A stimulus-responsive amphiphilic conjugated polymer and its preparation method
By preparing amphiphilic conjugated polymer nanoparticles PEI-NPs and using the Schiff base reaction to form a stimulus-responsive conjugated polymer, the problems of conjugated polymer solubility and biocompatibility were solved, achieving effective penetration and killing of bacterial biofilms and exhibiting highly efficient photothermal therapy effects.
Patent Information
- Application Number
- CN202410092663.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-23
- Publication Date
- 2026-11-10
- Estimated Expiration
- 2044-01-23
AI Technical Summary
Existing conjugated polymers have a planar molecular structure due to intermolecular conjugation interactions and strong π-π stacking, which reduces solubility and increases the difficulty of functionalization modification. Meanwhile, nanoparticles have problems such as low encapsulation efficiency, easy dissociation and poor biocompatibility, making it difficult to effectively penetrate bacterial biofilms for treatment.
Amphiphilic conjugated polymer nanoparticles PEI-NPs were prepared under neutral conditions. They were then reacted with CHO-Ar-COO-PEGn-COO-Ar-CHO to form a stimulus-responsive conjugated polymer. The nanoparticles were exposed with positive surface charge in a slightly acidic environment, targeting the bacterial surface and generating heat to kill the bacteria under near-infrared light irradiation.
The high water solubility and biocompatibility of the conjugated polymer were achieved. The nanoparticles can effectively penetrate bacterial biofilms, have photothermal effects, and significantly kill bacteria. The synthesis method is simple and low-cost, and has broad potential for biomedical applications.
Smart Images

Figure QLYQS_1 
Figure QLYQS_2 
Figure QLYQS_3
Abstract
Description
Technical Field
[0001] This invention belongs to the field of materials, specifically relating to a stimulus-responsive amphiphilic conjugated polymer and its preparation method, which can penetrate bacterial biofilms and can be used to treat bacterial infection-related diseases. Background Technology
[0002] Conjugated polymers (CPs) have many advantages, such as strong photostability, high absorption factor, strong structural controllability, high biocompatibility, and adjustable response spectrum. Therefore, CPs have attracted widespread attention as photothermal agents in the fields of antibacterial and biofilm disruption.
[0003] Existing one-dimensional linear conjugated polymers and conjugated porous polymers suffer from planar molecular structures and molecular rigidity due to intermolecular conjugation interactions and strong π-π stacking. This reduces the solubility of conjugated polymers and increases the difficulty of functionalization modification, hindering the application and promotion of conjugated polymer materials. Currently, a common method is to encapsulate conjugated polymers into highly water-dispersible and biocompatible nanoparticles using methods such as dispersion with biocompatible amphiphilic polymers. However, these nanoparticles have certain limitations, such as low encapsulation efficiency, easy dissociation, short cycle time, and poor biocompatibility. Furthermore, developing novel therapeutic agents capable of penetrating biofilm barriers to enter bacteria is of great significance for treating biofilm infections. Summary of the Invention
[0004] One objective of this invention is to provide a stimulus-responsive amphiphilic conjugated polymer and a method for preparing the same.
[0005] The stimulus-responsive amphiphilic conjugated polymer provided by this invention is prepared by reacting amphiphilic conjugated polymer nanoparticles PEI-NPs and CHO-Ar-COO-PEGn-COO-Ar-CHO (Ar represents a substituted or unsubstituted aromatic group, wherein the substituted aromatic group is at least one of the following: at least one H on at least one C of the aromatic group is substituted by a halogen, a C1-C6 alkyl group, a C1-C6 alkoxy group, or a C1-C6 alkyl group substituted by a halogen; n represents the molecular weight of polyethylene glycol, n = 500-2000) under neutral conditions with a Schiff base reaction.
[0006] The amphiphilic conjugated polymer nanoparticles PEI-NPs can be prepared from the polymer shown in Formula II:
[0007]
[0008] In Formula II, R can be any of the following groups:
[0009]
[0010] in, express p is an integer between 3 and 10, specifically 5; n = 10 - 50, m = 1 - 50; a = 10 - 50, b = 1 - 50; c = 1 - 50;
[0011] X+Y=1, where the value of X ranges from 0.1 to 0.9; n represents the degree of aggregation, which ranges from 10 to 1000.
[0012] The ratio of X to Y affects the light absorption characteristics. Specifically, when X > Y, the absorption peak wavelength is 650-850 nm; when X = Y, the absorption peak wavelength is 800-900 nm; and when X < Y, the absorption peak wavelength is 950-1200 nm.
[0013] Specifically, the polymer shown in Formula II can be:
[0014]
[0015] The polymer shown in Formula II above is prepared by a method comprising the following steps:
[0016] 1) In the presence of a catalyst and ligand, the compound shown in Formula III undergoes Stille polycondensation with the compound shown in Formula IV and the compound shown in Formula VI to obtain an intermediate;
[0017]
[0018] In equation III above, the definition of R1 is the same as the definition of R in equation II (R1 is...). Where p is an integer between 3 and 10;
[0019] 2) The obtained intermediate was reacted with N3-PEG-PEI (where PEG-PEI represents PEI-modified PEG) to obtain the polymer shown in Formula II;
[0020] In step 1), the catalyst may be at least one of tetra(triphenylphosphine)palladium, di(triphenylphosphine)palladium dichloride, tri(dibenzylacetone)palladium and di(dibenzylacetone)palladium;
[0021] The ligand is selected from at least one of triphenylphosphine, tris(o-tolyl)phosphine, and tris(furanyl)phosphine.
[0022] The molar amount of the compound shown in Formula III can be 0.95 to 1.05 parts;
[0023] The molar amount of the compound shown in Formula IV can be 0.95 to 1.05 parts;
[0024] The molar amount of the compound shown in Formula VI can be 1.9 to 2.1 parts;
[0025] The molar amount of the catalyst can be 0.02 to 0.1 parts;
[0026] The molar amount of the ligand can be 0.1 to 0.2 parts;
[0027] Specifically, the molar ratio of the compound shown in Formula III, the compound shown in Formula IV, the compound shown in Formula VI, the catalyst, and the ligand can be 1.0:1.0:2.0:0.089:0.2;
[0028] The Stille polycondensation reaction can be carried out at a temperature of 100–120°C for 2–3 hours.
[0029] The Stille polycondensation reaction is carried out in a solvent, which may specifically be toluene or chlorobenzene.
[0030] In step 2), the molar ratio of the intermediate to N3-PEG-PEI can be 1:3-5, specifically 1:4.2;
[0031] The reaction is carried out under the catalysis of cuprous iodide; the molar ratio of the intermediate to cuprous iodide can be 1:10-20;
[0032] The reaction temperature is 20-50℃, specifically 25℃, and the reaction time is 24-72h, specifically 48h.
[0033] The present invention also provides a method for preparing polymer nanoparticles as shown in Formula II above.
[0034] The polymer nanoparticles shown in Formula II above are prepared by a method comprising the following steps:
[0035] (1) Dissolve the polymer shown in Formula II in an organic solvent, remove the organic solvent by vacuum distillation, and form a thin film;
[0036] (2) The resulting mixture was added to ultrapure water, and an aqueous solution of nanoparticles was obtained by self-assembly.
[0037] (3) The obtained nanoparticles are obtained by dialysis of the aqueous solution of the nanoparticles.
[0038] In step (1) of the above method, the organic solvent may specifically be chloroform;
[0039] In step (2) of the above method, the volume of ultrapure water can be 8-15 mL, specifically 10 mL;
[0040] In step (3) of the above method, the molecular weight cutoff of the dialysis bag for dialysis is 10000kDa.
[0041] Specifically, CHO-Ar-COO-PEGn-CO-Ar-CHO can be: CHO-Ph-COO-PEG 1000 -CO-Ph–CHO;
[0042] The neutral conditions are specifically pH = 7.0 to 8.0, and the mass ratio of PEI-NPs / CHO-Ar-COO-PEGn-CO-Ar-CHO is 1:0 to 1:20 (endpoint 0 is not acceptable); preferably 1:12.
[0043] The Schiff base reaction can be carried out at room temperature for 1-4 hours, specifically 2 hours.
[0044] In a specific embodiment of the present invention, the structural formula of the stimulus-responsive amphiphilic conjugated polymer is shown in Formula I:
[0045]
[0046] In Formula I, PEG-PEI represents PEG modified with PEI, specifically as follows:
[0047]
[0048] in, express p = 4, n = 16, m = 4.
[0049] The stimulus-responsive polymer-based nanoparticles have a particle size of 175.8 nm to 241.3 nm, particularly in PEI-NPs / CHO-Ph-COO-PEG. 1000 When the mass ratio of -CO-Ph–CHO is 1:12, the nanoparticle size reaches its minimum of 175.8 nm.
[0050] The surface charge of the stimulus-responsive polymer-based nanoparticles is +15.9 mV to +36.1 mV, particularly in PEI-NPs / CHO-Ph-COO-PEG. 1000 When the mass ratio of -CO-Ph–CHO is 1:20, the surface charge reaches its minimum of +15.9mV.
[0051] When the stimulus-responsive polymer-based nanoparticles are in a slightly acidic environment with a pH less than 6.8, the Schiff base bonds will be broken, and the surface charge and particle size will increase. Specifically, at pH = 6.8, the surface charge is +36.1 mV and the particle size is 241.3 nm.
[0052] The application of the above-mentioned stimulus-responsive polymer-based nanoparticles in the preparation of products for treating bacterial infection-related diseases also falls within the scope of protection of this invention.
[0053] The stimulus-responsive polymer-based nanoparticles can penetrate bacterial biofilms and can be used to treat diseases related to bacterial infections.
[0054] The bacteria in question may specifically be Staphylococcus aureus.
[0055] This invention also provides a novel antibacterial method. When pH-responsive nanoparticles enter the slightly acidic environment of a biofilm, their positive surface charge is exposed, allowing them to target the surface of Staphylococcus aureus. Then, in response to near-infrared light, they generate a large amount of heat, thereby killing the bacteria.
[0056] The advantages of this invention are:
[0057] 1. The synthesis method is simple, the synthesis route is short, the raw materials are inexpensive and readily available, the process is highly safe, the operation is simple, the production cost is low, and the reaction yield is high;
[0058] 2. The structure of the conjugated polymer is determined and can be accurately characterized;
[0059] 3. The prepared nanoparticles have uniform morphology and stable structure, which solves the problem of poor water solubility of conjugated polymers.
[0060] 4. This conjugated polymer has amphiphilic and self-assembly effects. After forming nanoparticles, the absorption spectrum red-shifts, resulting in a stronger photothermal effect. By modifying the hydrophilic side chain groups, it can utilize hydrophobic interactions to self-assemble into water-soluble nanomaterials with photothermal effects.
[0061] 5. The pH-responsive conjugated polymer nanoparticles provided by this invention exhibit significant advantages in neutral environments, including a smaller zeta potential, more compact size, and enhanced stability. In slightly acidic environments, their surface positive charge increases, and the positive charges on the side chains interact with the bacterial cell surface. Once the biofilm is disrupted, the nanomaterials can penetrate the biofilm and continuously generate heat under near-infrared light irradiation, leading to biofilm destruction. This pH-responsive system has the potential to be applied to other polycationic nanoparticles with amino groups on their surfaces, showing broad application prospects in the biomedical field. Attached Figure Description
[0062] Figure 1 This is a synthetic route diagram for preparing the compound of formula II in Example 1 of the present invention.
[0063] Figure 2 The UV-Vis absorption spectra of the compounds prepared in Examples 1 and 2 of this invention are shown.
[0064] Figure 3 The image shows the photothermal effect of the DPP-BBT-PEI-NPs nanoparticles prepared in Example 2 of this invention.
[0065] Figure 4This is a TEM image of the DPP-BBT-PEI-NPs nanoparticles prepared in Example 2 of the present invention.
[0066] Figure 5 The image shows the photothermal effect of the PEI / CHO-NPs nanoparticles prepared in Example 3 of this invention.
[0067] Figure 6 This is a TEM image of the PEI / CHO-NPs nanoparticles prepared in Example 3 of the present invention.
[0068] Figure 7 The image shows the zeta potential of nanoparticles with a mass ratio of PEI / CHO = 1:(0,4,8,12,16,20) prepared in Example 3 of this invention.
[0069] Figure 8 The particle size characterization diagram is shown for the nanoparticles with a mass ratio of PEI / CHO = 1:(0,4,8,12,16,20) prepared in Example 3 of the present invention.
[0070] Figure 9 This is a CLSM diagram of bacterial biofilm treated with pH-responsive nanoparticles PEI / CHO-NPs in Example 4 of the present invention. Detailed Implementation
[0071] The present invention will now be described in further detail with reference to specific embodiments. The given embodiments are merely illustrative of the invention and not intended to limit its scope. The embodiments provided below can serve as a guide for further improvements by those skilled in the art and do not constitute a limitation on the invention in any way.
[0072] Unless otherwise specified, the experimental methods used in the following examples are conventional methods, performed according to the techniques or conditions described in the literature in this field or according to the product instructions. Unless otherwise specified, the materials and reagents used in the following examples are commercially available.
[0073] Example 1: Synthesis of the conjugated polymer DPP-BBT-PEI
[0074] according to Figure 1 The synthetic route shown is used to prepare DPP-BBT-PEI
[0075] (1) Synthesis of 3,6-bis(thiophen-2-yl)pyrrolo[3,4-c]pyrrolo-1,4(2H,5H)-dione
[0076] Sodium tert-amyl alcohol (24.8 g, 225 mmol) was added to 90 mL of tert-amyl alcohol under an argon atmosphere. The mixture was heated to 90 °C and stirred for 0.5 h to ensure complete dissolution. 2-Cyanothiophene (16.4 g, 150 mmol) was added dropwise to the solution, followed by the slow addition of diisopropyl succinate (12.1 g, 60 mmol). The suspension turned a deep red color. After the addition was complete, the reaction mixture was stirred at this temperature for another 2 h. The reaction temperature was lowered to 50 °C, diluted with 65 mL of methanol, and neutralized with 25 mL of glacial acetic acid. The mixture was stirred at this temperature for 15 min and then cooled to room temperature. The reaction mixture was filtered, and the filter cake was extracted with anhydrous methanol and dried under vacuum at 40 °C. 18 g of a red solid was obtained, with a yield of 80%.
[0077] (2) Synthesis of 2,5-bis(hexane-5-yn-1-yl)-3,6-bis(thiophen-2-yl)-2,5-dihydropyrrolo[3,4-c]pyrrolo-1,4-dione
[0078] 3,6-bis(thiophen-2-yl)pyrrolo[3,4-c]pyrrolo-1,4(2H,5H)-dione (3.15 g, 10.5 mmol) was added to a 100 mL round-bottom flask containing anhydrous N,N-dimethylformamide (50 mL) under argon protection. Potassium tert-butoxide (3.06 g, 27.3 mmol) was then added, and the mixture was stirred for 20 min (immediately changing from red to purple). 5-Hexynyl p-toluenesulfonate (9 g, 35.7 mmol) was added to the purple suspension, and the mixture was stirred at 110 °C under argon for 3 h. The reacted solution was extracted with water and dichloromethane, dried over anhydrous sodium sulfate, and the solvent was removed under reduced pressure. The residue was purified by column chromatography (petroleum ether: dichloromethane = 1:3). 3.5 g of a deep red solid was given, in 54.4% yield.
[0079] The structural characterization data are as follows:
[0080] Mass spectrometry: [HR-MS (TOF)] m / z: 460.61
[0081] ¹H NMR spectrum: 400 MHz, Chloroform-d δ 8.90 (d, J = 3.8 Hz, 2H), 7.65 (d, J = 5.0 Hz, 2H), 4.12 (t, J = 7.6 Hz, 4H), 2.26 (dt, J = 9.0, 4.4 Hz, 4H), 1.97–1.82 (m, 8H), 1.67 (q, J = 7.5 Hz, 4H).
[0082] (3) Synthesis of 3-(4-bromothiophen-2-yl)-6-(5-bromothiophen-2-yl)-2,5-di(hexyl-5-yn-1-yl)-2,5-dihydropyrrolo[3,4-c]pyrrolo-1,4-dione
[0083] Compounds 2,5-di(hexane-5-yn-1-yl)-3,6-di(thiophen-2-yl)-2,5-dihydropyrrolo[3,4-c]pyrrolo-1,4-dione (0.4 g, 0.434 mmol), N-bromosuccinimide (0.31 g, 0.868 mmol), and 10 mL of chloroform were added sequentially to a 25 mL single-necked flask. A magnetic stir bar was added, and the mixture was stirred in an ice bath for 6 h. The reacted solution was extracted with water and dichloromethane, dried over anhydrous sodium sulfate, and the solvent was removed under reduced pressure. The residue was purified by column chromatography (petroleum ether: dichloromethane = 1:3), followed by filtration with methanol to give 0.33 g of a purple-red solid, with a yield of 61.1%.
[0084] The structural characterization data are as follows:
[0085] Mass spectrometry: [HR-MS (TOF)] m / z: 618.40
[0086] 1H NMR spectrum: 1H NMR (400MHz, Methylene Chloride-d2) δ 8.71 (d, J = 4.1 Hz, 1H), 7.33 (d, J = 4.0 Hz, 1H), 4.07 (t, J = 7.6 Hz, 2H), 2.35–2.26 (m, 2H), 2.04 (d, J = 2.9 Hz, 1H), 1.87 (q, J = 7.7 Hz, 2H), 1.72–1.63 (m, 2H).
[0087] (4) Synthesis of conjugated polymer DPP-BBT
[0088] To a 25 mL two-necked flask, 3-(4-bromothiophen-2-yl)-6-(5-bromothiophen-2-yl)-2,5-di(hexyl-5-yn-1-yl)-2,5-dihydropyrrolo[3,4-c]pyrrolo-1,4-dione (0.1 g, 0.16 mmol), BBT (0.119 g, 0.16 mmol), 2,5-bis(trimethyltinyl)thiophene (0.13 g, 0.32 mmol), Pd2(dba)3 (0.0133 g, 0.0142 mmol), and tris(o-tolyl)phosphine (0.0096 g, 0.0315 mmol) were added sequentially, followed by 5 mL of toluene. The mixture was degassed by three freeze-thaw cycles, and then reacted at 110 °C under nitrogen for 2 h. After the reaction was complete, the resulting solution was precipitated in ice-cold methanol. The precipitate was collected by filtration, washed three times with methanol, and dried under vacuum to obtain 15 mg of dark green solid, with a yield of 11.5%.
[0089] (5) Synthesis of conjugated polymer DPP-BBT-PEI
[0090] Polymer DPP-BBT (2 mg, 0.0017 mmol), N3-PEG1000-PEI1800 (20 mg, 0.00714 mmol), and cuprous iodide (6 mg, 0.0315 mmol) were added to a 10 mL two-necked flask, followed by the addition of 2 mL of chloroform. The reaction was carried out at 25 °C under nitrogen atmosphere for 48 h. After the reaction was complete, the solvent was removed under reduced pressure. A dark green film of 10 mg was obtained, with a yield of 50%.
[0091] Example 2: Preparation of conjugated polymer self-assembled nanoparticles DPP-BBT-PEI-NPs
[0092] (1) The conjugated polymer DPP-BBT-PEI film was dissolved in 10 ml of water and self-assembled to form nanoparticles;
[0093] (2) Dialyze the nanoparticles for two days using a 10000kDa dialysis bag to remove excess small molecules and solvents;
[0094] (3) Filter with a 220nm filter membrane and store the resulting dark green filtrate at -4℃.
[0095] Figure 2 The images show the UV-Vis absorption spectra of the prepared conjugated polymer and its self-assembly into nanoparticles. The conjugated polymer DPP-BBT-PEI exhibits a strong absorption peak around 870 nm, and after self-assembly into nanoparticles, the strong absorption peak is around 850 nm, indicating that it has a strong near-infrared light absorption capability.
[0096] Figure 3 The image shows the photothermal effect of DPP-BBT-PEI-NPs nanoparticles.
[0097] Figure 4 The image shows a TEM image of DPP-BBT-PEI-NPs nanoparticles, which are spherical with uniform particle size.
[0098] Example 3: Preparation of pH-responsive conjugated polymer nanoparticles PEI / CHO-NPs
[0099] (1) Add CHO-Ph-COO-PEG at concentrations of 0, 1, 2, 3, 4, and 5 mg / mL to a DPP-BBT-PEI-NPs (0.25 mg / mL) solution. 1000-CO-Ph–CHO aqueous solution, the pH of the solution was adjusted to 7.4. After reacting at room temperature for 2 h, PEI / CHO-NPs with a mass ratio of PEI / CHO = 1:(0,4,8,12,16,20) were obtained.
[0100] (2) Dialyze the nanoparticles for two days using a 10000kDa dialysis bag to remove excess small molecules.
[0101] (3) Filter with a 220nm filter membrane and store the resulting dark green filtrate at -4℃.
[0102] Figure 5 The image shows the photothermal effect of PEI / CHO-NPs nanoparticles (PEI / CHO mass ratio = 1:12).
[0103] Figure 6 The image shows a TEM image of PEI / CHO-NPs nanoparticles (PEI / CHO mass ratio = 1:12), which are spindle-shaped with uniform particle size.
[0104] Figure 7 The zeta potential changes for PEI / CHO-NPs with different mass ratios are shown. The zeta potential decreases with increasing CHO-PEG-CHO mass.
[0105] Figure 8 The particle size variation of PEI / CHO-NPs with different mass ratios is shown. The particle size is smallest when the mass ratio of PEI / CHO = 1:12.
[0106] Example 4: Antibacterial application of pH-responsive conjugated polymer nanoparticles
[0107] This embodiment verifies the antibacterial effect by treating bacterial biofilms with pH-responsive nanoparticles and then analyzing their bactericidal effect under 880nm near-infrared light irradiation.
[0108] The specific operation method of this embodiment is as follows:
[0109] 1) Place cell smears pre-soaked in anhydrous ethanol solution into 48-well plates and sterilize with UV light for 1 hour. Then, dilute the washed Staphylococcus aureus (OD600=1) 50-fold and add 500 μL of bacterial suspension to each well of the 48-well plates containing the cell smears. Incubate at 37°C for 48 hours. Then, use a 1 ml syringe to remove the supernatant liquid culture medium and wash three times with sterile water to remove free bacteria, finally obtaining mature Staphylococcus aureus biofilm.
[0110] 2) Add 500 μL of NPs-CHO nanoparticles (PEI / CHO mass ratio = 1:12) to a 48-well plate containing the biofilm to treat the biofilm and incubate for 12 h.
[0111] 3) Wash with sterile water to remove residual nanoparticles, then fix with 2.5% glutaraldehyde for 4 hours, remove the glutaraldehyde, and wash with deionized water.
[0112] 4) Add 120 μL of SYTO-9 / PI dye to each well at a ratio of 1:1. After staining for 15 min, remove the dye and wash twice with deionized water.
[0113] 5) Place the biofilm-containing slide onto a glass slide, cover it with a coverslip, and use a 488nm laser to perform laser confocal microscopy (CLSM) imaging on the sample using SYTO-9 and a 559nm laser to PI.
[0114] As shown in the attached image, via laser confocal laser. Figure 9 As shown, after treatment of the biofilm with pH-responsive nanoparticles PEI / CHO-NPs, the biofilm exhibited overall red fluorescence upon irradiation with near-infrared light, indicating that most bacteria were damaged. This demonstrates that pH-responsive amphiphilic nanoparticles have a significant bactericidal effect and are effective antibacterial materials.
[0115] The present invention has been described in detail above. Those skilled in the art will recognize that the invention can be practiced in a wide range of ways with equivalent parameters, concentrations, and conditions without departing from its spirit and scope, and without requiring unnecessary experiments. While specific embodiments have been provided, it should be understood that further modifications can be made to the invention. In summary, according to the principles of the invention, this application is intended to include any changes, uses, or improvements to the invention, including changes made using conventional techniques known in the art that depart from the scope disclosed herein.
Claims
1. Amphiphilic conjugated polymer nanoparticles PEI-NPs, prepared from the polymer shown in Formula II: In Formula II, R is any one of the following groups: in, express p is an integer between 3 and 10; n = 10 - 50, m = 1 - 50; a = 10 - 50, b = 1 - 50; c = 1 - 50; In Equation II, X+Y=1, and the value of X ranges from 0.1 to 0.9; A represents the degree of polymerization, which is 10-1000.
2. The polymer shown in Formula II of claim 1, having the following structural formula: 。 3. A method for preparing the polymer of formula II according to claim 1 or 2, comprising the following steps: 1) in the presence of a catalyst and a ligand, the compound of formula III undergoes a Stille polycondensation reaction with the compound of formula IV and the compound of formula VI to obtain an intermediate. In Equation III, R1 is , where p is an integer between 3 and 10; 2) The obtained intermediate is reacted with N3-R2 to obtain the polymer shown in Formula II, where R2 represents R removed. The remaining portion.
4. A method for preparing the amphiphilic conjugated polymer nanoparticles PEI-NPs of claim 1, comprising the following steps: (1) dissolving the polymer shown in formula II in an organic solvent, removing the organic solvent by vacuum distillation, and forming a thin film; (2) The obtained film was added to ultrapure water, and an aqueous solution of nanoparticles was obtained by self-assembly. (3) The obtained nanoparticles were obtained by dialysis of the aqueous solution of the nanoparticles.
5. A stimulus-responsive amphiphilic conjugated polymer, prepared by reacting the polymer nanoparticles PEI-NPs and CHO-Ar-COO-PEGd-CO-Ar-CHO under neutral conditions via a Schiff base reaction. In CHO-Ar-COO-PEGd-CO-Ar-CHO, Ar represents a substituted or unsubstituted aromatic group, where... The substituted aromatic group is a C1-C6 alkyl group in which at least one H on the aromatic group is substituted by at least one of halogen, C1-C6 alkyl, C1-C6 alkoxy, or halogen-substituted C1-C6 alkyl. d represents the molecular weight of polyethylene glycol, d = 500-2000.
6. The stimulus-responsive amphiphilic conjugated polymer according to claim 5, characterized in that, The described CHO-Ar-COO-PEGd-CO-Ar-CHO is: CHO-Ph-COO-PEG 1000 -CO- Ph –CHO; The neutral conditions are pH=7.0~8.0, and the mass ratio of PEI-NPs / CHO-Ar-COO-PEGd-CO-Ar-CHO is 1:0~1:20, with the endpoint 0 being unacceptable; The Schiff base reaction was carried out at room temperature for 1-4 hours.
7. Stimulus-responsive polymer-based nanoparticles prepared from the stimulus-responsive amphiphilic conjugated polymer of claim 5 or 6.
8. The use of the amphiphilic conjugated polymer nanoparticles PEI-NPs of claim 1, or the stimulus-responsive amphiphilic conjugated polymer of claim 5 or 6, or the stimulus-responsive polymer-based nanoparticles of claim 7, in the preparation of medicaments for treating bacterial infections.
Citation Information
Patent Citations
Near-infrared IIb fluorescent probe, nano particle and preparation method and application thereof
CN114591729A
Low band gap conjugated polymeric compositions and applications thereof
US20150069302A1