Methods for forming germanium-boron source and drain in FDSOI
By employing germanium-silicon epitaxial technology and a multilayer cap structure in FDSOI, and utilizing oxygen radical catalytic oxidation and P-type ion diffusion, the problem of difficulty in increasing Ge and B concentrations was solved, achieving high mobility and low resistance in the SiGe source/drain structure.
Patent Information
- Application Number
- CN202410114694.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-26
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-01-26
AI Technical Summary
In existing technologies, it is difficult to achieve high concentrations of Ge and B in the germanium-silicon epitaxial layer of FDSOI at the same time, which affects the device's ability to simultaneously meet the requirements of high mobility and low resistance.
A seed epitaxial layer is formed in the source/drain region using a germanium-silicon epitaxial process. Through a multilayer cap structure and annealing, the concentrations of Ge and B in the germanium-silicon host epitaxial layer and the seed epitaxial layer are gradually increased by utilizing oxygen free radical catalytic oxidation and P-type ion diffusion.
A SiGe source/drain structure with high Ge and P-type ion concentrations was achieved, and the device simultaneously meets the requirements of high mobility and low resistance.
Smart Images

Figure CN117954327B_ABST
Abstract
Description
Technical Field
[0001] This invention relates to the field of semiconductor technology, and in particular to a method for forming germanium-boron source and drain in FDSOI. Background Technology
[0002] Stress-channel transistors are widely studied in the integrated circuit industry. In FDSOI (fully depleted silicon-on-insulator), the raised SiGe technology can be used to further improve the carrier mobility of the channel, thereby improving the performance of the device, and thus continuously shrinking the size of the transistor to achieve larger-scale integration.
[0003] In FDSOI, an elevated SiGe source / drain structure is employed, with the epitaxial growth process as follows: First, a seed epitaxial layer with low Ge and P-type ion concentrations (e.g., B) is epitaxially grown to reduce lattice mismatch between the epitaxial layer and the substrate. Then, a germanium-silicon host epitaxial layer with higher Ge and B concentrations is epitaxially grown. The distribution of channel stress field and source / drain current field can be simultaneously controlled by adjusting the B and Ge concentrations in the germanium-silicon host epitaxial layer. Finally, Si:B is epitaxially grown as a cap layer, which is then deposited with NiPt and annealed to form a NiSi layer. However, during the epitaxial growth of the germanium-silicon host epitaxial layer, the increased GeH4 flux limits the reaction between B2H6 and the substrate, thus limiting the increase in B concentration in the epitaxial layer. It is difficult to simultaneously achieve high concentrations of Ge and B, ultimately affecting the device's ability to simultaneously meet the requirements of high mobility and low resistance.
[0004] To address the aforementioned issues, a novel method for forming germanium-boron source / drain in FDSOI is required. Summary of the Invention
[0005] In view of the shortcomings of the prior art described above, the purpose of this invention is to provide a method for forming germanium-boron source and drain in FDSOI, which solves the problem that the concentrations of Ge and P-type ions in the epitaxial layer are difficult to reach high concentrations at the same time in the prior art, ultimately affecting the device's ability to simultaneously meet the requirements of high mobility and low resistance.
[0006] To achieve the above and other related objectives, the present invention provides a method for forming a germanium-boron source / drain in an FDSOI, comprising:
[0007] Step 1: Provide a silicon-on-insulator substrate, which is composed of a silicon substrate, a buried oxide layer and a silicon layer stacked sequentially from bottom to top. A gate structure is formed on the silicon layer, and the two sides of the gate structure are source and drain regions.
[0008] Step 2: Using germanium-silicon epitaxial technology, a seed epitaxial layer is formed on the source and drain regions, and a germanium-silicon host epitaxial layer of the target thickness is formed on the seed epitaxial layer. Both the germanium-silicon seed epitaxial layer and the germanium-silicon host epitaxial layer are doped with P-type ions.
[0009] Step 3: Form a first cap layer on the main epitaxial layer. The first cap layer is a silicon layer doped with p-type ions. Form a second cap layer on the first cap layer. The second cap layer is a pure silicon layer.
[0010] Step 4: Form a first oxide layer with O radicals on the second cap layer. Annealing causes the silicon at the second cap layer to form a second oxide layer, and germanium ions diffuse downward to form germanium and silicon source / drain. Continue annealing to form a third oxide layer on the silicon at the first cap layer. P-type ions in the first cap layer diffuse downward to the main epitaxial layer and the seed epitaxial layer, so that the germanium ions and P-type ions in the main epitaxial layer and the seed epitaxial layer are at the target concentration.
[0011] Step 5: Remove the first to trioxide layers and form a third cap layer on the main epitaxial layer.
[0012] Preferably, the silicon-on-insulator substrate in step one is composed of a silicon substrate, a buried oxide layer, and a silicon layer stacked sequentially from bottom to top.
[0013] Preferably, the germanium concentration in the germanium-silicon host epitaxial layer in step two is 20% to 45%.
[0014] Preferably, the P-type ions in steps two and three are B-type ions.
[0015] Preferably, the total thickness of the first and second cap layers in step three is 100 to 200 angstroms.
[0016] Preferably, the first cap layer in step three is doped with B ions ranging from 2e20 to 1e21cm-3.
[0017] Preferably, the material of the first oxide layer in step four is La2O3.
[0018] Preferably, the first oxide layer is formed in step four using atomic layer deposition.
[0019] Preferably, the thickness of the first oxide layer in step four is 1 to 10 nanometers.
[0020] Preferably, the annealing in step four is carried out in an oxygen partial pressure annealing environment at a temperature of 900 to 1000 degrees Celsius.
[0021] Preferably, in step five, the first to third oxide layers are removed using a surface pre-cleaning process.
[0022] As described above, the method for forming germanium-boron source / drain in FDSOI of the present invention has the following beneficial effects:
[0023] This invention enables the fabrication of SiGe source-drain uplift structures with high Ge and P-type ion (e.g., B) concentrations, allowing the device to simultaneously meet the requirements of high mobility and low resistance. Attached Figure Description
[0024] Figure 1 The diagram shown is a schematic representation of the process flow of the present invention.
[0025] Figure 2 The diagram shown illustrates the formation of the gate structure according to the present invention.
[0026] Figure 3 The diagram shown illustrates the formation of the seed epitaxial layer according to the present invention.
[0027] Figure 4 The diagram shown illustrates the formation of the germanium-silicon epitaxial layer according to the present invention.
[0028] Figure 5 The diagram shows the formation of the first and second cap layers according to the present invention.
[0029] Figure 6 The diagram shown illustrates the formation of the first oxide layer according to the present invention.
[0030] Figure 7 This is a schematic diagram of the first stage of annealing according to the present invention;
[0031] Figure 8 This is a schematic diagram of the second stage of annealing in this invention;
[0032] Figure 9 The diagram shown illustrates the removal of the first to third oxide layers according to the present invention. Detailed Implementation
[0033] The following specific examples illustrate the implementation of the present invention. Those skilled in the art can easily understand other advantages and effects of the present invention from the content disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and various details in this specification can also be modified or changed based on different viewpoints and applications without departing from the spirit of the present invention.
[0034] Please see Figure 1 This invention provides a method for forming a germanium-boron source / drain in an FDSOI, comprising:
[0035] Step 1, please refer to Figure 2 A silicon-on-insulator substrate is provided, which is composed of a silicon substrate 101, a buried oxide layer 102 and a silicon layer 103 stacked sequentially from bottom to top. A gate structure 104 is formed on the silicon layer 103, and the two sides of the gate structure 104 are source and drain regions.
[0036] The gate structure 104 may consist of a gate dielectric layer and a gate layer; a protective layer may be formed on the outer surface of the gate dielectric layer and the gate layer, and the material of the protective layer may be an oxide or a nitride.
[0037] The gate dielectric layer 103 includes an interface layer (e.g., silicon oxide layer 103) and / or a high-k gate dielectric layer above the interface layer. The high-k gate dielectric includes a dielectric material having a high dielectric constant, for example, greater than the dielectric constant of thermally heated silicon oxide (~3.9).
[0038] In some embodiments, the silicon-on-insulator substrate in step one consists of a silicon substrate 101, a buried oxide layer 102, and a silicon layer 103 stacked sequentially from bottom to top.
[0039] Step 2: Using germanium-silicon epitaxial technology, a seed epitaxial layer 105 is formed on the source and drain regions, forming a structure as shown in the figure. Figure 3 The structure shown depicts a germanium-silicon host epitaxial layer 106 of the target thickness formed on the seed epitaxial layer 105, forming a structure as shown. Figure 4 The structure shown has a germanium-silicon seed epitaxial layer 105 and a germanium-silicon main epitaxial layer 106 both doped with P-type ions.
[0040] In some embodiments, the P-type ion in step two is a boron (B) ion, but other types of P-type ions may also be selected according to the actual process.
[0041] Step 3: A first cap layer 107 is formed on the main epitaxial layer. The first cap layer 107 is a silicon layer 103 doped with p-type ions. A second cap layer 108 is formed on the first cap layer 107. The second cap layer 108 is a pure silicon layer 103, forming a structure as shown in the figure. Figure 5 The structure shown;
[0042] In some embodiments, the P-type ion in step three is a B-type ion, but other types of P-type ions can also be selected according to the actual process.
[0043] In some embodiments, the total thickness of the first and second cap layers in step three is 100 to 200 angstroms.
[0044] In some embodiments, the first cap layer 107 in step three is doped with B ions ranging from 2e20 to 1e21cm-3.
[0045] Step 4: Form a first oxide layer 109 containing O free radicals on the second cap layer 108, forming a structure as shown in the figure. Figure 6 Please refer to the structure shown. Figure 7Annealing causes the silicon at the second cap layer 108 to form the second oxide layer 110, and germanium ions diffuse downwards to form germanium and silicon source / drain. Specifically, under the catalytic oxidation of the special O radicals in the first oxide layer 109, the Si at the first oxide layer 109 / Si is rapidly oxidized to SiO2. Simultaneously, Ge aggregation occurs at the SiO2 / SiGe interface, and the Ge at the interface diffuses into the lower SiGe / Si layer, forming SiGe source / drain. Compared to direct thermal oxidation of Si, this method increases the oxidation rate by 10 times, significantly shortening the oxidation time. Simultaneously, the oxidation temperature is reduced, for example, from a high temperature of 1050 degrees Celsius to 900-1000 degrees Celsius in this example, thereby reducing the thermal budget during SiGe channel fabrication, minimizing the reflow effect of the SiGe layer, and protecting the unaggregated SiGe structure below the interface during Ge aggregation. After thermal oxidation, silicon forms a dense SiO2 film, which acts as a masking film for P-type ion diffusion.
[0046] Please see Figure 8 Continued annealing causes the silicon at the first cap layer 107 to form a third oxide layer. P-type ions in the first cap layer 107 diffuse downwards into the host epitaxial layer and the seed epitaxial layer 105, resulting in target concentrations of germanium ions and P-type ions in both layers. That is, during continuous thermal oxidation, the Si in the first cap layer 107 is oxidized to SiO2, while P-type ions continuously diffuse into the germanium-silicon host epitaxial layer 106 and the germanium-silicon seed epitaxial layer 105. In the germanium-silicon host epitaxial layer 106, Si is continuously consumed. Ge, due to its lower binding affinity to O and its smaller atomic size preventing it from penetrating SiO2, can only diffuse downwards. The buried oxide layer 102 of the SOI structure acts as a natural barrier for Ge and P-type ions. The entire process continuously increases the concentrations of Ge and P-type ions in the source and drain regions.
[0047] In some embodiments, the material of the first oxide layer 109 in step four is La2O3. La2O3 can typically be formed using atomic layer deposition, but other materials capable of catalyzing the formation of silicon dioxide can also be selected here.
[0048] In some embodiments, the thickness of the first oxide layer 109 in step four is 1 to 10 nanometers.
[0049] In some embodiments, the annealing in step four is carried out in an oxygen partial pressure annealing environment at a temperature of 900 to 1000 degrees Celsius.
[0050] Step 5: Remove the first to third oxide layers to form a layer like... Figure 9 The structure shown has a third cap layer formed on the main epitaxial layer. The third cap layer can be doped with P-type ions, thereby creating a SiGe source-drain lift structure with high Ge and P-type ion concentrations, so that the device can simultaneously meet the requirements of high mobility and low resistance.
[0051] In some embodiments, step five utilizes a surface pre-cleaning process to remove the first to trioxide layers.
[0052] It should be noted that the illustrations provided in this embodiment are only schematic representations of the basic concept of the present invention. Therefore, the drawings only show the components related to the present invention and are not drawn according to the actual number, shape and size of the components in the actual implementation. In the actual implementation, the form, quantity and proportion of each component can be arbitrarily changed, and the layout of the components may also be more complex.
[0053] In summary, this invention enables the fabrication of SiGe source-drain uplift structures with high Ge and P-type ion (e.g., B) concentrations, allowing the device to simultaneously meet the requirements of high mobility and low resistance. Therefore, this invention effectively overcomes the various shortcomings of the prior art and has high industrial applicability.
[0054] The above embodiments are merely illustrative of the principles and effects of the present invention and are not intended to limit the invention. Any person skilled in the art can modify or alter the above embodiments without departing from the spirit and scope of the present invention. Therefore, all equivalent modifications or alterations made by those skilled in the art without departing from the spirit and technical concept disclosed in the present invention should still be covered by the claims of the present invention.
Claims
1. A method for forming a germanium-boron source / drain in an FDSOI, characterized in that, At least including: Step 1: Provide a silicon-on-insulator substrate, which is composed of a silicon substrate, a buried oxide layer and a silicon layer stacked sequentially from bottom to top. A gate structure is formed on the silicon layer, and the two sides of the gate structure are source and drain regions. Step 2: Using germanium-silicon epitaxial technology, a seed epitaxial layer is formed on the source and drain regions, and a germanium-silicon host epitaxial layer of the target thickness is formed on the seed epitaxial layer. Both the germanium-silicon seed epitaxial layer and the germanium-silicon host epitaxial layer are doped with P-type ions. Step 3: Form a first cap layer on the main epitaxial layer. The first cap layer is a silicon layer doped with p-type ions. Form a second cap layer on the first cap layer. The second cap layer is a pure silicon layer. Step 4: Form a first oxide layer with O radicals on the second cap layer, and anneal to form a second oxide layer with silicon at the second cap layer. Germanium ions diffuse downward to form germanium and silicon source / drain. Continue annealing to form a third oxide layer with silicon at the first cap layer. P-type ions in the first cap layer diffuse downward to the main epitaxial layer and the seed epitaxial layer, so that the germanium ions and P-type ions in the main epitaxial layer and the seed epitaxial layer are at the target concentration. Step 5: Remove the first to trioxide layers and form a third cap layer on the main epitaxial layer.
2. The method for forming germanium-boron source / drain in FDSOI according to claim 1, characterized in that: The germanium concentration in the germanium-silicon host epitaxial layer in step two is 20% to 45%.
3. The method for forming germanium-boron source / drain in FDSOI according to claim 1, characterized in that: The P-type ions mentioned in steps two and three are B ions.
4. The method for forming germanium-boron source / drain in FDSOI according to claim 1, characterized in that: The total thickness of the first and second cap layers in step three is 100 to 200 angstroms.
5. The method for forming germanium-boron source / drain in FDSOI according to claim 3, characterized in that: In step three, the first cap layer is doped with B ions ranging from 2e20 to 1e21cm-3.
6. The method for forming germanium-boron source / drain in FDSOI according to claim 1, characterized in that: The material of the first oxide layer in step four is La2O3.
7. The method for forming germanium-boron source / drain in FDSOI according to claim 6, characterized in that: In step four, the first oxide layer is formed using atomic layer deposition.
8. The method for forming germanium-boron source / drain in FDSOI according to claim 1, characterized in that: The thickness of the first oxide layer in step four is 1 to 10 nanometers.
9. The method for forming germanium-boron source / drain in FDSOI according to claim 1, characterized in that: The annealing in step four is carried out in an oxygen partial pressure annealing environment at a temperature of 900 to 1000 degrees Celsius.
10. The method for forming a germanium-boron source / drain in an FDSOI according to claim 1, characterized in that: In step five, the first to third oxide layers are removed using a surface pre-cleaning process.
Citation Information
Patent Citations
Manufacturing method of embedded germanium-silicon device and embedded germanium-silicon device structure