High-plasticity soluble magnesium alloys and their preparation methods

By preparing a highly ductile soluble magnesium alloy, the problem of incomplete dissolution of soluble rubber in high-temperature mines has been solved, enabling controlled dissolution at high temperatures and low-cost application of magnesium alloys, suitable for components such as bridge plugs and packer sealing rings.

CN118006990BActive Publication Date: 2026-11-10LONGNAN LONGYI HEAVY RARE EARTH TECH CO LTD +1
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410101747.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-25
Publication Date
2026-11-10
Estimated Expiration
2044-01-25

AI Technical Summary

Technical Problem

Existing soluble rubber sealing components do not dissolve completely or at a slow rate in high-temperature mines, which may clog the shaft, causing delays in the mining process and increased costs. Furthermore, the existing high-plasticity soluble magnesium alloys are expensive to manufacture and difficult to industrialize.

Method used

The high-plasticity soluble magnesium alloy comprises 0.7%-1.2% Al, 1.1%-2.2% Zn, 0.7%-1.5% Ni and 0.1%-0.5% X (X is selected from Ca, Gd, Ce and Sm). The magnesium alloy is prepared by melting, electromagnetic semi-continuous casting and extrusion molding processes, and the dissolution rate is controlled.

Benefits of technology

The prepared high-plasticity soluble magnesium alloy exhibits excellent plasticity and a controllable dissolution rate in high-temperature mines. It can be completely dissolved without secondary drilling and milling, resulting in low cost. It is suitable for components such as bridge plugs and packer sealing rings.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118006990B_ABST
    Figure CN118006990B_ABST
Patent Text Reader

Abstract

This invention discloses a high-plasticity soluble magnesium alloy and its preparation method. The magnesium alloy comprises, by mass percentage: 0.7%-1.2% Al, 1.1%-2.2% Zn, 0.7%-1.5% Ni, 0.1%-0.5% X, with the balance being Mg. The X is selected from one or more of Ca, Gd, Ce, and Sm. The high-plasticity soluble magnesium alloy of this invention exhibits excellent service plasticity and moderate strength. Compared to soluble rubber, the dissolution rate of this soluble magnesium alloy in the service environment is controllable, allowing for complete dissolution without clogging the wellbore and eliminating the need for secondary drilling and milling. It can replace soluble rubber in components such as bridge plug slips and sealing rings. The preparation method of this high-plasticity soluble magnesium alloy is simple, low-cost, and has great potential for industrial-scale production.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This invention belongs to the field of metallic materials technology, specifically relating to a highly ductile soluble magnesium alloy and its preparation method. Background Technology

[0002] Existing soluble fracturing plugs and packers mainly use rubber as their sealing element. However, rubber does not dissolve completely or at a slow rate in high-temperature mines, which may clog the shaft and require additional drilling and milling, thus delaying the mining process and increasing mining costs.

[0003] Chinese patent CN114411029A discloses a highly ductile, rapidly degradable Mg-Li-Gd-Ni alloy and its preparation method. The chemical composition, by mass percentage, includes: Gd: 1.0%–10.0%, Ni: 0.2%–2.0%, Li: 5.5%–10.0%, with the remainder being Mg and unavoidable impurities, the total impurity content being less than or equal to 0.3%. While this highly ductile, rapidly degradable Mg-Li-Gd-Ni alloy exhibits high elongation, its preparation process requires a vacuum induction furnace and necessitates the use of numerous expensive magnesium-lithium master alloys and magnesium-gadolinium master alloys, resulting in high production costs, low market acceptance, and difficulty in large-scale industrial production.

[0004] Chinese Patent Publication No. CN113667871A discloses a highly ductile soluble magnesium-lithium alloy, its preparation method, and its applications. The alloy is composed of the following components by mass percentage: Li: 9.0%–12.0%, Al: 0–2.5%, Zn: 0.1%–1.0%, Ni: 0.1%–1.0%, Cu: 0.2%–1.0%, RE≤1.0%, and the balance being Mg. This invention also uses a relatively large amount of magnesium-lithium master alloy in its preparation process, resulting in high production costs.

[0005] Therefore, in view of the above-mentioned technical problems, it is necessary to provide a highly ductile soluble magnesium alloy that can replace soluble rubber.

[0006] The information disclosed in this background section is intended only to enhance the understanding of the overall background of the invention and should not be construed as an admission or in any way implying that the information constitutes prior art known to those skilled in the art. Summary of the Invention

[0007] The purpose of this invention is to provide a highly ductile soluble magnesium alloy and its preparation method, which exhibits excellent plasticity and a controllable dissolution rate in high-temperature mines.

[0008] To achieve the above objectives, a specific embodiment of the present invention provides the following technical solution: a highly ductile soluble magnesium alloy, wherein the alloy comprises, by mass percentage: 0.7%-1.2% Al, 1.1%-2.2% Zn, 0.7%-1.5% Ni, 0.1%-0.5% X, with the balance being Mg, wherein X is selected from one or more of Ca, Gd, Ce and Sm.

[0009] In one or more embodiments of the present invention, the magnesium alloy comprises, by mass percentage: 0.7% Al, 2.2% Zn, 0.1% Ca, 0.7% Ni, with the balance being Mg.

[0010] In one or more embodiments of the present invention, the magnesium alloy comprises, by mass percentage: 1.0% Al, 2.0% Zn, 0.2% Ca, 1.5% Ni, 0.2% Gd, with the balance being Mg.

[0011] In one or more embodiments of the present invention, the magnesium alloy comprises, by mass percentage: 0.9% Al, 1.1% Zn, 0.2% Ca, 0.7% Ni, 0.3% Ce, with the balance being Mg.

[0012] In one or more embodiments of the present invention, the magnesium alloy comprises, by mass percentage: 1.2% Al, 1.6% Zn, 0.2% Ca, 1.2% Ni, 0.1% Gd, 0.2% Sm, with the balance being Mg.

[0013] Another embodiment of the present invention provides the following technical solution: a method for preparing a highly ductile soluble magnesium alloy, comprising:

[0014] Raw material proportions: Weigh magnesium ingots, aluminum ingots, zinc ingots, magnesium-nickel master alloys, and materials containing X according to the following mass percentages: Al: 0.7%-1.2%, Zn: 1.1%-2.2%, Ni: 0.7%-1.5%, X: 0.1%-0.5%, and the balance being Mg.

[0015] Melting and casting: The magnesium ingots, aluminum ingots and zinc ingots are placed in a pit-type resistance furnace and held at 740℃-750℃ until completely melted. Then, a magnesium-nickel master alloy is added at 720℃-740℃ and stirred until completely melted. The melt temperature is controlled at 710℃-720℃ and then a material containing X is added. After stirring evenly, the temperature is controlled at 700℃-710℃ to obtain a soluble magnesium alloy melt. Then, magnesium alloy ingots are obtained using electromagnetic semi-continuous casting technology.

[0016] Homogenization treatment: The magnesium alloy ingot is kept at 370℃-410℃ for 18 hours;

[0017] Extrusion molding: The homogenized magnesium alloy ingot is held at 110℃~230℃ for a period of time and then extruded to obtain magnesium alloy rods. The magnesium alloy rods are then cooled with water to obtain soluble magnesium alloy.

[0018] In one or more embodiments of the present invention, the material containing X is selected from one or more of magnesium-calcium master alloy, magnesium-gadolinium master alloy, magnesium-cerium master alloy and magnesium-samarium master alloy.

[0019] In one or more embodiments of the present invention, during the electromagnetic semi-continuous casting process, the electromagnetic frequency of the electromagnetic stirring is between 15Hz and 30Hz, and the electromagnetic stirring current is between 100A and 120A.

[0020] In one or more embodiments of the present invention, the heat preservation time of the extrusion molding is between 3h and 4h.

[0021] In one or more embodiments of the present invention, the extrusion speed of the extrusion molding is between 0.5 mm / s and 5 mm / s.

[0022] Compared with existing technologies, the high-plasticity soluble magnesium alloy of this invention exhibits excellent service plasticity, moderate strength, and a simple and low-cost production process. Compared to soluble rubber, the dissolution rate of this soluble magnesium alloy in the service environment is controllable, allowing for complete dissolution without clogging the wellbore and eliminating the need for secondary drilling and milling. It can replace soluble rubber in components such as bridge plug slips and sealing rings. The preparation method of the high-plasticity soluble magnesium alloy of this invention is simple, low-cost, and has great potential for industrial-scale production. Attached Figure Description

[0023] To more clearly illustrate the technical solutions in the embodiments of the present invention or the prior art, the drawings used in the description of the embodiments or the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For those skilled in the art, other drawings can be obtained based on these drawings without creative effort.

[0024] Figure 1 This is a schematic flowchart of a method for preparing a highly ductile soluble magnesium alloy according to an embodiment of the present invention;

[0025] Figure 2 The room temperature engineering stress-strain diagrams are of the high-plasticity soluble magnesium alloys of Examples 1-4 and Comparative Examples 1-2 of this invention.

[0026] Figure 3 The stress-strain diagrams of the high-plasticity soluble magnesium alloys of Examples 1-4 and Comparative Examples 1-2 of the present invention at a high temperature of 93°C are shown. Detailed Implementation

[0027] To enable those skilled in the art to better understand the technical solutions of this invention, the technical solutions of the embodiments of this invention will be clearly and completely described below with reference to the accompanying drawings. Obviously, the described embodiments are only some embodiments of this invention, and not all embodiments. Based on the embodiments of this invention, all other embodiments obtained by those skilled in the art without creative effort should fall within the scope of protection of this invention.

[0028] In one embodiment of the present invention, the high plasticity soluble magnesium alloy comprises, by mass percentage, 0.7%-1.2% Al, 1.1%-2.2% Zn, 0.7%-1.5% Ni, 0.1%-0.5% X, with the balance being Mg, wherein X is selected from one or more of Ca, Gd, Ce and Sm.

[0029] The addition of Al is controlled between 0.7 wt.% and 1.2 wt.%. When the Al addition is less than 0.7 wt.%, the strength of the alloy may not be very high, while when the addition is greater than 1.2 wt.%, the Mg content in the alloy... 17 Al 12 A higher concentration of certain phases can affect the plasticity of the alloy.

[0030] The amount of Zn added should be controlled between 1.1 wt.% and 2.2 wt.%. When the amount of Zn added is greater than 2.2 wt.%, the dissolution rate of the magnesium alloy will be slower, and when the amount added is less than 1.1 wt.%, the hot cracking sensitivity of the alloy will increase, making casting more difficult.

[0031] By controlling the amount of Ni added between 0.7 wt.% and 1.5 wt.%, the dissolution rate of the alloy will be neither too high nor too low, while also ensuring certain mechanical properties.

[0032] The addition of Ca, Gd, Ce, and Sm, alone or in combination, can weaken the texture, promote non-basal slip, and improve the plasticity of soluble magnesium alloys. However, the addition of Ca, Gd, Ce, and Sm should not be too high, and the total addition should be controlled below 0.5 wt.%. Excessive addition will lead to a decrease in plasticity, while the effect will be poor if the addition is below 0.1 wt.%.

[0033] Preferably, in one embodiment of the present invention, the high plasticity soluble magnesium alloy comprises, by mass percentage: 0.7% Al, 2.2% Zn, 0.1% Ca, 0.7% Ni, with the balance being Mg.

[0034] Preferably, in one embodiment of the present invention, the high plasticity soluble magnesium alloy comprises, by mass percentage: 1.0% Al, 2.0% Zn, 0.2% Ca, 1.5% Ni, 0.2% Gd, with the balance being Mg.

[0035] Preferably, in one embodiment of the present invention, the high plasticity soluble magnesium alloy comprises, by mass percentage: 0.9% Al, 1.1% Zn, 0.2% Ca, 0.7% Ni, 0.3% Ce, with the balance being Mg.

[0036] Preferably, in one embodiment of the present invention, the high-plasticity soluble magnesium alloy comprises, by mass percentage: 1.2% Al, 1.6% Zn, 0.2% Ca, 1.2% Ni, 0.1% Gd, 0.2% Sm, with the balance being Mg.

[0037] like Figure 1 As shown, a method for preparing a highly ductile soluble magnesium alloy according to an embodiment of the present invention includes steps S1-S4.

[0038] Step S1: Raw material ratio: Weigh magnesium ingots, aluminum ingots, zinc ingots, magnesium-nickel master alloy and materials containing X according to the following ratios: Al: 0.7%-1.2%, Zn: 1.1%-2.2%, Ni: 0.7%-1.5%, X: 0.1%-0.5% and the balance being the mass percentage of Mg.

[0039] Specifically, in step S1, magnesium ingots, aluminum ingots, zinc ingots, magnesium-nickel master alloys, and materials containing X are weighed according to the following mass percentages: Al: 0.7%-1.2%, Zn: 1.1%-2.2%, Ni: 0.7%-1.5%, X: 0.1%-0.5%, and the balance being Mg. The materials containing X are selected from one or more of magnesium-calcium master alloys, magnesium-gadolinium master alloys, magnesium-cerium master alloys, and magnesium-samarium master alloys.

[0040] Specifically, the master alloys for magnesium and nickel are Mg-20Ni, for magnesium and gadolinium they are Mg-30Gd, for magnesium and calcium they are Mg-30Ca, for magnesium and cerium they are Mg-30Ce, and for magnesium and samarium they are Mg-30Sm.

[0041] Step S2: Melting and casting: Magnesium ingots, aluminum ingots and zinc ingots are placed in a pit-type resistance furnace and held at 740℃-750℃ until completely melted. Then, magnesium-nickel master alloy is added at 720℃-740℃ and stirred until completely melted. The melt temperature is controlled at 710℃~720℃ and then materials containing X are added. After stirring evenly, the temperature is controlled at 700℃-710℃ to obtain a soluble magnesium alloy melt. Then, magnesium alloy ingots are obtained using electromagnetic semi-continuous casting technology.

[0042] Specifically, in step S2, firstly, magnesium ingots, aluminum ingots, and zinc ingots are placed in a pit-type resistance furnace and held at 740℃-750℃ until completely melted. Secondly, a magnesium-nickel master alloy is added and stirred until completely melted at a temperature of 720℃-740℃. Next, the melt temperature is controlled at 710℃-720℃, and a material containing X is added. After stirring evenly, the temperature is controlled at 700℃-710℃ to obtain a soluble magnesium alloy melt. Finally, a magnesium alloy ingot is obtained using electromagnetic semi-continuous casting technology. During the casting process, an electromagnetic frequency of 15Hz-30Hz is set to electromagnetically stir the soluble magnesium alloy melt and the ingot. Simultaneously, the electromagnetic stirring current is between 100A and 120A.

[0043] When adding materials containing X, the melt temperature in the resistance furnace needs to be measured to ensure that the melt temperature is controlled between 710℃ and 720℃ before adding material X. If the temperature is too high, the yield of materials containing X will be significantly lower than expected. Furthermore, the electromagnetic frequency and current are ideal parameters obtained through multiple experimental tests. Due to differences in the added elements, the hot cracking susceptibility of the alloy varies; therefore, appropriate electromagnetic parameters are required to ensure the smooth progress of the casting process.

[0044] Step S3: Homogenization treatment: Hold the magnesium alloy ingot at 370℃-410℃ for 18 hours.

[0045] Specifically, in step S3, the magnesium alloy ingot is held at 370℃-410℃ for 18 hours. Homogenization treatment of the aluminum alloy ingot can improve alloy segregation and make the microstructure of the magnesium alloy more uniform.

[0046] Step S4: Extrusion molding: After homogenization treatment, the magnesium alloy ingot is held at 110℃~230℃ for a period of time and then extruded to obtain magnesium alloy rods. The magnesium alloy rods are then cooled with water to obtain soluble magnesium alloy.

[0047] Specifically, in step S4, the homogenized magnesium alloy ingot is machined into a cylinder with a diameter of Φ78mm*300mm. Then, after holding at 110℃~230℃ for 3-4 hours, it is extruded at an extrusion speed of 0.5mm / s-5mm / s to obtain a magnesium alloy rod. The magnesium alloy rod is then cooled with water to obtain a soluble magnesium alloy. The extrusion ratio is 6.7.

[0048] The extrusion speed of magnesium alloys should not exceed 5 mm / s, and the temperature should not exceed 230℃. If the speed and temperature are too high, cracks and burrs will appear on the surface of the extruded material, and the mechanical properties will be unsatisfactory. The extrusion speed should not be lower than 0.5 mm / s, and the temperature should not be lower than 110℃. If the temperature and speed are too low, the extruded bar will basically be an incompletely recrystallized structure with low room temperature plasticity.

[0049] The present invention will be further described below with reference to embodiments and comparative examples.

[0050] Example 1

[0051] The soluble magnesium alloy of Example 1 is composed of the following elements by mass percentage: 0.7% Al, 2.2% Zn, 0.1% Ca, 0.7% Ni, with the balance being Mg.

[0052] Raw material proportions: Weigh magnesium ingots, aluminum ingots, zinc ingots, magnesium-nickel master alloy and magnesium-calcium master alloy according to the proportions.

[0053] Melting and casting: Magnesium ingots, aluminum ingots, and zinc ingots are placed in a pit-type resistance furnace and held at 750℃ until completely melted. Then, a magnesium-nickel master alloy is added at 720℃ and stirred until completely melted. A magnesium-calcium master alloy is then added at 720℃ and stirred until homogeneous. The melt temperature is then controlled at 710℃ to obtain a soluble magnesium alloy melt. Magnesium alloy ingots are obtained using electromagnetic semi-continuous casting technology. During the casting process, an electromagnetic frequency of 15Hz is set to electromagnetically stir the melt and ingots. The current of the electromagnetic system is 100A during electromagnetic stirring.

[0054] Homogenization treatment: The magnesium alloy ingot is kept at 370℃ for 18 hours.

[0055] Extrusion molding: The homogenized magnesium alloy ingot is machined into a cylinder with a diameter of 78mm and a diameter of 300mm, and then extruded after being held at 110℃ for 3 hours; the obtained magnesium alloy rod is cooled with water to obtain soluble magnesium alloy.

[0056] The prepared soluble magnesium alloy was subjected to mechanical property testing and degradation rate testing according to GB / T228.1-2010 Metallic Materials - Tensile Testing.

[0057] Test results: Elongation at room temperature: 22%, tensile strength: 260 MPa, yield strength: 220 MPa.

[0058] Elongation at 93℃: 40%, tensile strength: 235MPa, yield strength: 188MPa.

[0059] The dissolution rate in 93℃ and 3.0% KCl reached 30 mg*cm. -2 *h -1 .

[0060] Example 2

[0061] The soluble magnesium alloy of Example 2 is composed of the following elements by mass percentage: 1.0% Al, 2.0% Zn, 0.2% Ca, 0.2% Gd and 1.5% Ni, with the balance being Mg.

[0062] Raw material proportions: Weigh magnesium ingots, aluminum ingots, zinc ingots, magnesium-nickel master alloy, magnesium-calcium master alloy, and magnesium-gadolinium master alloy according to the proportions.

[0063] Melting and casting: Magnesium ingots, aluminum ingots, and zinc ingots are placed in a pit-type resistance furnace and held at 750°C until completely melted. Then, magnesium-nickel master alloy is added at a temperature controlled at 730°C and stirred until completely melted. Magnesium-calcium master alloy and magnesium-gadolinium master alloy are then added at a temperature controlled at 710°C and stirred evenly. The melt temperature is then controlled at 710°C to obtain a soluble magnesium alloy melt. Magnesium alloy ingots are obtained using electromagnetic semi-continuous casting technology. During the casting process, an electromagnetic frequency of 20Hz is set to electromagnetically stir the melt and ingots. The current of the electromagnetic system is 105A during electromagnetic stirring.

[0064] Homogenization treatment: The magnesium alloy ingot is kept at 390℃ for 18 hours.

[0065] Extrusion molding: The homogenized magnesium alloy ingot is machined into a cylinder with a diameter of 78mm and a diameter of 300mm, and then extruded after being kept at 230℃ for 4 hours; the obtained magnesium alloy rod is cooled with water to obtain soluble magnesium alloy.

[0066] The prepared soluble magnesium alloy was subjected to mechanical property testing and degradation rate testing according to GB / T228.1-2010 Metallic Materials - Tensile Testing.

[0067] Test results: Elongation at room temperature: 25%, tensile strength: 240 MPa, yield strength: 200 MPa.

[0068] Elongation at 93℃: 50%, tensile strength: 220MPa, yield strength: 175MPa.

[0069] The dissolution rate in 93℃ and 3.0% KCl reached 60 mg*cm. -2 *h -1 .

[0070] Example 3

[0071] The soluble magnesium alloy of Example 3 is composed of the following elements by mass percentage: 0.9% Al, 1.1% Zn, 0.2% Ca, 0.3% Ce and 0.9% Ni, with the balance being Mg.

[0072] Raw material proportions: Weigh magnesium ingots, aluminum ingots, zinc ingots, magnesium-nickel master alloy, magnesium-calcium master alloy and magnesium-cerium master alloy according to the proportions.

[0073] Melting and casting: Magnesium ingots, aluminum ingots, and zinc ingots are placed in a pit-type resistance furnace and held at 750°C until completely melted. The addition temperature is controlled at 730°C, then magnesium-nickel master alloy is added and stirred until completely melted. The melt temperature is then controlled at 720°C, and magnesium-calcium master alloy and magnesium-cerium master alloy are added. After stirring evenly, the melt temperature is controlled at 720°C to obtain a soluble magnesium alloy melt. Magnesium alloy ingots are obtained using electromagnetic semi-continuous casting technology. During the casting process, an electromagnetic frequency of 20Hz is set to electromagnetically stir the melt and ingot. The current of the electromagnetic system is 110A during electromagnetic stirring.

[0074] Homogenization treatment: The magnesium alloy ingot is held at 410℃ for 18 hours.

[0075] Extrusion molding: The homogenized magnesium alloy ingot is machined into a cylinder with a diameter of 78mm and a diameter of 300mm, and then extruded after being kept at 180℃ for 3 hours; the obtained magnesium alloy rod is cooled with water to obtain soluble magnesium alloy.

[0076] The prepared soluble magnesium alloy was subjected to mechanical property testing and degradation rate testing according to GB / T228.1-2010 Metallic Materials - Tensile Testing.

[0077] Test results: Elongation at room temperature: 28%, tensile strength: 230 MPa, yield strength: 195 MPa.

[0078] Elongation at 93℃: 70%, tensile strength: 195MPa, yield strength: 185MPa.

[0079] The dissolution rate in 3.0% KCl at 93℃ reaches 70 mg*cm. -2 *h -1 .

[0080] Example 4

[0081] The soluble magnesium alloy of Example 4 is composed of the following elements by mass percentage: 1.2% Al, 1.6% Zn, 0.2% Ca, 0.1% Gd, 0.2% Sm and 1.2% Ni, with the balance being Mg.

[0082] Raw material proportions: Weigh magnesium ingots, aluminum ingots, zinc ingots, magnesium-nickel master alloy, magnesium-calcium master alloy, magnesium-gadolinium master alloy and magnesium-samarium master alloy according to the proportions.

[0083] Melting and casting: Magnesium ingots, aluminum ingots, and zinc ingots are placed in a pit-type resistance furnace and held at 740℃ until completely melted. The temperature is controlled at 740℃. Then, magnesium-nickel master alloy is added and stirred until completely melted. The melt temperature is controlled at 710℃, and then magnesium-calcium master alloy, magnesium-gadolinium master alloy, and magnesium-samarium master alloy are added and stirred evenly. The melt temperature is controlled at 710℃ to obtain a soluble magnesium alloy melt. Magnesium alloy ingots are obtained using electromagnetic semi-continuous casting technology. During the casting process, an electromagnetic frequency of 30Hz is set to electromagnetically stir the melt and ingot. The current of the electromagnetic system is 120A during electromagnetic stirring.

[0084] Homogenization treatment: The magnesium alloy ingot is kept at 370℃ for 18 hours.

[0085] Extrusion molding: The homogenized magnesium alloy ingot is machined into a cylinder with a diameter of 78mm and a diameter of 300mm, and then extruded after being kept at 180℃ for 3 hours; the obtained magnesium alloy rod is cooled with water to obtain soluble magnesium alloy.

[0086] The prepared soluble magnesium alloy was subjected to mechanical property testing and degradation rate testing according to GB / T228.1-2010 Metallic Materials - Tensile Testing.

[0087] Test results: Elongation at room temperature: 33%, tensile strength: 225 MPa, yield strength: 180 MPa.

[0088] Elongation at 93℃: 70%, tensile strength: 188MPa, yield strength: 175MPa.

[0089] The dissolution rate in 93℃ and 3.0% KCl reached 50 mg*cm. -2 *h -1 .

[0090] Comparative Example 1

[0091] The soluble magnesium alloy of Comparative Example 1 is composed of the following elements by mass percentage: 0.7% Al, 2.2% Zn, 0.7% Ni, with the balance being Mg.

[0092] Raw material proportions: Weigh magnesium ingots, aluminum ingots, zinc ingots, and magnesium-nickel master alloy according to the proportions.

[0093] Melting and casting: Magnesium ingots, aluminum ingots, and zinc ingots are placed in a pit-type resistance furnace and held at 800℃ until completely melted. Then, the temperature is controlled at 760℃ and a magnesium-nickel master alloy is added. After stirring evenly, the melt temperature is controlled at 740℃ to obtain a soluble magnesium alloy melt. Magnesium alloy ingots are obtained using electromagnetic semi-continuous casting technology. During the casting process, an electromagnetic frequency of 15Hz is set to electromagnetically stir the melt and ingots. The current of the electromagnetic system is 100A during electromagnetic stirring.

[0094] Homogenization treatment: The magnesium alloy ingot is held at 420℃ for 18 hours.

[0095] Extrusion molding: The homogenized magnesium alloy ingot is machined into a cylinder with a diameter of 78mm and a diameter of 300mm, and then extruded after being held at 110℃ for 3 hours; the obtained magnesium alloy rod is cooled with water to obtain soluble magnesium alloy.

[0096] The prepared soluble magnesium alloy was subjected to mechanical property testing and degradation rate testing according to GB / T228.1-2010 Metallic Materials - Tensile Testing.

[0097] Test results: Elongation at room temperature: 18%, tensile strength: 240 MPa, yield strength: 210 MPa.

[0098] Elongation at 93℃: 28%, tensile strength: 215MPa, yield strength: 165MPa.

[0099] The dissolution rate in 93℃ and 3.0% KCl reached 26 mg*cm. -2 *h -1 .

[0100] Comparative Example 2

[0101] The soluble magnesium alloy of Comparative Example 2 is composed of the following elements by mass percentage: 1.2% Al, 1.6% Zn and 1.2% Ni, with the balance being Mg.

[0102] Raw material proportions: Weigh magnesium ingots, aluminum ingots, zinc ingots, and magnesium-nickel master alloy according to the proportions.

[0103] Melting and casting: Magnesium ingots, aluminum ingots, and zinc ingots are placed in a pit-type resistance furnace and held at 700°C until completely melted. The addition temperature is controlled at 750°C, and then a magnesium-nickel master alloy is added. After stirring until completely melted, the melt temperature is controlled at 710°C to obtain a soluble magnesium alloy melt. Magnesium alloy ingots are obtained using electromagnetic semi-continuous casting technology. During the casting process, an electromagnetic frequency of 30Hz is set to electromagnetically stir the melt and ingots. The current of the electromagnetic system is 120A during electromagnetic stirring.

[0104] Homogenization treatment: The magnesium alloy ingot is kept at 370℃ for 18 hours.

[0105] Extrusion molding: The homogenized magnesium alloy ingot is machined into a cylinder with a diameter of 78mm and a diameter of 300mm, and then extruded after being kept at 180℃ for 3 hours; the obtained magnesium alloy rod is cooled with water to obtain soluble magnesium alloy.

[0106] The prepared soluble magnesium alloy was subjected to mechanical property testing and degradation rate testing according to GB / T228.1-2010 Metallic Materials - Tensile Testing.

[0107] Test results: Elongation at room temperature: 23%, tensile strength: 201 MPa, yield strength: 164 MPa.

[0108] Elongation at 93℃: 41%, tensile strength: 154MPa, yield strength: 145MPa.

[0109] The dissolution rate in 3.0% KCl at 93℃ reached 59 mg*cm. -2 *h -1 .

[0110] like Figure 2 and Figure 3 As shown, Examples 1-4 exhibit higher room temperature elongation and high temperature elongation compared to Comparative Examples 1-2. The high-plasticity soluble magnesium alloy of this invention possesses excellent service plasticity, moderate strength, and a simple and low-cost production process. Compared to soluble rubber, the dissolution rate of this soluble magnesium alloy in the service environment is controllable, allowing for complete dissolution without clogging the wellbore and eliminating the need for secondary drilling and milling. It can replace soluble rubber in components such as bridge plug slips and sealing rings. The extrusion process used in this preparation method is simple to operate, yields a high yield, and produces excellent room temperature and high temperature elongation of the bar stock.

[0111] It will be apparent to those skilled in the art that the present invention is not limited to the details of the exemplary embodiments described above, and that the invention can be implemented in other specific forms without departing from its spirit or essential characteristics. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description. Thus, all variations falling within the meaning and scope of equivalents of the claims are intended to be included within the present invention. No reference numerals in the claims should be construed as limiting the scope of the claims.

[0112] Furthermore, it should be understood that although this specification describes embodiments, not every embodiment contains only one independent technical solution. This narrative style is merely for clarity. Those skilled in the art should consider the specification as a whole, and the technical solutions in each embodiment can also be appropriately combined to form other embodiments that can be understood by those skilled in the art.

Claims

1. A highly ductile soluble magnesium alloy, characterized in that, The magnesium alloy comprises, by mass percentage: 0.7%-1.2% Al, 1.1%-2.2% Zn, 0.7%-1.5% Ni, 0.1%-0.5% X, with the balance being Mg, wherein X is selected from one or more of Ca, Gd, Ce and Sm; The method for preparing the highly ductile soluble magnesium alloy includes: Raw material proportions: Weigh magnesium ingots, aluminum ingots, zinc ingots, magnesium-nickel master alloys, and materials containing X according to the following mass percentages: Al: 0.7%-1.2%, Zn: 1.1%-2.2%, Ni: 0.7%-1.5%, X: 0.1%-0.5%, and the balance being Mg. Melting and casting: The magnesium ingots, aluminum ingots and zinc ingots are placed in a pit-type resistance furnace and held at 740℃-750℃ until completely melted. Then, a magnesium-nickel master alloy is added at 720℃-740℃ and stirred until completely melted. The melt temperature is controlled at 710℃-720℃ and then a material containing X is added. After stirring evenly, the temperature is controlled at 700℃-710℃ to obtain a soluble magnesium alloy melt. Then, magnesium alloy ingots are obtained using electromagnetic semi-continuous casting technology. Homogenization treatment: The magnesium alloy ingot is kept at 370℃-410℃ for 18 hours; Extrusion molding: The homogenized magnesium alloy ingot is held at 110℃~230℃ for a period of time and then extruded at an extrusion speed of 0.5mm / s-5mm / s to obtain magnesium alloy rods. The magnesium alloy rods are then cooled with water to obtain soluble magnesium alloy.

2. The high-plasticity soluble magnesium alloy according to claim 1, characterized in that, The magnesium alloy comprises, by mass percentage: 0.7% Al, 2.2% Zn, 0.1% Ca, 0.7% Ni, with the balance being Mg.

3. The high-plasticity soluble magnesium alloy according to claim 1, characterized in that, The magnesium alloy comprises, by mass percentage: 1.0% Al, 2.0% Zn, 0.2% Ca, 1.5% Ni, 0.2% Gd, with the balance being Mg.

4. The high-plasticity soluble magnesium alloy according to claim 1, characterized in that, The magnesium alloy comprises, by mass percentage: 0.9% Al, 1.1% Zn, 0.2% Ca, 0.7% Ni, 0.3% Ce, with the balance being Mg.

5. The high-plasticity soluble magnesium alloy according to claim 1, characterized in that, The magnesium alloy comprises, by mass percentage: 1.2% Al, 1.6% Zn, 0.2% Ca, 1.2% Ni, 0.1% Gd, 0.2% Sm, with the balance being Mg.

6. A method for preparing a highly ductile soluble magnesium alloy according to any one of claims 1-5, characterized in that, include: Raw material proportions: Weigh magnesium ingots, aluminum ingots, zinc ingots, magnesium-nickel master alloys, and materials containing X according to the following mass percentages: Al: 0.7%-1.2%, Zn: 1.1%-2.2%, Ni: 0.7%-1.5%, X: 0.1%-0.5%, and the balance being Mg. Melting and casting: The magnesium ingots, aluminum ingots and zinc ingots are placed in a pit-type resistance furnace and held at 740℃-750℃ until completely melted. Then, a magnesium-nickel master alloy is added at 720℃-740℃ and stirred until completely melted. The melt temperature is controlled at 710℃-720℃ and then a material containing X is added. After stirring evenly, the temperature is controlled at 700℃-710℃ to obtain a soluble magnesium alloy melt. Then, magnesium alloy ingots are obtained using electromagnetic semi-continuous casting technology. Homogenization treatment: The magnesium alloy ingot is kept at 370℃-410℃ for 18 hours; Extrusion molding: The homogenized magnesium alloy ingot is held at 110℃~230℃ for a period of time and then extruded to obtain magnesium alloy rods. The magnesium alloy rods are then cooled with water to obtain soluble magnesium alloy.

7. The method for preparing a highly ductile soluble magnesium alloy according to claim 6, characterized in that, The material containing X is selected from one or more of magnesium-calcium master alloy, magnesium-gadolinium master alloy, magnesium-cerium master alloy, and magnesium-samarium master alloy.

8. The method for preparing a highly ductile soluble magnesium alloy according to claim 6, characterized in that, In the electromagnetic semi-continuous casting process, the electromagnetic frequency of the electromagnetic stirring is between 15Hz and 30Hz, and the electromagnetic stirring current is between 100A and 120A.

9. The method for preparing a highly ductile soluble magnesium alloy according to claim 6, characterized in that, The heat preservation time for extrusion molding is between 3 and 4 hours.

Citation Information

Patent Citations

  • High-ductility soluble magnesium-lithium alloy and preparation method and application thereof

    CN113667871A

  • High-plasticity rapidly-degradable Mg-Li-Gd-Ni alloy and preparation method thereof

    CN114411029A

  • Magnesium alloy capable of being dissolved in chlorine-containing solution as well as preparation method and application of magnesium alloy

    CN116287918A

  • Mg Alloys Containing Misch Metal Manufacturing Method of Wrought Mg Alloys Containing Misch Metal, and Wrought Mg Alloys Thereby