A kind of refining slag for reducing aluminum loss in VD refining process and its preparation method and application

By using refining slag of a specific composition during the VD refining process and adjusting the ratio and particle size of calcium oxide to silicon oxide, the problem of serious aluminum loss is solved, effective control of aluminum content is achieved, the need for aluminum supplementation is reduced, and resource consumption is reduced and production costs, improving product quality.

CN118006867BActive Publication Date: 2024-10-11UNIV OF SCI & TECH BEIJING
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410208907.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-26
Publication Date
2024-10-11
Estimated Expiration
2044-02-26

AI Technical Summary

Technical Problem

During the VD refining process, the aluminum content in the molten steel is severely lost, resulting in aluminum alloy waste and increased production costs, affecting green manufacturing.

Method used

By adding a specific refining slag during the VD refining process, the composition includes K2O, SiO2, CaO, Al2O3 and MgO, adjusting the ratio and particle size of calcium oxide and silicon oxide, forming a new primary crystal phase to reduce SiO2 activity, Reduce the reaction between aluminum and refining slag, thereby controlling the aluminum content in the molten steel.

Benefits of technology

It effectively reduces the loss of aluminum, reduces the need for subsequent aluminum replenishment, reduces resource and energy consumption, reduces production costs, and improves product quality.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of iron and steel metallurgy, and specifically relates to a refining slag for reducing aluminum loss in a VD refining process, a preparation method thereof and an application thereof. A certain amount of K2O is added to an existing VD refining slag system, so that the Al content of molten steel in the refining process can be controlled, the aluminum loss in the refining process is reduced, and the amount of aluminum alloy subsequently supplemented with aluminum to meet the aluminum content requirement of the steel grade is reduced. The invention is simple to operate, can reduce resource and energy consumption, reduce production costs, improve product quality, and is easy to promote and apply.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of iron and steel metallurgy, and in particular to a refining slag for reducing aluminum loss in a VD refining process, and a preparation method and application thereof. Background Art

[0002] VD vacuum refining furnace is widely used in the production of high-quality steel due to its excellent removal of gas impurities in molten steel. In order to accelerate the rapid separation of gas elements dissolved in molten steel from the molten steel during the VD process, high-intensity argon is usually blown from the bottom to provide good kinetic conditions. At the same time, it also makes the contact between molten steel and refined slag more sufficient, and the reaction of slag is more sufficient. Oxidizing components in slag (such as FeO, SiO 2 The aluminum content of the molten steel is as high as 0.070-0.080wt% before VD refining. After VD refining, the aluminum content of the molten steel is 0.008-0.015wt%, and the aluminum recovery rate is only 10-20%, and aluminum needs to be supplemented to meet the Al content requirements in the steel. Therefore, the loss of aluminum in the traditional VD refining process is extremely large, resulting in a waste of aluminum alloys, which is not conducive to green manufacturing and also increases production costs. Summary of the invention

[0003] In order to solve the problems existing in the prior art, the main purpose of the present invention is to provide a refining slag for reducing aluminum loss in the VD refining process and a preparation method and application thereof.

[0004] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:

[0005] A refining slag for reducing aluminum loss in a VD refining process, comprising, by mass percentage, K 2 O: 2.5~5wt%SiO 2 : 8~10wt%, CaO: 47~51wt%, Al 2 O 3 : 27~31wt%, MgO: 4~7wt%, and the rest are inevitable impurities.

[0006] As a preferred solution of the refining slag for reducing aluminum loss in the VD refining process described in the present invention, the mass ratio of calcium oxide to silicon oxide in the refining slag is 4-7.

[0007] As a preferred solution of the refining slag for reducing aluminum loss in the VD refining process of the present invention, wherein: its composition, by mass percentage, includes: K 2 O: 3.5~5wt%SiO 2 : 8.5~9.5wt%, CaO: 47.5~50wt%, Al 2 O 3 : 27.5~30wt%, MgO: 4~6.5wt%, and the rest are inevitable impurities.

[0008] As a preferred solution of the refining slag for reducing aluminum loss in the VD refining process according to the present invention, wherein: K 2 O by K 2 O powder may decompose K 2 O's salt is provided.

[0009] As a preferred solution of the refining slag for reducing aluminum loss in the VD refining process described in the present invention, the average particle size of the refining slag is 1 to 5 mm.

[0010] To solve the above technical problem, according to another aspect of the present invention, the present invention provides the following technical solution:

[0011] A method for preparing the above-mentioned refining slag for reducing aluminum loss in the VD refining process comprises weighing silicon oxide powder, calcium oxide powder, aluminum oxide powder, magnesium oxide powder and potassium oxide powder or a powder that can be decomposed into K according to the mass percentage of the composition of the refining slag. 2 O salt (such as potassium carbonate), after processing and grinding to a particle size of ≤3mm, is mixed and stirred evenly, and after pre-melting and crushing, a refining slag that reduces aluminum loss in the VD refining process is obtained.

[0012] To solve the above technical problem, according to another aspect of the present invention, the present invention provides the following technical solution:

[0013] A VD refining method for cold heading steel, adding 8-10 kg / t 钢 The above-mentioned refining slag reduces aluminum loss during VD refining.

[0014] As a preferred solution of the VD refining method for cold heading steel described in the present invention, the aluminum yield in the VD refining process is ≥26%.

[0015] The beneficial effects of the present invention are as follows:

[0016] The present invention provides a refining slag for reducing aluminum loss in the VD refining process, and a preparation method and application thereof. A certain amount of K is added to the existing VD refining slag system. 2O, so that the Al content of the molten steel during the refining process can be effectively controlled, the aluminum loss during the refining process is reduced, and the amount of aluminum alloy that is subsequently supplemented with aluminum to meet the aluminum content requirements of the steel grade is reduced. The present invention is simple to operate, can reduce resource and energy consumption, reduce production costs, improve product quality, and is easy to promote and apply. DETAILED DESCRIPTION

[0017] The following will be described clearly and completely in conjunction with the technical solutions in the embodiments. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] The main purpose of the present invention is to provide a refining slag for reducing aluminum loss in the VD refining process and its preparation method and application, which can reduce the aluminum loss problem in the VD refining process and control the Al content of the molten steel after the refining process.

[0019] According to one aspect of the present invention, the present invention provides the following technical solution:

[0020] A refining slag for reducing aluminum loss in a VD refining process, comprising, by mass percentage, K 2 O: 2.5~5wt%SiO 2 : 8~10wt%, CaO: 47~51wt%, Al 2 O 3 : 27~31wt%, MgO: 4~7wt%, and the rest are inevitable impurities.

[0021] K 2 O is a strong alkaline oxide, and it reacts with the acidic oxide SiO 2 The binding ability is stronger than MgO and Al 2 O 3 The primary phase of the pre-melted refined slag can be changed from pyroxene (2CaO·MgO·2SiO 2 -2CaO·Al 2 O 3 ·SiO 2 ) is transformed into magnesium-aluminum spinel phase (MgO·Al 2 O 3 ), that is, SiO in the refined slag 2 The content is relatively reduced, making the SiO 2 The activity of steel slag is reduced, according to the reaction of Al in steel slag with SiO 2 It can be seen from the reaction that Al in the molten steel is not easy to react with the refined slag, thereby increasing the Al content in the molten steel.

[0022] Preferably, the mass ratio of calcium oxide to silicon oxide in the refining slag for reducing aluminum loss during VD refining is 4-7.

[0023] Preferably, its composition, by mass percentage, includes: K 2 O: 3.5~5wt%SiO 2 : 8.5~9.5wt%, CaO: 47.5~50wt%, Al 2 O 3 : 27.5~30wt%, MgO: 4~6.5wt%, and the rest are inevitable impurities.

[0024] Preferably, K 2 O by K 2 O powder may decompose K 2 O's salt is provided.

[0025] Preferably, the average particle size of the refining slag for reducing aluminum loss during VD refining is 1 to 5 mm.

[0026] According to another aspect of the present invention, the present invention provides the following technical solution:

[0027] A method for preparing the above-mentioned refining slag for reducing aluminum loss in the VD refining process comprises weighing silicon oxide powder, calcium oxide powder, aluminum oxide powder, magnesium oxide powder and potassium oxide powder or a K-containing powder that can be decomposed at high temperature according to the mass percentage of the composition of the refining slag. 2 O salt (such as potassium carbonate), after processing and grinding to a particle size of ≤3mm, is mixed and stirred evenly, and after pre-melting and crushing, a refining slag that reduces aluminum loss in the VD refining process is obtained.

[0028] According to another aspect of the present invention, the present invention provides the following technical solution:

[0029] A VD refining method for cold heading steel, adding 8-10 kg / t 钢 The above-mentioned refining slag reduces aluminum loss during VD refining.

[0030] Preferably, the aluminum yield in the VD refining process is ≥26%.

[0031] The technical solution of the present invention is further described below in conjunction with specific embodiments.

[0032] Example 1

[0033] A VD refining method for cold heading steel, wherein the aluminum content of the molten steel before refining is 0.0652wt%, and 10kg / t 钢 The composition of the refining slag for reducing aluminum loss in the VD refining process is calculated by mass percentage, including: K 2O: 4.97wt%, SiO 2 :8.86wt%, CaO: 47.66wt%, Al 2 O 3 : 27.93wt%, MgO: 5.62wt%, and the rest are inevitable impurities. The mass ratio of calcium oxide to silicon oxide in the refined slag is 5.38, and the average particle size is 1-5mm.

[0034] The aluminum content of the molten steel after treatment in this embodiment is 0.017wt%, and the aluminum yield is 28%.

[0035] Example 2

[0036] A VD refining method for cold heading steel, wherein the aluminum content of the molten steel before refining is 0.0652wt%, and 8kg / t 钢 The composition of the refining slag for reducing aluminum loss in the VD refining process is calculated by mass percentage, including: K 2 O: 3.79wt%, SiO 2 :9.22wt%, CaO: 49.23wt%, Al 2 O 3 : 29.87wt%, MgO: 4.36wt%, and the rest are inevitable impurities. The mass ratio of calcium oxide to silicon oxide in the refined slag is 5.34, and the average particle size is 1-5mm.

[0037] The aluminum content of the molten steel after treatment in this embodiment is 0.016wt%, and the aluminum recovery rate is 26%.

[0038] Example 3

[0039] A VD refining method for cold heading steel, wherein the aluminum content of the molten steel before refining is 0.0652wt%, and 10kg / t 钢 The composition of the refining slag for reducing aluminum loss in the VD refining process is calculated by mass percentage, including: K 2 O: 2.97wt%, SiO 2 :8.99wt%, CaO: 47.65wt%, Al 2 O 3 : 28.33wt%, MgO: 6.10wt%, and the rest are inevitable impurities. The mass ratio of calcium oxide to silicon oxide in the refined slag is 5.30, and the average particle size is 1-5mm.

[0040] The aluminum content of the molten steel after treatment in this embodiment is 0.016wt%, and the aluminum recovery rate is 26%.

[0041] Comparative Example 1

[0042] A VD refining method for cold heading steel, wherein the aluminum content of the molten steel before refining is 0.0652wt%, and 10kg / t 钢 The composition of the refined slag, measured by mass percentage, includes SiO 2 :9.92wt%, CaO: 50.13wt%, Al 2 O 3 : 30.06wt%, MgO: 5.24wt%, and the rest are inevitable impurities. The mass ratio of calcium oxide to silicon oxide in the refined slag is 5.05, and the average particle size is 1-5mm.

[0043] The aluminum content of the molten steel after treatment in this comparative example is 0.012wt%, and the aluminum recovery rate is 20%.

[0044] Comparative Example 2

[0045] A VD refining method for cold heading steel, wherein the aluminum content of the molten steel before refining is 0.0652wt%, and 10kg / t 钢 The composition of the refined slag is calculated by mass percentage, including: K 2 O: 1.25wt%, SiO 2 :9.72wt%, CaO: 49.22wt%, Al 2 O 3 : 30.00wt%, MgO: 4.93wt%, and the rest are inevitable impurities. The mass ratio of calcium oxide to silicon oxide in the refined slag is 5.07, and the average particle size is 1-5mm.

[0046] The aluminum content of the molten steel after treatment in this embodiment is 0.013wt%, and the aluminum yield is 21%.

[0047] Comparative Example 3

[0048] A VD refining method for cold heading steel, wherein the aluminum content of the molten steel before refining is 0.0652wt%, and 10kg / t 钢 The composition of the refined slag is calculated by mass percentage, including: K 2 O: 2.10wt%, SiO 2 :9.32wt%, CaO: 49.02wt%, Al 2 O 3 : 30.55wt%, MgO: 5.02wt%, and the rest are inevitable impurities. The mass ratio of calcium oxide to silicon oxide in the refined slag is 5.26, and the average particle size is 1-5mm.

[0049] The aluminum content of the molten steel after treatment in this embodiment is 0.014wt%, and the aluminum yield is 23%.

[0050] It can be seen from the above embodiments and comparative examples that the present invention adds a certain amount of K 2 The novel slag system obtained by the present invention can effectively control the Al content of the molten steel during the refining process, reduce the aluminum loss during the refining process, and reduce the amount of aluminum alloy that is subsequently supplemented with aluminum to meet the aluminum content requirements of the steel grade. The present invention is simple to operate, can reduce resource and energy consumption, reduce production costs, improve product quality, and is easy to promote and apply.

[0051] The above description is only a preferred embodiment of the present invention, and does not limit the patent scope of the present invention. All equivalent structural changes made by using the contents of the present invention specification under the inventive concept of the present invention, or directly / indirectly applied in other related technical fields are included in the patent protection scope of the present invention.

Claims

1. A refining slag for reducing aluminum loss in VD refining process, Features: Its composition, by mass percentage, includes: K 2 O: 2.97~5wt%, SiO 2 : 8~10wt%, CaO: 47~51wt%, Al 2 O 3 : 27~31wt%, MgO: 4~7wt%, and the rest are inevitable impurities; the aluminum recovery rate in the VD refining process is ≥26%.

2. The refining slag for reducing aluminum loss in VD refining process according to claim 1, Features: The mass ratio of calcium oxide to silicon oxide in the refined slag is 4-7.

3. The refining slag for reducing aluminum loss in VD refining process according to claim 1, Features: Its composition, by mass percentage, includes: K 2 O: 3.5~5wt%, SiO 2 : 8.5~9.5wt%, CaO: 47.5~50wt%, Al 2 O 3 : 27.5~30wt%, MgO: 4~6.5wt%, and the rest are inevitable impurities.

4. The refining slag for reducing aluminum loss in VD refining process according to claim 1, Features: K 2 O by K 2 O powder may decompose K 2 O's salt is provided.

5. The refining slag for reducing aluminum loss in VD refining process according to claim 1, Features: The average particle size of the refined slag is 1-5 mm.

6. A method for preparing a refining slag for reducing aluminum loss in a VD refining process according to any one of claims 1 to 4, Features The preparation method comprises the following steps: according to the mass percentage of the composition of the refined slag, weighing silicon oxide powder, calcium oxide powder, aluminum oxide powder, magnesium oxide powder and potassium oxide powder or potassium oxide powder that can be decomposed into K 2 The salt of VD is processed and ground to a particle size of ≤3mm, then mixed and stirred evenly, and after pre-melting and crushing, the refined slag for reducing aluminum loss in the VD refining process is obtained.

7. A VD refining method for cold heading steel, It is characterized in that Add 8~10kg / t during VD refining process 钢 The refining slag for reducing aluminum loss in VD refining process according to any one of claims 1 to 4.

Citation Information

Cited By

  • VD vacuum refining method for inhibiting manganese loss and strengthening degassing

    CN121250026A