Collect and seal the prepared pure vegetable oil-based polyol.

[0078] Example 3

[0079] This embodiment provides a pure vegetable oil-based polyol, comprising the following raw materials in parts by weight: 40 parts by weight of vegetable oil, 40 parts by weight of hydrogen peroxide, 0.5 parts by weight of a strongly acidic ion exchange resin, 12 parts by weight of formic acid, 50 parts by weight of glycerol, 0.6 parts by weight of a catalyst, and 80 parts by weight of n-hexane;

[0080] Wherein, the vegetable oil is soybean oil;

[0081] The catalyst is a solid acid catalyst SO4 2- / ZrO2;

[0082] A method for preparing pure vegetable oil-based polyols comprises the following steps:

[0083] Ⅰ. Preparation of epoxidized vegetable oil using vegetable oil, hydrogen peroxide, strongly acidic ion exchange resin and formic acid;

[0084] Wherein, the preparation of epoxidized vegetable oil comprises the following steps:

[0085] 11) A certain amount of vegetable oil and a strong acid ion exchange resin are put into a reactor, and then a certain amount of hydrogen peroxide and formic acid are weighed and mixed and added into the reactor, and the reaction is stopped after mechanical stirring at 80° C. for 6 hours;

[0086] 12) After separating the catalyst, wash the oil phase with a large amount of saturated sodium chloride solution until it becomes neutral;

[0087] 13) finally, the treated solution is subjected to vacuum rotary evaporation at 80° C. to obtain epoxidized vegetable oil;

[0088] 14) Collecting the prepared epoxidized vegetable oil.

[0089] Ⅱ. Quantitatively weigh epoxidized vegetable oil, n-hexane, glycerol and catalyst into a reactor, heat to 100°C and continue stirring to react for 3 hours; wherein, the stirring method is a combination of mechanical stirring and ultrasonic stirring.

[0090] III. After the reaction is completed, the catalyst is separated by filtration, and then deionized water is added to the reaction solution for repeated washing until no glycerol is detected in the lower layer solution, and then the solvent n-hexane is removed by vacuum rotary evaporation to obtain a mixed solution;

[0091] The process of filtering and separating the catalyst is as follows: cooling the post-reaction solution to room temperature, then filtering and separating the solution using a filter to remove the catalyst and solid impurities, and collecting the filtered solution.

[0092] Among them, the detection of glycerol is carried out using copper sulfate solution, and the detection process is: take a certain amount of sample from the repeatedly washed reaction solution, add the obtained sample to the copper sulfate solution to observe the color change, if the sample contains glycerol, it will react with copper sulfate, causing the color of the solution to change to green or dark blue.

[0093] IV. Drying the mixed solution in the previous step to obtain pure vegetable oil-based polyol;

[0094] The drying process is carried out under vacuum, using far infrared radiation and near infrared radiation to dry the mixed solution; the drying process time is 110 minutes;

[0095] The far-infrared radiation source and the near-infrared radiation source are respectively located on the upper and lower sides of the mixed product, and radiate alternately toward the mixed product at the same time:

[0096] The wavelength of the far-infrared radiation is 20 μm, the distance between the radiation source of the far-infrared radiation and the mixed product is 15 cm, and the temperature of the radiation source of the far-infrared radiation is 130° C.;

[0097] The wavelength of the near-infrared radiation is 1.4 μm, the distance between the radiation source of the near-infrared radiation and the mixed product is 12 cm, and the temperature of the radiation source of the near-infrared radiation is 90° C.;

[0098] The alternating radiation refers to irradiating the mixed product by alternating far-infrared radiation and near-infrared radiation at an exchange frequency of 12 minutes per time, and the first radiation is far-infrared radiation.

[0099] V. Collect and seal the prepared pure vegetable oil-based polyol.

[0100] Example 4

[0101] The pure vegetable oil-based polyol and the preparation method thereof provided in this embodiment are substantially the same as those in Example 1, the main difference being that glycerol is replaced by methanol.

[0102] Test and result analysis:

[0103] The pure vegetable oil-based polyols prepared by Examples 1-3 are respectively recorded as Experimental Examples 1-3; the pure vegetable oil-based polyols prepared by Example 4 are used as a comparative example; the performance of the pure vegetable oil-based polyols is tested and the relevant data are recorded in Table 1;

[0104] Table 1: Test data record table

[0105]

[0106] It can be seen from Table 1 that, compared with the comparative example, the pure vegetable oil-based polyols prepared in Examples 1-3 can significantly improve the ring-opening conversion rate, the product hydroxyl value is as high as 365 mgKOH / g, and the viscosity is good at room temperature. The pure vegetable oil-based polyols prepared in Examples 1-3 have good thermal stability, moderate viscosity, and high reaction activity.

[0107] In the pure vegetable oil-based polyol prepared by the present invention, glycerol is used as a ring-opening agent. Glycerol is a byproduct of biodiesel. Not only is the raw material source extensive, but also the hydroxyl value of the polyol obtained by using methanol is high and the viscosity is moderate. It is more conducive to being used as a raw material for the one-step synthesis of polyurethane. By using a solid acid catalyst SO4 2- / ZrO2, during the preparation process, the catalyst is separated from the reaction product by simple filtration, which simplifies the product post-treatment process, reduces the production cost, and avoids the generation of a large amount of waste acid and waste liquid to pollute the environment.

[0108] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A pure vegetable oil-based polyol, characterized in that: The invention comprises the following raw materials in parts by weight: 20-40 parts by weight of vegetable oil, 25-40 parts by weight of hydrogen peroxide, 0.2-0.5 parts by weight of strongly acidic ion exchange resin, 10-12 parts by weight of formic acid, 30-50 parts by weight of glycerol, 0.3-0.6 parts by weight of a catalyst and 50-80 parts by weight of n-hexane; The vegetable oil is selected from one or more of soybean oil, linseed oil, castor oil, rice bran oil, rapeseed oil, olive oil, sesame oil, cottonseed oil and palm oil; The catalyst is a solid acid catalyst SO4 2- / ZrO2.

2. A method for preparing the pure vegetable oil-based polyol according to claim 1, characterized in that: The following steps are involved: S1. Preparing epoxidized vegetable oil using vegetable oil, hydrogen peroxide, strongly acidic ion exchange resin and formic acid, wherein the preparation of epoxidized vegetable oil comprises the following steps: S11, taking a certain amount of vegetable oil and a strong acid ion exchange resin and putting them into a reactor, then weighing a certain amount of hydrogen peroxide and formic acid and mixing them and adding them into the reactor, and mechanically stirring at 80° C. for 6 hours and then stopping the reaction; S12, after separating the catalyst, washing the oil phase with a large amount of saturated sodium chloride solution until it becomes neutral; S13, finally, the treated solution is subjected to vacuum rotary evaporation at 80° C. to obtain epoxidized vegetable oil; S14, collecting the prepared epoxidized vegetable oil; S2, putting the epoxidized vegetable oil, n-hexane, glycerol and catalyst obtained in the previous step into a reaction kettle, heating to 100° C. and stirring continuously for 2 h; S3, after the reaction is completed, the catalyst is separated by filtration, and then deionized water is added to the reaction solution for repeated washing until no glycerol is detected in the lower layer solution, and then the solvent n-hexane is removed by vacuum rotary evaporation to obtain a mixed solution; S4, drying the mixed solution in the previous step to obtain pure vegetable oil-based polyol; S5. Collect and seal the prepared pure vegetable oil-based polyols for storage.

3. The method for preparing a pure vegetable oil-based polyol according to claim 2, characterized in that: In step S2, the stirring is carried out by combining mechanical stirring with ultrasonic stirring.

4. The method for preparing a pure vegetable oil-based polyol according to claim 2, characterized in that: In step S3, the process of filtering and separating the catalyst is as follows: cooling the post-reaction solution to room temperature, then filtering and separating the solution using a filter to remove the catalyst and solid impurities, and collecting the filtered solution.

5. The method for preparing a pure vegetable oil-based polyol according to claim 2, characterized in that: In step S3, the glycerol is detected using a copper sulfate solution, and the detection process is as follows: a certain amount of sample is taken from the repeatedly washed reaction solution, the sample is added to the copper sulfate solution to observe the color change, if the sample contains glycerol, it will react with the copper sulfate, causing the color of the solution to change to green or dark blue.

6. The method for preparing a pure vegetable oil-based polyol according to claim 2, characterized in that: In step S4, the drying is performed under vacuum by using far-infrared radiation and near-infrared radiation to dry the mixed solution; The far-infrared radiation source and the near-infrared radiation source are respectively located at the upper and lower sides of the mixed solution, and radiate alternately toward the mixed solution: The wavelength of the far-infrared radiation is 20-23 μm, the distance between the radiation source of the far-infrared radiation and the mixed product is 15-17 cm, and the temperature of the radiation source of the far-infrared radiation is 130-180° C.; The wavelength of the near infrared radiation is 1.4-2.0 μm, the distance between the radiation source of the near infrared radiation and the mixed product is 12-14 cm, and the temperature of the radiation source of the near infrared radiation is 90-130° C.; The alternating radiation refers to irradiating the mixed product by alternating far-infrared radiation and near-infrared radiation at an exchange frequency of 12 minutes per time, and the first radiation is far-infrared radiation.

7. The method for preparing a pure vegetable oil-based polyol according to claim 6, characterized in that: The drying treatment time is 100-130 minutes.

Citation Information

Patent Citations

  • Preparation method and application of bio-based polyol

    CN116535314A