High packing density graphene / Ag-TCNQ materials, preparation methods and applications

By preparing a high-density graphene/Ag-TCNQ composite material, the problems of existing carbon-based catalysts not being able to be directly used as electrode materials and low Faraday efficiency were solved, realizing a highly efficient two-electron oxygen reduction reaction and improving the production rate and Faraday efficiency of hydrogen peroxide.

CN117987849BActive Publication Date: 2026-11-17NANJING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202211332958.1
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2022-10-28
Publication Date
2026-11-17
Estimated Expiration
2042-10-28

AI Technical Summary

Technical Problem

Existing carbon-based catalysts used for the electrochemical synthesis of hydrogen peroxide suffer from problems such as not being able to be directly used as electrode materials and having low Faraday efficiency, making it difficult to achieve efficient two-electron oxygen reduction reactions.

Method used

By preparing a high-density graphene/Ag-TCNQ composite material, a two-dimensional graphene hydrogel membrane was used as a carrier to load zero-dimensional Ag-TCNQ quantum dots. Vacuum filtration and N-methylpyrrolidone solvent treatment were used, combined with capillary compression technology to adjust the packing density and physical absorption area of ​​the material.

Benefits of technology

It achieves highly efficient two-electron oxygen reduction selectivity, improves hydrogen peroxide production and Faraday efficiency, and significantly enhances material stability and catalytic activity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117987849B_ABST
    Figure CN117987849B_ABST
Patent Text Reader

Abstract

This invention discloses a high-packing-density graphene / Ag-TCNQ composite material, its preparation method, and its applications. A two-dimensional graphene hydrogel membrane is used as a carrier, and zero-dimensional Ag-TCNQ quantum dots are loaded onto the carrier. The steps are as follows: Reduced graphene is filtered to form a membrane; the membrane is placed in a mixed solution of water and N-methylpyrrolidone for exchange; the material is placed in a silver nitrate solution and allowed to stand for a period of time, then soaked in water for preservation; the material is then added to an acetonitrile solution containing the organic ligand 7,7,8,8-tetracyano-p-benzoquinone dimethane, and allowed to stand for another period of time. The surface is then washed with acetonitrile to obtain the composite material. This material exhibits excellent electrocatalytic oxygen reduction performance. By controlling the compression degree of the composite material, the number of electrons transferred during the electrochemical reaction process can be controlled, showing broad application prospects in energy, catalysis, and other fields.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention relates to a high packing density graphene / Ag-TCNQ material, belonging to the field of composite material preparation technology. Background Technology

[0002] Hydrogen peroxide (H₂O₂) is a valuable chemical substance widely used in synthesis, degradation of organic pollutants, the semiconductor industry, and the mining industry. Currently, there are four main methods for synthesizing hydrogen peroxide: the anthraquinone method, direct thermocatalytic or photocatalytic synthesis using H₂ and O₂, and the two-electron electrocatalytic oxygen reduction reaction (2e⁻). - ORR). Among these, the anthraquinone process requires multiple reaction / extraction steps, large amounts of Pt / Ni catalyst, and harsh reaction conditions. Direct thermal catalysis and photocatalysis suffer from low activity, insufficient hydrogen peroxide productivity, and fire hazards. In contrast, 2e - ORR has the advantages of simple operation and mild reaction conditions.

[0003] In recent years, many carbon-based catalysts have exhibited electrochemical performance comparable to that of noble metal-based catalysts. - ORR activity. 2e- ... - ORR performance can be modulated by morphology (e.g., nanotubes and nanosheets), pore structure (e.g., micropores, mesopores, macropores), heteroatom doping or modification (e.g., B, N, S, etc.), introduction of small amounts of metal atoms (e.g., Fe, Co, Ni, Ag, etc.), hydrophilicity, and adjustment of electrolyte pH. Transition metal-based tetracyanodimethyl ether (TM-TCNQ) is an emerging electrocatalytic SAC. Theoretical calculations show that TCNQ can increase the positive charge density or spin density of various transition metals (TM = Fe, Co, Ni, Mn), which is beneficial for O2 adsorption and activation. Interfacial TCNQ enhances electron transfer between silver nanoparticles and the glassy carbon electrode (GCE), facilitating the two-electron oxygen reduction reaction.

[0004] A hybrid electrocatalyst composed of Ag-TCNQ nanodots / reduced graphene oxide (rGO) hydrogel was reported in the literature for the electrochemical synthesis of hydrogen peroxide via a two-electron oxygen reduction reaction. The electrocatalyst exhibited a productivity of 0.78 mg / h. -1 The FE content is 71.2%. This catalyst has the problem that it cannot be used directly as an electrode material and has low FE efficiency. By adjusting the packing density of the graphene / Ag-TCNQ composite material, a material that can be directly used as an electrode and has high two-electron oxygen reduction selectivity can be obtained. Summary of the Invention

[0005] The purpose of this invention is to provide a high-packing-density graphene / Ag-TCNQ composite material and its preparation method. This material has high two-electron oxygen reduction selectivity and can be used for efficient electrochemical synthesis of hydrogen peroxide.

[0006] The technical solution to achieve the purpose of this invention is as follows: A high packing density graphene / Ag-TCNQ quantum dot composite material, using a two-dimensional graphene hydrogel film as a carrier, with zero-dimensional Ag-TCNQ quantum dots loaded on the carrier.

[0007] The preparation method of the above-mentioned high packing density graphene / Ag-TCNQ quantum dot composite material includes the following steps: Step 1: After reducing the graphene oxide solution, filter it to obtain a two-dimensional graphene hydrogel membrane. Step 2: Immerse the hydrogel membrane obtained in Step 1 in a mixed solution of water and N-methylpyrrolidone (NMP) for a period of time, and then remove the solvent to obtain a high-density graphene film. Step 3: Immerse the graphene film obtained in Step 2 in silver nitrate solution for a period of time; Step four: Transfer the mixture into an acetonitrile solution containing the organic ligand 7,7,8,8-tetracyano-p-benzoquinone dimethane (TCNQ), let it stand for a period of time, and then clean the surface with acetonitrile to obtain the composite material.

[0008] Preferably, in step one, the concentration of the graphene oxide solution is 0.2 mg / mL.

[0009] Preferably, in step two, the volume ratio of water to N-methylpyrrolidone is 85:15; and the mixture is allowed to stand for at least 12 hours.

[0010] Preferably, in step three, the graphene film is immersed in silver nitrate solution for more than 8 hours.

[0011] Preferably, in step four, the plant should be left to stand for at least 6 hours.

[0012] Compared with the prior art, the present invention has the following significant advantages: 1) The preparation method is simple and has prospects for large-scale application; 2) The small volume makes the material compact and convenient; 3) Comparison of oxygen reduction reaction between compressed graphene and the original material revealed that the compressed graphene is more inclined to selective two-electron reaction. Attached Figure Description

[0013] Figure 1 This is a schematic diagram of the process for preparing high-packing-density rGo / Ag-TCNQ materials according to the present invention.

[0014] Figure 2These are field emission scanning electron microscope (AD) images of materials with different compression degrees prepared in Examples 1-4.

[0015] Figure 3 This is a linear relationship graph between film thickness and packing density of materials with different degrees of compression prepared in the examples.

[0016] Figure 4 This is the X-ray photoelectron spectroscopy full spectrum analysis diagram (ad) of the material prepared in Example 1.

[0017] Figure 5 This is the X-ray diffraction pattern of the material prepared in Example 1.

[0018] Figure 6 The Fourier transform infrared spectrum is that of the material prepared in Example 1.

[0019] Figure 7 These are the Raman spectra of Example 1 and the comparative example.

[0020] Figure 8 The images show the absorption spectra (a) and linear relationship (b) of different concentrations of H2O2 in the electrolyte during electrocatalytic oxygen reduction of the materials in Examples 1-4 of this invention.

[0021] Figure 9 The graphs show the yield and Faraday efficiency of hydrogen peroxide at different potentials in Example 1 (a) and the yield and Faraday efficiency of hydrogen peroxide at the optimal potential in Examples 1-4 (b).

[0022] Figure 10 The results of the RRDE test of the material in Example 1 of this invention in electrocatalytic oxygen reduction are shown in (a) and (b) are the number of electrons transferred by the material in Example 1 at different rotation speeds.

[0023] Figure 11 The figures (a) and (b) are CV graphs of the material in Example 1 of this invention under oxygen and Ar atmospheres, and (c) is a comparison of the CV values ​​after 100 h of testing with those after 5 h of testing. Detailed Implementation

[0024] The present invention will now be described in further detail with reference to the accompanying drawings and specific embodiments.

[0025] In this invention, Ag-TCNQ / rGO films of varying thicknesses were prepared by vacuum filtration and vacuum drying using a H₂O / N-methylpyrrolidone (NMP) mixed solvent. The shrinkage of the reduced graphene oxide gel film was induced by capillary compression, and the film thickness and packing density were adjusted by evaporating NMP from the gel film. The optimized Ag-TCNQ / rGO-85 film exhibited excellent hydrogen peroxide yield and high Faradaic efficiency. Further mechanistic analysis revealed that its excellent 2e⁻ content... - ORR performance stems from the increase in ECSA and physical absorption area caused by capillary compression, providing more 2e - The active site of ORR improves mass transfer and reaction kinetics.

[0026] Combination Figure 1 The method for synthesizing high packing density rGo / Ag-TCNQ composite functional materials used in this invention includes the following steps: Step 1: Filter the graphene into a two-dimensional hydrogel membrane; Step 2: Immerse the hydrogel film extracted in Step 1 in a mixed solution of water and N-methylpyrrolidone (NMP), and then place it in a vacuum oven to remove the volatile solvent. Step 3: Immerse the high-density graphene film obtained in Step 2 in silver nitrate solution for a period of time.

[0027] Step four: Transfer the graphene film from step three into an acetonitrile solution containing the organic ligand 7,7,8,8-tetracyano-p-benzoquinone dimethane, let it stand for a period of time, and then clean the surface with acetonitrile to obtain the composite material.

[0028] Example 1 Step 1: Graphene sheet material is oxidized to obtain graphene oxide, and a 0.2 mg / mL graphene oxide solution is prepared by ultrasonic dispersion in water. Then, a reduced graphene oxide solution is obtained by reduction reaction, and finally, a two-dimensional graphene hydrogel membrane is obtained by vacuum filtration. Step 2: Immerse the hydrogel film extracted in Step 1 in a mixed solution of water and N-methylpyrrolidone (NMP) (H2O / NMP = 85:15) for more than 12 hours, and then place it in a vacuum oven to remove the volatile solvent. Step 3: Immerse the high-density graphene film obtained in Step 2 in silver nitrate solution for more than 8 hours.

[0029] Step four: The graphene film from step three is transferred into an acetonitrile solution containing the organic ligand 7,7,8,8-tetracyano-p-benzoquinone dimethane, and soaked for more than 6 hours. The surface is then cleaned with acetonitrile to obtain the composite material.

[0030] The field emission scanning electron microscope image of the target product rGo / Ag-TCNQ is shown below. Figure 2 As shown in figure a, the compressibility of rGo / Ag-TCNQ was characterized, indicating that the film underwent a compressive effect, and the packing density of the material changed as shown in figure a. Figure 3 As shown; X-ray photoelectron spectroscopy full spectrum analysis is as follows Figure 4 As shown in figures a~d, the obtained rGo / Ag-TCNQ contains four elements: C, O, Ag, and N. The X-ray diffraction pattern is shown below. Figure 5 As shown, the characteristic diffraction peaks of the obtained rGo / Ag-TCNQ and Ag-TCNQ / Ag materials are basically consistent, and both correspond well to the standard spectrum (JCPDS No. 04-0783). Furthermore, there is no significant difference in the peak intensity of the diffraction peaks between the two samples. The Fourier transform infrared spectra are as follows: Figure 6 As shown, TCNQ - The C≡N stretching mode at 2166 and 2189 cm -1 There are two spectral bands at 1507 cm⁻¹. -1 The band at 824 cm⁻¹ corresponds to the C=C stretching mode of the benzene ring in TCNQ, while CH at 824 cm⁻¹... -1 The downward bending mode corresponds to that of Ag-TCNQ nanodots. Raman spectra are as follows... Figure 7 As shown, all the films are at approximately 1340 cm. -1 (D-band) and 1580cm -1 There are two distinct characteristic peaks in the (g-band), which are caused by the in-plane vibrations of defective / disordered carbon and graphite, respectively. The d-band and g-band (I) of the reduced graphene oxide hydrogel film... D / I G The strength ratio of Ag / rGO (1.239) and Ag-TCNQ / rGO (1.242) was 1.104. D / I G The increase in [amount] may indicate an interaction between Ag-TCNQ and rGO.

[0031] Example 2 Step 1: Graphene sheet material is oxidized to obtain graphene oxide, and a 0.2 mg / mL graphene oxide solution is prepared by ultrasonic dispersion in water. Then, a reduced graphene oxide solution is obtained by reduction reaction, and finally, a two-dimensional graphene hydrogel membrane is obtained by vacuum filtration. Step 2: Immerse the hydrogel film extracted in Step 1 in a mixed solution of water and N-methylpyrrolidone (NMP) (H2O / NMP = 0:100) for more than 12 hours, and then place it in a vacuum oven to remove the volatile solvent. Step 3: Immerse the high-density graphene film obtained in Step 2 in silver nitrate solution for more than 8 hours.

[0032] Step four: The graphene film from step three was transferred into an acetonitrile solution containing the organic ligand 7,7,8,8-tetracyano-p-benzodiquinone dimethane and immersed for at least 6 hours. The surface was then washed with acetonitrile to obtain the composite material. The field emission scanning electron microscope image of the obtained target product rGo / Ag-TCNQ is shown below. Figure 2 As shown in b, the compressibility of rGo / Ag-TCNQ was characterized, indicating that the film underwent a compressive effect, and the material's packing density changed as shown in Figure b. Figure 3 As shown.

[0033] Example 3 Step 1: Graphene sheet material is oxidized to obtain graphene oxide, and a 0.2 mg / mL graphene oxide solution is prepared by ultrasonic dispersion in water. Then, a reduced graphene oxide solution is obtained by reduction reaction, and finally, a two-dimensional graphene hydrogel membrane is obtained by vacuum filtration. Step 2: Immerse the hydrogel film extracted in Step 1 in a mixed solution of water and N-methylpyrrolidone (NMP) (H2O / NMP = 50:50) for more than 12 hours, and then place it in a vacuum oven to remove the volatile solvent. Step 3: Immerse the high-density graphene film obtained in Step 2 in silver nitrate solution for more than 8 hours.

[0034] Step four: The graphene film from step three was transferred into an acetonitrile solution containing the organic ligand 7,7,8,8-tetracyano-p-benzodiquinone dimethane and immersed for at least 6 hours. The surface was then washed with acetonitrile to obtain the composite material. The field emission scanning electron microscope image of the obtained target product rGo / Ag-TCNQ is shown below. Figure 2 As shown in c, the compressibility of rGo / Ag-TCNQ was characterized, indicating that the film underwent a compressive effect, and the material's packing density changed as shown in Figure c. Figure 3 As shown.

[0035] Example 4 Step 1: Graphene sheet material is oxidized to obtain graphene oxide, and a 0.2 mg / mL graphene oxide solution is prepared by ultrasonic dispersion in water. Then, a reduced graphene oxide solution is obtained by reduction reaction, and finally, a two-dimensional graphene hydrogel membrane is obtained by vacuum filtration. Step 2: Immerse the hydrogel film extracted in Step 1 in a mixed solution of water and N-methylpyrrolidone (NMP) (H2O / NMP = 100:0) for more than 12 hours, and then place it in a vacuum oven to remove the volatile solvent. Step 3: Immerse the high-density graphene film obtained in Step 2 in silver nitrate solution for more than 8 hours.

[0036] Step four: The graphene film from step three was transferred into an acetonitrile solution containing the organic ligand 7,7,8,8-tetracyano-p-benzodiquinone dimethane and immersed for at least 6 hours. The surface was then washed with acetonitrile to obtain the composite material. The field emission scanning electron microscope image of the obtained target product rGo / Ag-TCNQ is shown below. Figure 2 As shown in d, the compressibility of rGo / Ag-TCNQ is characterized, indicating that the film undergoes a compressive effect, and the material's packing density changes as shown in the figure. Figure 3 As shown.

[0037] Comparative Example 1 Step 1: Prepare a 0.2 mg / mL solution of graphene oxide; Step 2: Add 280 μL of ammonia water and 16.5 μL of hydrazine hydrate to the solution and react at 95 °C for 1 h; Step 3: Filter the reduced graphene solution obtained in Step 2 through a filter membrane to obtain a reduced graphene oxide hydrogel membrane.

[0038] Comparative Example 2 Step 1: Dissolve an appropriate amount of AgNO3 in water and reduce it to elemental Ag using hydrazine hydrate; Step 2: Centrifuge, wash, and freeze-dry the above product; Step 3: Take 100 mg of 7,7,8,8-tetracyano-p-benzoquinone dimethane ligand and dissolve it in 10 ml of acetonitrile; Step 4: Grind the Ag from Step 2 into a fine powder, pour it into the solution from Step 3, and let it stand for 24 hours. Step 5: After the above reaction is complete, gently wash the insoluble matter on the surface with acetonitrile, and finally wash with water and freeze dry.

[0039] Electrochemical two-electron oxygen reduction synthesis of hydrogen peroxide performance test: Electrochemical two-electron oxygen reduction (O2-ORR) tests were conducted under environmental conditions using an H-type electrolytic cell in 0.1 M KOH electrolyte. A Nafion 115 membrane was used to separate the cathode and anode chambers. The cathode used an rGo / Ag-TCNQ thin film. The electrocatalytic performance of the cell in generating hydrogen peroxide from two-electron oxygen was tested at different current densities. All test data were collected without battery internal resistance compensation. Hydrogen peroxide was detected using TiOSO4 colorimetry. The absorbance of the solution was recorded under UV conditions, and the yield of hydrogen peroxide was calculated by converting it to a standard curve in 0.1 M KOH electrolyte. Figure 8 As shown in a and b in the figure. The performance test results of the two-electron oxygen reduction reaction are as follows. Figure 9 As shown, where Figure 9 Figure 'a' shows the hydrogen peroxide production and Faraday efficiency of rGo / Ag-TCNQ-85 at different potentials, with 2e starting at a potential of -0.24V. -ORR( vs. The RHE (hydrogen peroxide) yield was 49.97% Faraday efficiency and 1.47 mg / cm². -2 h -1 Activity increases from -0.24V to 0.16V. vs. The Faraday efficiency of RHE was 90.5%, and the hydrogen peroxide surface yield was 2.05 mg / cm². -2 h -1 Further increase the potential to 0.56V ( vs. Due to the significant hydrogen evolution reaction and four-electron oxygen reduction reaction, the activity of the material (RHE) decreased significantly to 69.62%, and the hydrogen peroxide area yield was 0.79 mg / cm². -2 h -1 . Figure 9 The b in the text includes rGo / Ag-TCNQ-0, rGo / Ag-TCNQ-50, rGo / Ag-TCNQ-85, and rGo / Ag-TCNQ-100 at 0.16 V ( vs. The hydrogen peroxide yield and Faraday efficiency at the RHE potential showed that the area yield and Faraday efficiency increased as the H₂O / NMP ratio increased from 0 to 85 / 15. Further increasing the H₂O / NMP ratio led to performance degradation. In contrast, the volumetric yield of hydrogen peroxide increased rapidly with thinner films. The volumetric yields of Ag-TCNQ / rGO-85 and Ag-TCNQ / rGO-100 were 37.91 and 53.92 g∙cm⁻¹, respectively. -3 h -1 Under capillary compression, their volumetric yields were 6 and 8 times that of the Ag-TCNQ / rGO-0 membrane, respectively. Among them, the rGo / Ag-TCNQ-85 membrane achieved a Faraday efficiency of 90.5% in hydrogen peroxide production, with a yield of 37.91 g / cm³. -3 h -1 .

[0040] To prove that the reaction was a two-electron oxygen reduction reaction, a rotating disk electrode test (RRDE) was performed in the experiment. The test results are as follows: Figure 10 As shown, where Figure 10 In Example 1, 'a' represents a comparison of the number of electrons transferred at different potentials when the rotation speed is 1600 rpm. The number of transferred electrons is consistently around 2, demonstrating that the electrocatalytic reaction is a two-electron oxygen reduction reaction. Figure 10 In the figure, b represents the LSV curve of the material prepared in Example 1 at different rotational speeds. Figure 11 As shown, Figure 11 In the figure, a and b are the LSV and CV curves of the electrochemical reduction of the material under different atmospheres. Figure 11In the figure, 'c' represents the CV curve comparison between the material after 100 hours of testing and the material after 5 hours of testing, demonstrating the stability of the material.

[0041] In the preparation and processing, this invention utilizes vacuum-assisted self-assembly of a reduced graphene oxide (rGO) hydrogel membrane and silver-based tetracyanodimethylethane (Ag-TCNQ) via capillary compression. The resulting Ag-TCNQ / rGO-85 film exhibits significant catalytic activity for the two-electron oxygen reduction reaction.

Claims

1. A high packing density graphene / Ag-TCNQ quantum dot composite material, characterized in that, Zero-dimensional Ag-TCNQ quantum dots were loaded onto a two-dimensional graphene hydrogel membrane as a carrier. Prepared by the following steps: Step 1: After reducing the graphene oxide solution, filter it to obtain a two-dimensional graphene hydrogel membrane. Step 2: Immerse the hydrogel membrane obtained in Step 1 in a mixed solution of water and N-methylpyrrolidone for a period of time, and then remove the solvent to obtain a high-density graphene film. Step 3: Immerse the graphene film obtained in Step 2 in silver nitrate solution for a period of time; Step four: Transfer the mixture into an acetonitrile solution containing the organic ligand 7,7,8,8-tetracyano-p-benzoquinone dimethane (TCNQ), let it stand for a period of time, and then wash the surface with acetonitrile to obtain the composite material.

2. A method for preparing a high packing density graphene / Ag-TCNQ quantum dot composite material, characterized in that, Includes the following steps: Step 1: After reducing the graphene oxide solution, filter it to obtain a two-dimensional graphene hydrogel membrane. Step 2: Immerse the hydrogel membrane obtained in Step 1 in a mixed solution of water and N-methylpyrrolidone for a period of time, and then remove the solvent to obtain a high-density graphene film. Step 3: Immerse the graphene film obtained in Step 2 in silver nitrate solution for a period of time; Step four: Transfer the mixture into an acetonitrile solution containing the organic ligand 7,7,8,8-tetracyano-p-benzoquinone dimethane (TCNQ), let it stand for a period of time, and then wash the surface with acetonitrile to obtain the composite material.

3. The method of claim 2, wherein, In step one, the concentration of the graphene oxide solution is 0.2 mg / mL.

4. The method of claim 2, wherein, In step two, the volume ratio of water to N-methylpyrrolidone is 85:15; let it stand for more than 12 hours.

5. The method as described in claim 2, characterized in that, In step three, the graphene film is immersed in silver nitrate solution for more than 8 hours.

6. The method as described in claim 2, characterized in that, In step four, let it stand for at least 6 hours.