Preparation method of positive electrode composite material, positive electrode composite material and solid-state battery

By using silicon-carbon composite materials and cathode composite materials composed of asphalt, polyethylene glycol, polyethylene oxide and other components in solid-state batteries, the energy density and cycle stability of solid-state batteries are improved, and the problem of low cathode specific capacity is solved. , achieving a wider range of applications.

CN117976883BActive Publication Date: 2024-10-11广东瑞浦兰钧能源有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410208640.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-26
Publication Date
2024-10-11
Estimated Expiration
2044-02-26

AI Technical Summary

Technical Problem

The existing solid-state battery cathode has a low specific capacity, which limits the application range of solid-state batteries.

Method used

Silicon-carbon composite material is used as the cathode material, prepared by chemical vapor deposition method, and pitch, polyethylene glycol and polyethylene oxide are added to the silicon-carbon composite material for carbonization coating and doping to increase the specific capacity of the cathode and The cathode composite material is formed through hot press forming technology.

Benefits of technology

It significantly improves the energy density of solid-state batteries, solves the problem of low specific capacity of the positive electrode, and improves the cycle stability and safety of the battery by improving the problem of stress deformation caused by the expansion of lithium embedded in silicon-carbon composite materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117976883B_ABST
    Figure CN117976883B_ABST
Patent Text Reader

Abstract

The present invention relates to the field of battery technology, and specifically to a method for preparing a positive electrode composite material, a positive electrode composite material and a solid-state battery. The raw materials of the positive electrode composite material include: a silicon-carbon composite material, asphalt, polyethylene glycol and polyethylene oxide, wherein the mass percentage of asphalt in the positive electrode composite material is 4.0%-6.0%, the mass percentage of polyethylene glycol in the positive electrode composite material is 0.2%-0.5%, the mass percentage of polyethylene oxide in the positive electrode composite material is 1.5%-1.8%, and the sum of the mass percentages of polyethylene glycol and the polyethylene oxide in the positive electrode composite material is 2.0%. By using the silicon-carbon composite material as the positive electrode, the specific capacity of the positive electrode can be increased, thereby increasing the energy density of the solid-state battery, solving the problem that the positive electrode specific capacity of the existing solid-state battery is low and the application scope of the solid-state battery is limited, and the serious problem of lithium expansion of the silicon-carbon composite material is improved by carbonization coating of asphalt and doping with polyethylene glycol and polyethylene oxide.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of batteries, and in particular to a method for preparing a positive electrode composite material, a positive electrode composite material and a solid-state battery. Background Art

[0002] With the development of new energy technologies, lithium-ion batteries have become a development focus of the new energy industry. However, the energy density of traditional liquid electrolyte lithium-ion batteries has developed to a point close to the theoretical limit, so people have begun to explore solid-state battery technology to improve battery energy density and battery safety performance.

[0003] Existing solid-state batteries generally use traditional lithium-ion battery positive electrode materials as positive electrodes, such as lithium nickel cobalt manganese oxide (NCM), lithium iron phosphate (LFP), etc. Among them, NCM with a higher theoretical specific capacity can only reach 285mAh / g, and the actual specific capacity is lower than the theoretical specific capacity, which limits the application scope of solid-state batteries.

[0004] In view of this, providing a new method for preparing a positive electrode composite material, a positive electrode composite material and a solid-state battery has become a technical problem to be solved urgently in this field. Summary of the invention

[0005] In view of the defects in the prior art, the purpose of the present invention is to provide a method for preparing a positive electrode composite material, a positive electrode composite material and a solid-state battery, so as to solve the technical problem that the positive electrode specific capacity of the existing solid-state battery is low, which limits the application scope of the solid-state battery.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] On the one hand, the present invention provides a positive electrode composite material, the raw materials of which include the following components: a silicon-carbon composite material, asphalt, polyethylene glycol and polyethylene oxide, wherein the mass percentage of the asphalt in the positive electrode composite material is 4.0%-6.0%, the mass percentage of the polyethylene glycol in the positive electrode composite material is 0.2%-0.5%, the mass percentage of the polyethylene oxide in the positive electrode composite material is 1.5%-1.8%, and the sum of the mass percentages of the polyethylene glycol and the polyethylene oxide in the positive electrode composite material is 2.0%.

[0008] According to one embodiment of the present invention, the raw materials of the silicon-carbon composite material include the following components: spherical natural graphite, silane and acetylene, wherein the mass ratio of the silane to the acetylene is 5:1.

[0009] Another aspect of the present invention provides a method for preparing a positive electrode composite material, comprising the following steps:

[0010] Silicon-carbon composite materials were prepared by chemical vapor deposition;

[0011] Mixing 4.0%-6.0% of asphalt by mass into the silicon-carbon composite material, carbonizing and coating the mixture at 1200-1500° C., and then crushing, screening and demagnetizing the mixture to obtain a silicon-carbon composite material with graphite coated on the surface;

[0012] Mixing 0.2%-0.5% by weight of polyethylene glycol and 1.5%-1.8% by weight of polyethylene oxide into a silicon-carbon composite material coated with graphite, and stirring the mixture;

[0013] The uniformly stirred mixture is coated on a copper current collector sheet with a thickness of 200-500 μm, and molded at a temperature of 70-85° C. and a hot press of 10-15 MPa for 20-30 seconds to obtain the positive electrode composite material.

[0014] According to one embodiment of the present invention, the preparation of silicon-carbon composite material by chemical vapor deposition includes: placing spherical natural graphite in a reaction furnace, and introducing a mixed gas of silane and acetylene with a mass ratio of 5:1, completing chemical vapor deposition at a temperature of 900°C, to obtain the silicon-carbon composite material.

[0015] Another aspect of the present invention provides a solid-state battery, comprising a positive electrode sheet, wherein the positive electrode sheet comprises the positive electrode composite material or the positive electrode composite material prepared according to the preparation method.

[0016] According to one embodiment of the present invention, the solid-state battery also includes a battery casing, and a positive electrode copper tab, a positive electrode current collector, a solid electrolyte, a negative electrode sheet, a negative electrode current collector and a negative electrode copper tab are arranged in sequence in the battery casing, and the positive electrode sheet is arranged between the positive electrode current collector and the solid electrolyte.

[0017] According to an embodiment of the present invention, a conductive spring sheet with elasticity is further provided between the negative electrode copper tab and the negative electrode current collector.

[0018] According to one embodiment of the present invention, the solid electrolyte is lithium lanthanum zirconium oxide with a thickness of 200 μm.

[0019] According to one embodiment of the present invention, the negative electrode sheet is a lithium metal sheet with a thickness of 100-300 μm.

[0020] According to one embodiment of the present invention, the positive electrode current collector is made of copper foil with a thickness of 30-50 μm, and the negative electrode current collector is made of copper foil with a thickness of 60-100 μm.

[0021] Beneficial effects: The raw materials of the positive electrode composite material include the following components: a silicon-carbon composite material, asphalt, polyethylene glycol and polyethylene oxide, wherein the mass percentage of the asphalt in the positive electrode composite material is 4.0%-6.0%, the mass percentage of the polyethylene glycol in the positive electrode composite material is 0.2%-0.5%, the mass percentage of the polyethylene oxide in the positive electrode composite material is 1.5%-1.8%, and the sum of the mass percentages of the polyethylene glycol and the polyethylene oxide in the positive electrode composite material is 2.0%. By using the silicon-carbon composite material as the positive electrode, the specific capacity of the positive electrode can be increased, thereby improving the energy density of the solid-state battery, solving the technical problem that the specific capacity of the positive electrode of the existing solid-state battery is low and the application scope of the solid-state battery is limited. The problem of stress deformation caused by lithium insertion expansion of the silicon-carbon composite material can be improved by carbonizing and coating the asphalt and doping polyethylene glycol and polyethylene oxide. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is a schematic structural diagram of a solid-state battery according to an embodiment of the present invention;

[0023] Figure 2 is a schematic structural diagram of a conductive spring in a normal state according to an embodiment of the present invention;

[0024] Figure 3 is a schematic structural diagram of a conductive spring in an extruded state according to an embodiment of the present invention;

[0025] Figure 4 It is a schematic flow chart of a method for preparing a positive electrode composite material according to an embodiment of the present invention;

[0026] Figure 5 is a graph showing the cycle performance test results of the solid-state battery of Example 1 of the present invention;

[0027] Figure 6 is a graph showing the cycle performance test results of the solid-state battery of Example 2 of the present invention;

[0028] Figure 7 This is a graph showing the cycle performance test results of the solid-state battery of Example 3 of the present invention. DETAILED DESCRIPTION

[0029] The technical solution of the present invention is described below through specific embodiments.

[0030] See also Figure 1 The solid-state battery 100 of the embodiment of the present invention comprises a battery housing 101, a positive electrode copper tab 102, a positive electrode current collector 103, a positive electrode sheet 104, a solid electrolyte 105, a negative electrode sheet 106, a negative electrode current collector 107 and a negative electrode copper tab 108 arranged in sequence in the battery housing 101. The positive electrode sheet 104 of this embodiment is made of a silicon-carbon composite material.

[0031] In some possible implementations, such as Figure 1 As shown, a conductive spring sheet 109 with elasticity is provided between the negative electrode copper tab 108 and the negative electrode current collector 107. Figure 2 As shown, the conductive spring 109 is stretched in a normal state. Figure 3 As shown, the conductive spring 109 is compressed in an extruded state. The negative electrode copper tab 108, the negative electrode current collector 107 and the conductive spring 109 are movably connected. This embodiment utilizes the elasticity of the conductive spring 109 to exert a certain extrusion effect on the battery core material, and can maintain close contact between the materials. Furthermore, the conductive spring 109 can be made of a designed polyacetylene material, which has physical elasticity and good conductivity.

[0032] In some achievable embodiments, the solid electrolyte 105 is lithium lanthanum zirconium oxide and has a thickness of 200 μm.

[0033] In some achievable embodiments, the negative electrode sheet 106 is a lithium metal sheet with a thickness of 100-300 μm, preferably 200-300 μm.

[0034] In some feasible embodiments, the positive electrode current collector 103 uses a copper foil with a thickness of 30-50 μm. The negative electrode current collector 107 uses a copper foil with a thickness of 60-100 μm, preferably 65-100 μm. Because the positive electrode material is a silicon-carbon composite material, its electrode potential is relatively low. If a traditional aluminum material is used as the positive electrode current collector, low-potential aluminum metal lithium will be embedded to form an aluminum-lithium alloy. Therefore, the positive electrode current collector 103 and the negative electrode current collector 107 are replaced with copper foil. Furthermore, the positive electrode current collector 103 has a frosted toothed surface on one side that contacts the positive electrode material, and the height difference between the highest and lowest points of the tooth is 5 μm, which can improve the bonding force between the positive electrode material and the positive electrode current collector 103 and the conductivity of the contact interface. Furthermore, the thickness of the negative electrode collector 107 is increased relative to the thickness of the positive electrode collector 103, because a conductive spring 109 is provided between the negative electrode copper tab 108 and the negative electrode collector 107, and the thickness is increased to cope with the extrusion pressure brought by the conductive spring 109. The side of the negative electrode collector 107 that contacts the negative electrode material is a frosted serrated surface, and the height difference between the highest and lowest points of the serrations is 5 μm, which can improve the bonding force between the negative electrode material and the negative electrode collector 107 and the conductivity of the contact interface.

[0035] In some feasible implementations, the battery housing 101 is made of an aluminum shell with good rigidity and strength. The battery housing 101 serves to isolate the battery core material from the external environment and plays a certain structural protection role.

[0036] The assembly process of the solid-state battery 100 is as follows: complete the assembly of the above materials in a nitrogen environment of a glove box, place the positive electrode sheet 104 and the negative electrode sheet 106 with the sides coated with active material facing each other, and sandwich the solid electrolyte 105 in the middle. The solid electrolyte 105 is sandwiched between the silicon-carbon composite material positive electrode and the lithium metal negative electrode to isolate the positive and negative electrode materials, conduct ions and insulate electrons. Press at a pressure of 5Mpa for 30s, weld the positive electrode copper tab 102 to the side of the positive electrode collector 103 that is not coated with active material, and play a role in positive electrode conductivity; sandwich a conductive spring sheet 109 between the negative electrode copper tab 108 and the negative electrode collector 107, and connect them in a movable state. The negative electrode copper tab 108 is then fixedly connected to the battery casing 101. All joints of the battery casing 101 are sealed to complete the battery assembly. The solid-state battery 100 adds a conductive spring sheet 109 between the negative electrode current collector 107 and the negative electrode copper tab 108 to compress the battery cell material. When the silicon-carbon composite material positive electrode expands due to lithium embedding, and the discharge volume of the lithium metal negative electrode decreases, the thickness of the entire battery cell will fluctuate. This compression effect can make the battery materials in close contact without causing cracks inside the battery due to deformation of the material, which will lead to increased internal resistance. At the same time, it also needs to have sufficient conductivity to act as a part of the tab.

[0037] An embodiment of the present invention also provides a positive electrode composite material, the raw materials of which include the following components: a silicon-carbon composite material, asphalt, polyethylene glycol and polyethylene oxide, wherein the mass percentage of asphalt in the positive electrode composite material is 4.0%-6.0%, the mass percentage of polyethylene glycol in the positive electrode composite material is 0.2%-0.5%, the mass percentage of polyethylene oxide in the positive electrode composite material is 1.5%-1.8%, and the sum of the mass percentages of polyethylene glycol and polyethylene oxide in the positive electrode composite material is 2.0%.

[0038] In some achievable embodiments, the raw materials of the silicon-carbon composite material include the following components: spherical natural graphite, silane and acetylene, wherein the mass ratio of silane to acetylene is 5: 1. The particle size of the spherical natural graphite can be selected to be 5 to 50 nm, and the role of the spherical natural graphite is to adjust the ratio of silicon to carbon in the silicon-carbon composite material.

[0039] The positive electrode composite material of the embodiment of the present invention uses a silicon-carbon composite material as the positive electrode, which can increase the specific capacity of the positive electrode, thereby increasing the energy density of the solid-state battery, solving the technical problem that the positive electrode specific capacity of the existing solid-state battery is low, which limits the application scope of the solid-state battery. The silicon-carbon composite material is carbonized and coated with asphalt and doped with polyethylene glycol and polyethylene oxide to improve the problem of stress deformation caused by lithium insertion expansion.

[0040] The present invention also provides a method for preparing a positive electrode composite material. Figure 4As shown, the preparation method comprises the following steps:

[0041] Step S1: preparing a silicon-carbon composite material by chemical vapor deposition.

[0042] In this step, spherical natural graphite is placed in a reactor, and a mixed gas of silane and acetylene with a mass ratio of 5:1 is introduced at a rate of 2L / min, and chemical vapor deposition is completed at a temperature of 900°C to obtain a silicon-carbon composite material. In the silicon-carbon composite material, the theoretical specific capacity of carbon is 372mAh / g, and the theoretical specific capacity of silicon is 4200mAh / g. The silicon-carbon composite material obtains different specific capacities through different ratios of the two, which is significantly improved compared with the specific capacity of traditional positive electrode materials.

[0043] Step S2: 4.0%-6.0% by mass of asphalt is mixed into the silicon-carbon composite material, and carbonization coating is performed at 1200-1500° C., and then crushing, screening and demagnetization are performed to obtain a silicon-carbon composite material with a surface coated with graphite.

[0044] In this step, coating with graphite can effectively improve the conductivity of the silicon-carbon composite material.

[0045] Step S3: mixing 0.2%-0.5% by weight of polyethylene glycol and 1.5%-1.8% by weight of polyethylene oxide into the silicon-carbon composite material with the surface coated with graphite, and stirring the mixture.

[0046] In this step, doping a certain proportion of polyethylene glycol and polyethylene oxide can reduce the stress deformation caused by lithium insertion and expansion of the positive electrode material.

[0047] Step S4: coating the uniformly stirred mixture on a copper current collector sheet with a thickness of 200-500 μm, and molding the mixture at a temperature of 70-85° C. and a hot press of 10-15 MPa for 20-30 seconds to obtain a positive electrode composite material.

[0048] The preparation method of the positive electrode composite material in the embodiment of the present invention uses a silicon-carbon composite material as the positive electrode, which can improve the specific capacity of the positive electrode, thereby improving the energy density of the solid-state battery, solving the technical problem that the positive electrode specific capacity of the existing solid-state battery is low and limits the application scope of the solid-state battery, and improves the problem of stress deformation caused by lithium embedding expansion of the silicon-carbon composite material by carbonization coating with asphalt and doping with polyethylene glycol and polyethylene oxide.

[0049] Example 1

[0050] (1) Preparation of positive electrode composite materials

[0051] Spherical natural graphite is placed in a furnace, and a mixed gas of silane and acetylene with a mass ratio of 5:1 is introduced at a rate of 2L / min, and chemical vapor deposition is completed at a temperature of 900°C to prepare a silicon-carbon composite material, which is then crushed and screened; 4.0% of asphalt is mixed into the silicon-carbon composite material, and carbonization and coating are carried out at 1300°C, and then crushed, screened and demagnetized to obtain a silicon-carbon composite material with graphite coated on the surface; finally, 0.2% of polyethylene glycol and 1.8% of polyethylene oxide are mixed into the silicon-carbon composite material with graphite coated on the surface, and after sufficient stirring and mixing, it is coated on a copper current collector sheet with a thickness of 300μm, and hot pressed at 75°C and 10Mpa for 20s to obtain a positive electrode composite material.

[0052] (2) Other battery material options

[0053] The negative electrode sheet is made of a 200μm thick lithium metal sheet; the solid electrolyte is made of a 200μm thick lithium lanthanum zirconium oxide; the positive current collector is made of a 35μm thick copper foil, and the positive current collector has a frosted serrated surface on one side in contact with the positive electrode material, with a height difference of 5μm between the highest and lowest points of the teeth; the negative current collector is made of an 80μm thick copper foil, and the negative current collector has a frosted serrated surface on one side in contact with the negative electrode material, with a height difference of 5μm between the highest and lowest points of the teeth; the conductive spring is made of a designed and molded polyacetylene spring.

[0054] (3) Assemble batteries using the above materials and conduct battery performance tests

[0055] The battery theoretical voltage is between 2.245V and 3.045V (the actual battery voltage varies according to the ratio of silicon to carbon). Battery capacity test results: Figure 5 As shown, the actual voltage of the battery is 2.53V, the positive electrode specific capacity reaches 827.2mAh / g, the first coulombic efficiency is 92.6%, and the positive electrode specific capacity is 761.2mAh / g after 100 cycles, that is, the specific capacity loss after 100 cycles is 7.98%. The expansion rate of the silicon-carbon composite material positive electrode is only 29%, which can effectively reduce the harm caused by the battery volume expansion.

[0056] Example 2

[0057] (1) Preparation of positive electrode composite materials

[0058] Spherical natural graphite is placed in a furnace, and a mixed gas of silane and acetylene with a mass ratio of 5:1 is introduced at a rate of 2L / min, and chemical vapor deposition is completed at a temperature of 900°C to prepare a silicon-carbon composite material, which is then crushed and screened; 5.0% by mass of asphalt is mixed into the silicon-carbon composite material, and carbonization and coating are carried out at 1300°C, and then crushed, screened and demagnetized to obtain a silicon-carbon composite material with graphite coated on the surface; finally, 0.5% by mass of polyethylene glycol and 1.5% of polyethylene oxide are mixed into the silicon-carbon composite material with graphite coated on the surface, and after sufficient stirring and mixing, it is coated on a copper current collector sheet with a thickness of 400μm, and hot pressed at 80°C and 10Mpa for 20s to obtain a positive electrode composite material.

[0059] (2) Other battery material options

[0060] The negative electrode sheet is made of 250μm thick lithium metal sheet; the solid electrolyte is made of 200μm thick lithium lanthanum zirconium oxide; the positive electrode collector is made of 30μm thick copper foil, and the positive electrode collector has a frosted serrated surface on one side in contact with the positive electrode material, and the height difference between the highest and lowest points of the teeth is 5μm; the negative electrode collector is made of 65μm thick copper foil, and the negative current collector has a frosted serrated surface on one side in contact with the negative electrode material, and the height difference between the highest and lowest points of the teeth is 5μm; the conductive spring is made of designed and formed polyacetylene spring.

[0061] (3) Assemble batteries using the above materials and conduct battery performance tests

[0062] The battery theoretical voltage is between 2.245V and 3.045V (the actual battery voltage varies according to the ratio of silicon to carbon). Battery capacity test results: Figure 6 As shown, the actual voltage of the battery is 2.64V, the positive electrode specific capacity reaches 813.4mAh / g, the first coulombic efficiency is 91.7%, and the positive electrode specific capacity is 720mAh / g after 100 cycles, that is, the specific capacity loss after 100 cycles is 11.48%. The expansion rate of the silicon-carbon composite material positive electrode is only 31.5%, which can effectively reduce the harm caused by the battery volume expansion.

[0063] Example 3

[0064] (1) Preparation of positive electrode composite materials

[0065] Spherical natural graphite is placed in a furnace, and a mixed gas of silane and acetylene with a mass ratio of 5:1 is introduced at a rate of 2L / min, and chemical vapor deposition is completed at a temperature of 900°C to prepare a silicon-carbon composite material, which is then crushed and screened; 6.0% of asphalt is mixed into the silicon-carbon composite material, and carbonization and coating are carried out at 1300°C, and then crushed, screened and demagnetized to obtain a silicon-carbon composite material with graphite coated on the surface; finally, 0.5% of polyethylene glycol and 1.5% of polyethylene oxide are mixed into the silicon-carbon composite material with graphite coated on the surface, and after sufficient stirring and mixing, a 500μm thickness is coated on a copper current collector sheet, and hot pressing is performed at 80°C and 10Mpa for 30s to obtain a positive electrode composite material.

[0066] (2) Other battery material options

[0067] The negative electrode sheet is made of 300μm thick lithium metal sheet; the solid electrolyte is made of 200μm thick lithium lanthanum zirconium oxide; the positive electrode collector is made of 50μm thick copper foil, and the positive electrode collector has a frosted serrated surface on one side in contact with the positive electrode material, with a height difference of 5μm between the highest and lowest points of the teeth; the negative electrode collector is made of 100μm thick copper foil, and the negative electrode collector has a frosted serrated surface on one side in contact with the negative electrode material, with a height difference of 5μm between the highest and lowest points of the teeth; the conductive spring is made of designed and molded polyacetylene spring.

[0068] (3) Assemble batteries using the above materials and conduct battery performance tests

[0069] The battery theoretical voltage is between 2.245V and 3.045V (the actual battery voltage varies according to the ratio of silicon to carbon). Battery capacity test results: Figure 7 As shown, the actual voltage of the battery is 2.53V, the positive electrode specific capacity reaches 789.7mAh / g, the first coulombic efficiency is 89.5%, and the positive electrode specific capacity is 689.2mAh / g after 100 cycles, that is, the specific capacity loss after 100 cycles is 12.73%. The expansion rate of the silicon-carbon composite material positive electrode is only 32.8%, which can effectively reduce the harm caused by the battery volume expansion.

[0070] The present invention performs battery performance tests on Examples 1-3, and the test results are shown in Table 1.

[0071] Battery performance test: The Xinwei battery testing system is used. The testing method is as follows: the positive and negative electrodes are welded to the external pole ears. The electrode fixture of the battery testing system is connected to the external pole ears and then the charge and discharge cycle test is carried out. The battery gram capacity (i.e., mass specific capacity) and coulombic efficiency and other data are calculated based on the mass and charge and discharge capacity of the silicon-carbon composite material used in the solid-state battery.

[0072] Table 1: Battery performance test results of Examples 1-3.

[0073]

[0074] As shown in Table 1, the positive electrode specific capacity of Examples 1-3 reaches more than 780 mAh / g, and the positive electrode specific capacity can still reach more than 680 mAh / g after 100 cycles, indicating that the embodiments of the present application use the positive electrode composite material containing silicon-carbon composite material as the positive electrode, which effectively improves the positive electrode specific capacity compared with the traditional lithium-ion battery positive electrode material as the positive electrode. In addition, the positive electrode expansion rate is between 29% and 32.8%, and the surface is carbonized and coated with asphalt and doped with polyethylene glycol and polyethylene oxide to improve the serious expansion problem of silicon-carbon composite material embedded in lithium.

[0075] The above are only implementation modes of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.

Claims

1. A positive electrode sheet, It is characterized in that The positive electrode sheet includes a positive electrode composite material, and the raw materials of the positive electrode composite material include the following components: a silicon-carbon composite material, asphalt, polyethylene glycol and polyethylene oxide, wherein the mass percentage of the asphalt in the positive electrode composite material is 4.0%-6.0%, the mass percentage of the polyethylene glycol in the positive electrode composite material is 0.2%-0.5%, the mass percentage of the polyethylene oxide in the positive electrode composite material is 1.5%-1.8%, and the sum of the mass percentages of the polyethylene glycol and the polyethylene oxide in the positive electrode composite material is 2.0%; The raw materials of the silicon-carbon composite material include the following components: spherical natural graphite, silane and acetylene, wherein the mass ratio of the silane to the acetylene is 5:1; The method for preparing the positive electrode sheet comprises the following steps: The silicon-carbon composite material is prepared by chemical vapor deposition, comprising: placing spherical natural graphite in a reaction furnace, introducing a mixed gas of silane and acetylene in a mass ratio of 5:1, and completing chemical vapor deposition at a temperature of 900° C. to obtain the silicon-carbon composite material; Mixing 4.0%-6.0% of asphalt by mass into the silicon-carbon composite material, carbonizing and coating the mixture at 1200-1500° C., and then crushing, screening and demagnetizing the mixture to obtain a silicon-carbon composite material with graphite coated on the surface; Mixing 0.2%-0.5% by weight of polyethylene glycol and 1.5%-1.8% by weight of polyethylene oxide into a silicon-carbon composite material coated with graphite, and stirring the mixture; The uniformly stirred mixture is coated on a copper current collector sheet with a thickness of 200-500 μm, and is molded at a temperature of 70-85° C. and a hot press of 10-15 MPa for 20-30 seconds to obtain the positive electrode sheet.

2. A method for preparing the positive electrode sheet as claimed in claim 1, It is characterized in that The following steps are involved: The silicon-carbon composite material is prepared by chemical vapor deposition, comprising: placing spherical natural graphite in a reaction furnace, introducing a mixed gas of silane and acetylene in a mass ratio of 5:1, and completing chemical vapor deposition at a temperature of 900° C. to obtain the silicon-carbon composite material; Mixing 4.0%-6.0% of asphalt by mass into the silicon-carbon composite material, carbonizing and coating the mixture at 1200-1500° C., and then crushing, screening and demagnetizing the mixture to obtain a silicon-carbon composite material with graphite coated on the surface; Mixing 0.2%-0.5% by weight of polyethylene glycol and 1.5%-1.8% by weight of polyethylene oxide into a silicon-carbon composite material coated with graphite, and stirring the mixture; The uniformly stirred mixture is coated on a copper current collector sheet with a thickness of 200-500 μm, and is molded at a temperature of 70-85° C. and a hot press of 10-15 MPa for 20-30 seconds to obtain the positive electrode sheet.

3. A solid-state battery, It is characterized in that Including the positive electrode sheet according to claim 1 or the positive electrode sheet prepared by the preparation method according to claim 2.

4. The solid-state battery according to claim 3, It is characterized in that The solid-state battery also includes a battery shell, a positive electrode copper tab, a positive electrode current collector, a solid electrolyte, a negative electrode material, a negative electrode current collector and a negative electrode copper tab are arranged in sequence in the battery shell, and the positive electrode composite material is arranged between the positive electrode current collector and the solid electrolyte.

5. The solid-state battery according to claim 4, It is characterized in that A conductive spring sheet with elasticity is also provided between the negative electrode copper tab and the negative electrode current collector.

6. The solid-state battery according to claim 4, It is characterized in that The solid electrolyte is lithium lanthanum zirconium oxide and has a thickness of 200 μm.

7. The solid-state battery according to claim 4, It is characterized in that The negative electrode material is a lithium metal sheet with a thickness of 100-300 μm.

8. The solid-state battery according to claim 4, It is characterized in that The positive electrode current collector adopts a copper foil with a thickness of 30-50 μm, and the negative electrode current collector adopts a copper foil with a thickness of 60-100 μm.