A thin-film solar cell chip with a vertical structure and its preparation method and application

By arranging a front support block with matching thermal expansion coefficient on the front side of the thin film solar cell chip and setting a projection position in the back electrode welding area, the problem of welding damage to the back electrode of the thin film solar cell is solved, the welding yield is significantly improved and the photoelectric performance is maintained.

CN118016741BActive Publication Date: 2024-10-25SUN YAT SEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410055151.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-12
Publication Date
2024-10-25
Estimated Expiration
2044-01-12

AI Technical Summary

Technical Problem

The back electrode of vertically structured thin-film solar cells is easily damaged during welding. Existing improvement methods have limited capabilities and are difficult to completely solve the problem.

Method used

A front support block is provided in the front welding area of ​​the thin-film solar cell chip. The material includes metal, transparent metal oxide and transparent polymer. The thermal expansion coefficient matches the front electrode and grid line to reduce the risk of stress cracking during welding, and in the back electrode welding area Set the projection position to improve welding yield.

Benefits of technology

It significantly improves the welding yield of thin-film solar cell chips and avoids crack damage and thermal expansion stress cracking during welding. The welding yield reaches ≥99% and has almost no impact on the light-receiving area.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118016741B_ABST
    Figure CN118016741B_ABST
Patent Text Reader

Abstract

The present invention discloses a thin-film solar cell chip with a vertical structure and a preparation method and application thereof, belonging to the field of new energy technology. The thin-film solar cell chip with a vertical structure provided by the present invention comprises: a P / N junction functional layer; a back electrode; the back electrode is arranged on the A surface of the P / N junction functional layer; and is composed of a welding area and a non-welding area; a front electrode; the front electrode is arranged in a local area of ​​the B surface of the P / N junction functional layer; a front support block; the front support block is arranged on the B surface of the P / N junction functional layer and is located at the projection position of the welding area; a gate line; the gate line is arranged on the B surface of the P / N junction functional layer, in an area outside the front electrode and the front support block. Through structural design, the welding yield of thin-film solar cell chips can be effectively improved. The present invention also provides a preparation method and application of the above-mentioned thin-film solar cell chip with a vertical structure.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of new energy technology, and in particular to a thin-film solar cell chip with a vertical structure and a preparation method and application thereof. Background Art

[0002] The positive and negative electrodes of vertical thin-film solar cells are located on both sides of the cell. The electrode on the front side of the cell that receives light is generally called the front electrode, and the electrode on the back side of the cell is called the back electrode. In order to further reduce the weight of the cell and reduce production costs, the production of thin-film solar cells has a tendency to become thinner. However, when welding the battery components in series and parallel, the front electrode and the back electrode need to be welded separately. The thinner the cell, the more likely it is that the front side of the cell will be damaged when welding the back electrode.

[0003] To solve the problem of damage caused by welding on the back electrode of vertical thin-film solar cells, improvements can be made by optimizing the welding process, such as welding time, welding power, and number of welding times. However, these methods have limited ability to reduce abnormalities and cannot completely solve the problem. Summary of the invention

[0004] The present invention aims to solve at least one of the technical problems existing in the prior art. To this end, the present invention provides a thin-film solar cell chip with a vertical structure, which can effectively improve the welding yield of the thin-film solar cell chip.

[0005] The present invention also provides a method for preparing the vertically structured thin-film solar cell chip.

[0006] The present invention also provides the application of the vertical structure thin-film solar cell chip.

[0007] According to an embodiment of the first aspect of the present invention, there is provided a vertically structured thin-film solar cell chip, the thin-film solar cell chip comprising:

[0008] P / N junction functional layer;

[0009] Back electrode; the back electrode is arranged on the A surface of the P / N junction functional layer; and is composed of a welding area and a non-welding area;

[0010] A front electrode; the front electrode is disposed in a local area of ​​the B surface of the P / N junction functional layer;

[0011] A front support block; the front support block is arranged on the B surface of the P / N junction functional layer and is located at the projection position of the welding area;

[0012] Gate line; the gate line is arranged on the surface of the P / N junction functional layer B, in an area outside the front electrode and the front support block.

[0013] The vertical thin-film solar cell chip according to the embodiment of the present invention has at least the following beneficial effects:

[0014] The thickness of the thin-film solar cell chip with vertical structure is generally about 50~80μm, and there is no front support block on the front side; when the back electrode is welded by resistance welding (drawing current), it is easy to cause damage to the front side of the thin-film solar cell chip. There are two reasons for this: first, during welding, the grid line on the front side of the thin-film solar cell chip contacts the welding platform, and the welding stress area is only supported by the grid line. In addition, the thin-film solar cell chip is very thin as a whole, and the impact force of welding can easily cause crack damage to the thin-film solar cell chip; second, resistance welding is achieved through local instantaneous high heat energy. During the welding process, the front electrode / grid line area and other areas on the front side of the thin-film solar cell chip will produce instantaneous large stress due to the difference in thermal expansion coefficient, which will cause the chip to break.

[0015] The present invention sets a front support block on the front side of the thin-film solar cell chip, in the projection area of ​​the welding area, thereby enabling the thin-film solar cell chip to withstand welding impact during back welding and avoiding stress cracking caused by differences in thermal expansion coefficients of the thin-film solar cell chip.

[0016] According to some embodiments of the present invention, the material of the front support block includes at least one of metal, transparent metal oxide and transparent polymer film.

[0017] The material of the transparent polymer film includes at least one of polyimide and epoxy resin.

[0018] The material of the transparent metal oxide includes at least one of SiO2 and ITO.

[0019] When the material of the front support block is selected from the transparent metal oxide and the transparent compound film, the light receiving area of ​​the thin film solar cell chip is hardly reduced.

[0020] According to some embodiments of the present invention, the thermal expansion coefficient of the front support block is 45E-6 / °C to 50E-6 / °C. For example, it may be about 49E-6 / °C.

[0021] According to some embodiments of the present invention, the thickness of the front support block is 3-8 μm, for example, about 5 μm.

[0022] According to some embodiments of the present invention, the front support block and the front electrode have comparable thicknesses.

[0023] According to some embodiments of the present invention, the material of the front electrode includes silver.

[0024] According to some embodiments of the present invention, the gate line is made of silver.

[0025] According to some embodiments of the present invention, the thermal expansion coefficient of the front electrode is 15E-6 / °C to 20E-6 / °C, for example, about 18.7E-6 / °C.

[0026] Therefore, the thermal expansion coefficients of the front support block, the front electrode and the grid line are similar, and the back electrode will not crack due to the heat generated by welding; thus improving the welding yield of the obtained thin-film solar cell chip.

[0027] According to some embodiments of the present invention, the P / N junction functional layer includes a substrate and an epitaxial structure that are stacked together; and the back electrode is disposed on a surface of the substrate (surface A).

[0028] According to some embodiments of the present invention, the material of the substrate includes Ge.

[0029] According to some embodiments of the present invention, the thickness of the substrate is 45-60 μm, for example, about 50 μm or about 55 μm.

[0030] According to some embodiments of the present invention, the epitaxial structure comprises a gallium arsenide subcell.

[0031] According to some embodiments of the present invention, the thickness of the epitaxial structure is 5-10 μm, for example, 6-7 μm.

[0032] According to some embodiments of the present invention, the area of ​​the projection position accounts for 0.01-0.015% of the surface area of ​​the thin-film solar cell chip. For example, it can be about 0.012%. This small area has almost no effect on the light receiving area of ​​the thin-film solar cell chip.

[0033] According to some embodiments of the present invention, the thickness of the back electrode is 2-5 μm, for example, 3-4 μm.

[0034] According to some embodiments of the present invention, the material of the back electrode includes at least one of gold and silver.

[0035] It should be noted that there is no obvious boundary between the welding area and the non-welding area of ​​the back electrode. In actual production, the position of the welding area can be determined according to the requirements of the series-parallel circuit or the process requirements of the welding technology.

[0036] According to some embodiments of the present invention, the thickness of the thin-film solar cell chip is 50-80 μm, for example, about 60 μm, 65 μm, 70 μm or about 75 μm.

[0037] According to some embodiments of the present invention, the welding yield rate of the thin-film solar cell chip is ≥ 99%, for example, it may be about 100%.

[0038] According to an embodiment of the second aspect of the present invention, a method for preparing the thin-film solar cell chip is provided, the method comprising the following steps:

[0039] S1. Providing a P / N junction functional layer semi-finished product formed by stacking a substrate and an epitaxial structure, and providing the front electrode and the gate line on the surface of one side of the epitaxial structure of the P / N junction functional layer semi-finished product;

[0040] S2. Thinning the substrate and providing the back electrode on its surface;

[0041] S3. Setting the front support block.

[0042] Since the preparation method adopts all the technical solutions of the thin-film solar cell chip of the above embodiment, it at least has all the beneficial effects brought by the technical solutions of the above embodiment. Furthermore, the steps of the preparation method are reasonably designed, the production process is smooth, and the yield is high.

[0043] According to some embodiments of the present invention, in step S1, the material of the substrate includes Ge.

[0044] According to some embodiments of the present invention, in step S1, the thickness of the substrate is 125-180 μm, for example, about 150 μm.

[0045] According to some embodiments of the present invention, in step S1, the arrangement of the P / N junction functional layer semi-finished product includes arranging the epitaxial structure on the surface of the substrate.

[0046] According to some embodiments of the present invention, the epitaxial structure setting method includes at least one of a diffusion method and an MOCVD method, wherein the former is implemented by a diffusion furnace.

[0047] According to some embodiments of the present invention, in step S1, the front electrode and the gate line are independently arranged by at least one of printing sintering, chemical plating and electron beam evaporation. When the electron beam evaporation is selected, a photoresist is required to assist in positioning the front electrode and the gate line.

[0048] According to some embodiments of the present invention, in step S2, the thinning method includes at least one of grinding and polishing and wet etching.

[0049] After the base is thinned, a substrate is formed, and the substrate and the epitaxial structure together constitute the P / N junction functional layer.

[0050] The thickness ratio of the substrate to the base is 30-45:100, for example, about 35:100 or about 40:100.

[0051] According to some embodiments of the present invention, in step S2, the method for setting the back electrode includes at least one of printing sintering, chemical plating and electron beam evaporation.

[0052] According to some embodiments of the present invention, in step S3, the method for setting the front support block includes at least one of photolithography to form a thin film pattern and dispensing glue.

[0053] The photolithography method for forming a thin film pattern is applicable when the material of the front support block is selected from metal or transparent metal oxide.

[0054] The applicable scenario of the dispensing is when the material of the front support block is selected from the transparent polymer film.

[0055] In the preparation method, the numbering of step S2 and step S3 is only for the convenience of description and does not represent the order in which the steps are performed. In actual production, step S2 or step S3 can be performed first. For example, the front support block can be set after the front electrode and the gate line are set; the front support block can also be set after the back electrode is set.

[0056] According to some embodiments of the present invention, the dispensing includes sequentially performing dispensing, baking, exposure and secondary baking.

[0057] The glue spreading is carried out by using a glue dispensing machine.

[0058] The baking temperature is 100-120 μm, for example, about 110° C. The baking time is 1-5 min, for example, 2-3 min.

[0059] The exposure device includes an i-line exposure machine, and the exposure dose is 250-350 mJ / cm 2 , for example, about 300 mJ / cm 2 Thus, the transparent polymer film can be fully cross-linked.

[0060] The secondary baking temperature is 250-350° C., for example, about 300° C. The secondary baking time is 20-40 minutes, for example, about 30 minutes. Thus, the transparent polymer film can be fully cured.

[0061] According to an embodiment of the third aspect of the present invention, there is provided an application of the thin-film solar cell chip in ground photovoltaics and space photovoltaics.

[0062] Since the application adopts all the technical solutions of the thin-film solar cell chip of the above embodiment, it at least has all the beneficial effects brought by the technical solutions of the above embodiment.

[0063] Unless otherwise specified, "equivalent" in the present invention means that the difference is within 2%.

[0064] If there is no special explanation, the actual meaning of “about” in the present invention is that the error is allowed to be within the range of ±2%, for example, about 100 is actually 100±2%×100.

[0065] Unless otherwise specified, “between” in the present invention includes the number itself, for example, “between 2 and 3” includes the endpoint values ​​2 and 3.

[0066] Other features and advantages of the present invention will be set forth in the description which follows, and in part will be obvious from the description, or may be learned by practice of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0067] The above and / or additional aspects and advantages of the present invention will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0068] Figure 1 is a schematic diagram of the structure of the components obtained in step S1 of embodiment 1 of the present invention;

[0069] Figure 2 yes Figure 1 Section along line AB;

[0070] Figure 3 is a schematic diagram of the structure of the components obtained in step S2a of Example 1 of the present invention;

[0071] Figure 4 This is a schematic diagram of the structure of the thin-film solar cell chip obtained in Example 1 of the present invention;

[0072] Figure 5 This is a schematic diagram of the structure of the thin-film solar cell chip obtained in Comparative Example 1 of the present invention;

[0073] Figure 6 yes Figure 5 Section along line AB.

[0074] Reference numerals:

[0075] Base 100 , substrate 110 , epitaxial structure 200 , front electrode 301 , gate line 302 , projection position 303 , front support block 304 , back electrode 400 . DETAILED DESCRIPTION

[0076] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.

[0077] In the description of the present invention, the description with reference to the terms "one embodiment", "some embodiments", "illustrative embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0078] Example 1

[0079] refer to Figures 1 to 4 In this example, a thin-film solar cell chip is prepared. The specific steps are as follows:

[0080] S1. A P / N junction functional layer semi-finished product formed by stacking a substrate 100 and an epitaxial structure 200 is provided, and a front electrode 301 and a gate line 302 are provided on one side of the epitaxial structure 200 of the P / N junction functional layer semi-finished product; wherein,

[0081] The substrate 100 is a Ge sheet with a thickness of 150 μm;

[0082] The epitaxial structure 200 is provided by MOCVD, specifically a multi-junction gallium arsenide cell epitaxial structure layer, with a thickness of about 6 μm;

[0083] The front electrode 301 and the gate line 302 are formed by electron beam evaporation and photoresist stripping technology. The material is silver and the thickness is about 5 μm.

[0084] When setting the gate line 302, the projection position 303 of the welding area of ​​the back electrode 400 needs to be left empty; if the projection position 303 is not left empty, but all local gate lines 302 are used, the area occupied by the gate line 302 accounts for 0.012% of the area of ​​the epitaxial structure 200, which will not have a significant impact on the light receiving conditions of the thin-film solar cell chip.

[0085] The structural diagram of the components obtained in this step is as follows Figure 1 As shown (view from the front electrode side), Figure 1 The cross-section along line AB is as follows Figure 2 shown.

[0086] S2.

[0087] S2a. The substrate 100 is thinned by grinding to obtain a substrate 110. The substrate 110 and the epitaxial structure 200 together form a P / N junction functional layer. The thickness of the substrate 110 is about 51 μm. The structural schematic diagram is as shown in FIG. Figure 3 As shown;

[0088] S2b. A back electrode 400 made of silver is disposed on one side of the component substrate 110 obtained in step S2a. The back electrode 400 is disposed by electron beam evaporation, and has a thickness of about 3 μm.

[0089] S3. Use a dispensing machine to dispense glue in the projection position 303 area. The dispensing material is polyimide ZKPI-5100 with a thickness of 5μm. After dispensing, bake on a 110℃ hot plate for 2 minutes, and then use an i-line exposure machine for exposure. The exposure dose is 300mJ / cm 2 , so that the polyimide undergoes a cross-linking reaction. Finally, the polyimide is baked in an oven at 300° C. for 30 minutes to complete the curing of the polyimide, thereby forming a front support block 304;

[0090] The structure of the thin-film solar cell chip obtained in this example is as follows Figure 4 The overall thickness is about 65 μm.

[0091] The thermal expansion coefficient of silver, the main component of the front electrode 301, is 18.7E-6 / ℃, and the thermal expansion coefficient of polyimide, the material of the front support block 304, is 49.0E-6 / ℃, and there is no significant difference in the thermal expansion coefficients of the two. At the same time, polyimide has the characteristics of high temperature resistance, excellent mechanical properties, good stability, etc., which is conducive to the subsequent welding process.

[0092] Example 2

[0093] This example prepares a thin-film solar cell chip, and the specific steps differ from those in Example 1 in that:

[0094] In this example, the material of the front support block is SiO2; the specific method for setting the front support block is: using photolithography, electron beam evaporation and degumming methods, a front support block made of SiO2 with a thickness of 5μm is prepared in the projection position 303 area.

[0095] Comparative Example 1

[0096] refer to Figures 5 and 6 In this example, a thin-film solar cell chip is prepared. The specific steps are different from those in Example 1 in that:

[0097] (1) In step S1 , the projection position 303 is not left vacant, and the corresponding position is filled according to the rule of the grid lines 302 .

[0098] (2) Step S3 is not included, that is, the front support block 304 is not provided.

[0099] Test Case

[0100] This example tests the welding yield of the thin-film solar cell chips obtained in the embodiment and the comparative example. The specific testing method is as follows:

[0101] Place the thin-film solar cell chip face down on the welding platform (such as Figure 4 The welding operation is performed on the welding area of ​​the back electrode (i.e., the area directly above the front support block 304), with a welding voltage of 0.7 V and a welding time of 25 ms.

[0102] This example also uses an AM0 solar simulator, and the thin-film solar cell chip is placed on the AM0 simulator carrier with the back electrode side facing down. The carrier is connected to the positive electrode of the test circuit, and the front electrode is connected to the negative electrode of the test circuit. Turn on the simulator light source, and measure the short-circuit current of the thin-film solar cell chip obtained in the embodiment and the comparative example. The short-circuit current value is divided by the area of ​​the thin-film solar cell chip to obtain the current density of the thin-film solar cell chip.

[0103] In the thin-film solar cell chip obtained in Example 1, due to the support of the front support block 304, it withstands the welding impact force. After welding 200 cells, it was checked that there was no damage on the front of the solar cell chip, and the welding defect rate was zero. The average current density of the chip was 17.57 mA / cm 2 The test results show that the results obtained in Example 1 and Example 2 are comparable, and significantly better than Comparative Example 1.

[0104] In the thin-film solar cell chip obtained in Comparative Example 1, since the thin-film solar cell chip is very thin, only the thin metal grid line 302 supports the welding area during welding, and most of the welding area is in a suspended state. The welding impact force is more likely to cause dark cracks on the front of the thin-film solar cell chip. 58 of the 100 chips were welded with dark crack damage, and the welding defect rate was 58%. The average current density of the chip was 17.61mA / cm 2 .

[0105] The test results of the embodiments and comparative examples are summarized in Table 1.

[0106] Table 1 Test results of embodiments and comparative examples

[0107]

[0108] From this comparison, it can be seen that the front support block provided by the present invention can significantly improve the welding yield of the obtained thin-film solar cell chip, and has almost no effect on the photoelectric performance of the thin-film solar cell chip. It can be further predicted that the thin-film solar cell chip provided by the present invention is expected to be widely used in space and surface photovoltaics due to its good structural design and excellent performance.

[0109] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.

Claims

1. A vertical thin-film solar cell chip, It is characterized in that The thin film solar cell chip comprises: P / N junction functional layer; A back electrode, which is disposed on the back of the P / N junction functional layer and consists of a welding area and a non-welding area; A front electrode, the front electrode being disposed in a local area of ​​the front light-receiving surface of the P / N junction functional layer; A front support block, the front support block is arranged on the front light-receiving surface of the P / N junction functional layer and is located at the projection position of the welding area; the material of the front support block includes SiO 2 and at least one of a transparent polymer film; A gate line, which is arranged on the front light-receiving surface of the P / N junction functional layer and is located in a region outside the front electrode and the front support block; The thickness of the thin film solar cell chip is 50-80 μm.

2. The thin-film solar cell chip according to claim 1, It is characterized in that The thickness of the front support block is comparable to that of the front electrode.

3. The thin film solar cell chip according to claim 1, It is characterized in that The thickness of the front support block is 3-8 μm; and / or the thickness of the back electrode is 2-5 μm.

4. The thin-film solar cell chip according to any one of claims 1 to 3, It is characterized in that The welding yield rate of the thin-film solar cell chip is ≥99%.

5. A method for preparing a thin film solar cell chip according to any one of claims 1 to 4, It is characterized in that The preparation method comprises the following steps: S1. Providing a P / N junction functional layer semi-finished product formed by stacking a substrate and an epitaxial structure, and providing the front electrode and the gate line on the surface of one side of the epitaxial structure of the P / N junction functional layer semi-finished product; S2. Thinning the substrate and providing the back electrode on its surface; S3. Setting the front support block.

6. The preparation method according to claim 5, It is characterized in that In step S3, the method for setting the front support block includes at least one of photolithography to form a thin film pattern and glue dispensing.

7. The preparation method according to claim 5, It is characterized in that In step S2, the thinning method includes at least one of grinding and polishing and wet etching.

8. The preparation method according to any one of claims 5 to 7, It is characterized in that In step S1, the method for setting the front electrode and the gate line is independently selected from at least one of printing sintering, chemical plating and electron beam evaporation; and / or, in step S2, the method for setting the back electrode includes at least one of printing sintering, chemical plating and electron beam evaporation.

9. Application of the thin-film solar cell chip as claimed in any one of claims 1 to 4 in surface photovoltaics and space photovoltaics.