Method for preparing mesoporous GaN-based LED with mesoporous GaN DBR
By growing a p-GaN layer on the mesoporous GaN-based multiple quantum wells of mesoporous GaN DBR, the problem of low luminous efficiency of GaN-based LEDs is solved, efficient light extraction and heat dissipation are achieved, and it is suitable for industrial production.
Patent Information
- Application Number
- CN202410122154.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-29
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-01-29
AI Technical Summary
The luminous efficiency of existing GaN-based LEDs is low, mainly due to high defect density and low light extraction efficiency.
GaN-based LEDs are grown on nanoporous films, and p-GaN layers are grown on the mesoporous GaN-based multiple quantum wells of mesoporous GaN DBR. Through steps such as organometallic chemical vapor deposition technology and electrochemical etching, a medium-sized device is prepared. Mesoporous GaN-based LEDs with porous GaN DBR.
The luminous efficiency, service life and heat dissipation capacity of GaN-based LEDs are significantly improved, and the process conditions are easy to accurately control. The prepared LEDs have high uniformity and repeatability, and are suitable for industrial production.
Smart Images

Figure CN118016770B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of semiconductor optoelectronic materials, and in particular relates to a method for preparing a mesoporous GaN-based LED with a mesoporous GaN DBR. Background Art
[0002] Gallium nitride (GaN)-based light-emitting diodes (LEDs) have the advantages of being environmentally friendly and non-toxic, and have been widely used. However, their high stress, poor crystal quality, and low light extraction efficiency lead to low luminous efficiency. In order to improve the luminous efficiency of GaN-based LEDs, GaN-based LEDs can be grown on nanoporous films. At present, various structures such as porous Si and porous GaN have been tried. However, even if the peeling is achieved, the luminous efficiency is still low due to high defect density and low light extraction efficiency. A p-GaN layer is grown on a mesoporous GaN-based multiple quantum well (MQW) with a mesoporous GaN DBR to prepare a mesoporous GaN-based LED with a mesoporous GaN DBR. The reduction in defect density improves the crystal quality, and the high reflection effect of the DBR enhances the light extraction efficiency, resulting in a significant increase in its luminous intensity. Summary of the invention
[0003] The purpose of the present invention is to provide a method for preparing a mesoporous GaN-based LED having a mesoporous GaN DBR, which solves the problem of low luminous efficiency due to high defect density and low light extraction efficiency in the prior art.
[0004] The technical solution adopted by the present invention is: a method for preparing a mesoporous GaN-based LED having a mesoporous GaN DBR, which is specifically implemented according to the following steps:
[0005] Step 1: epitaxially growing a GaN buffer layer, a u-GaN / n-GaN periodic structure, a GaN-based superlattice and a multi-quantum well layer on a substrate in sequence by using an organic metal chemical vapor deposition technique to obtain a GaN-based MQW structure;
[0006] Step 2, electrochemically etching the GaN-based MQW structure in an electrolyte to prepare a mesoporous GaN-based MQW having a mesoporous GaN DBR;
[0007] Step 3: Using the mesoporous GaN-based MQW as a substrate, a p-GaN layer is grown using a regrowth technique to prepare a mesoporous GaN-based LED having a mesoporous GaNDBR.
[0008] The present invention is also characterized in that:
[0009] In step 1, the u-GaN / n-GaN periodic structure includes a low-doped GaN layer and a high-doped GaN layer, both of which have a thickness of 51-67 nm. The doping concentration of the low-doped GaN layer is 4.1×10 15-9.9×10 17 cm -3 ,The doping concentration of the highly doped GaN layer is 3.1×10 18 -3.9×10 19 cm -3 ,and the number of periods is 5 - 20.
[0010] The doping concentrations of both the GaN-based superlattice and multiple quantum well layers are 3.1×10 18 -3.9×10 19 cm -3 ,The superlattice structure is an In x Ga 1-x N / GaN superlattice structure with a period of 10 - 11, where 0 < x < 0.09. In each period, the thickness of In x Ga 1-x N is 3 - 4 nm, and the thickness of GaN is 7 nm; the multiple quantum well layer is an In y Ga 1-y N / GaN multiple quantum well structure with a period of 15 - 29, where 0.1 < y < 0.4. In each period, the thickness of In y Ga 1-y N is 4 - 6 nm, and the thickness of GaN is 10 - 11 nm.
[0011] In step 2, the electrolyte is any one of the aqueous solutions of nitric acid, sodium nitrate, sodium chloride, and sodium sulfate, with a concentration of 0.3 - 0.5 mol / ·L, the electrochemical etching voltage is 6 - 49 V, and the etching time range is 6 - 78 min.
[0012] In step 3, the p-GaN layer is a Mg-doped p-GaN layer.
[0013] The specific process of growing the p-GaN layer by the regrowth technique in step 3 is as follows: A Mg-doped p-GaN layer is used, the growth temperature is 800 - 1100 °C, and the doping concentration is 1.1×10 19 cm -3 -5.9×10 19 cm -3 ,and the thickness is 110 - 290 nm.
[0014] The beneficial effects of the present invention are:
[0015] 1) The mesoporous GaN-based MQW with a mesoporous GaN DBR has a unique mesoporous structure, high light reflection effect, large stress relaxation, and low defect density. Using it as a substrate, the grown p-GaN thin film exhibits large stress relaxation and high crystal quality, and is expected to significantly improve the luminous efficiency, service life, and heat dissipation capacity of GaN-based LEDs;
[0016] 2) The growth temperature of the p-GaN layer can affect the light reflectivity of the mesoporous GaN-based MQW with mesoporous GaN DBR and the crystal quality of the p-GaN film; when the p-GaN layer regrowth temperature is between 800-1100°C, the mesoporous GaN-based MQW with mesoporous GaN DBR maintains a high reflectivity, and the crystal quality of the film is significantly improved, which is beneficial to improving the luminous efficiency of GaN-based LEDs;
[0017] 3) The process conditions in the present invention are easy to accurately control, and the prepared mesoporous GaN-based LED with mesoporous GaN DBR has good uniformity and repeatability, which is convenient for industrial production; the prepared LED also has excellent characteristics such as high luminous efficiency, high stability, long service life and strong heat dissipation capacity, and has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 is a scanning electron microscope (SEM) image of a cross section of the MP MQW with MP GaN DBR prepared in Example 1, wherein the scale bar is 500 nm;
[0019] Figure 2 is a cross-sectional SEM image of the MP LED with MP GaN DBR prepared in Example 1, wherein the scale bar is 500 nm;
[0020] Figure 3 is the rocking curve corresponding to the InGaN (0002) peak of the two LEDs prepared in Example 1;
[0021] Figure 4 is the Raman spectra of two LEDs prepared in Example 1;
[0022] Figure 5 is the reflection spectrum of two LEDs prepared in Example 1;
[0023] Figure 6 is the current-voltage curve of two LEDs prepared in Example 1;
[0024] Figure 7 1 is the electroluminescence (EL) spectrum of two LEDs prepared in Example 1. DETAILED DESCRIPTION
[0025] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.
[0026] The method for preparing a mesoporous GaN-based LED having a mesoporous GaN DBR of the present invention is specifically implemented according to the following steps:
[0027] Step 1: Use metalorganic chemical vapor deposition technology to epitaxially grow a GaN buffer layer, a u-GaN / n-GaN periodic structure, a GaN-based superlattice, and a multiple quantum well (MQW) layer on a substrate in sequence to obtain a GaN-based MQW structure;
[0028] The u-GaN / n-GaN periodic structure includes a low-doped GaN layer and a high-doped GaN layer, both with a thickness of 51 - 67 nm. The doping concentration of the low-doped GaN layer is 4.1×10 15 -9.9×10 17 cm -3 , and the doping concentration of the high-doped GaN layer is 3.1×10 18 -3.9×10 19 cm -3 , and the number of periods is 5 - 20.
[0029] The doping concentrations of both the GaN-based superlattice and the multiple quantum well layer are 3.1×10 18 -3.9×10 19 cm -3 . The superlattice structure is an In x Ga 1-x N / GaN superlattice structure with a period of 10 - 11, where 0 < x < 0.09. In each period, the thickness of In x Ga 1-x N is 3 - 4 nm, and the thickness of GaN is 7 nm; the multiple quantum well layer is an In y Ga 1-y N / GaN multiple quantum well structure with a period of 15 - 29, where 0.1 < y < 0.4. In each period, the thickness of In y Ga 1-y N is 4 - 6 nm, and the thickness of GaN is 10 - 11 nm.
[0030] Step 2: Electrochemically etch the GaN-based MQW structure in an electrolyte to prepare a mesoporous GaN-based MQW with a mesoporous GaN DBR;
[0031] The electrolyte is any one of aqueous solutions of nitric acid, sodium nitrate, sodium chloride, and sodium sulfate, with a concentration of 0.3 - 0.5 mol / L. The electrochemical etching voltage is 6 - 49 V, and the etching time ranges from 6 - 78 min.
[0032] Step 3: Use the regrowth technology to grow a p-GaN layer on the mesoporous GaN-based MQW as a substrate to prepare a mesoporous GaN-based LED with a mesoporous GaN DBR.
[0033] The p-GaN layer is a Mg-doped p-GaN layer.
[0034] The specific process of growing p-GaN layer by regrowth technology is as follows: Mg-doped p-GaN layer is used, the growth temperature is 800-1100℃, and the doping concentration is 1.1×10 19 cm -3 -5.9×10 19 cm -3 , thickness is 110-290nm.
[0035] Example 1
[0036] The method for preparing a mesoporous GaN-based LED having a mesoporous GaN DBR of the present invention is specifically implemented according to the following steps:
[0037] Step 1: A GaN buffer layer is grown epitaxially at low temperature on a 2-inch C-plane sapphire substrate using metal organic chemical vapor deposition technology; then, a u-GaN / n-GaN periodic structure with 11 periods is grown, in which n-GaN is doped with Si at a doping concentration of 1×10 19 cm -3 , the thickness of n-GaN is 65nm, and the thickness of u-GaN is 51nm; then, at 810℃, 10 cycles of In 0.05 Ga 0.95 N / GaN superlattice structure, in which the well and barrier (GaN) thicknesses are 3nm and 7nm respectively, and the doping concentration is 1×10 19 cm -3 ; Finally, grow 20 cycles of In 0.2 Ga 0.8 N / GaN multi-quantum well structure, in which the growth temperature of the well and barrier is 780℃ and 860℃ respectively, the growth thickness is 4nm and 10nm respectively, and the doping concentration is 1×10 19 cm -3 , and a GaN-based MQW structure is obtained.
[0038] Step 2: 0.3 mol / L HNO 3 As the electrolyte, the GaN-based MQW structure was used as the anode and etched for 18 minutes at a constant voltage of 16 V. After the etching was completed, the instrument was turned off, the sample was removed, and the etched sample was immersed in deionized water for 5 minutes and then dried with nitrogen to prepare the mesoporous GaN-based MQW with mesoporous GaN DBR.
[0039] Step 3: Using the mesoporous GaN-based MQW with mesoporous GaN DBR as the substrate, a p-GaN layer was regrown using the regrowth technology to prepare a mesoporous GaN-based LED with mesoporous GaN DBR. The p-GaN layer was a Mg-doped p-GaN layer with a growth temperature of 900°C and a doping concentration of 4.5×10 19 cm -3, thickness is 155nm.
[0040] Example 2
[0041] The method for preparing a mesoporous GaN-based LED having a mesoporous GaN DBR is specifically implemented according to the following steps:
[0042] Step 1: A GaN buffer layer is grown epitaxially at low temperature on a 2-inch SiC substrate using metal organic chemical vapor deposition technology. Next, a u-GaN / n-GaN periodic structure with 15 periods is grown, where n-GaN is doped with Si at a doping concentration of 1.2×10 19 cm -3 , the thickness of n-GaN is 69nm, and the thickness of u-GaN is 52nm; then, 14 cycles of In 0.05 Ga 0.95 N / GaN superlattice structure, where the well and barrier thicknesses are 3nm and 7nm respectively, and the doping concentration is 1×10 19 cm -3 ; Finally, grow 20 cycles of In 0.2 Ga 0.8 N / GaN multi-quantum well structure, the growth thickness is 4nm and 10nm, and the doping concentration is 1×10 19 cm -3 .
[0043] Step 2: 0.5 mol / L HNO 3 As the electrolyte, the GaN-based MQW structure was used as the anode and etched for 25 minutes at a constant voltage of 14 V. After the etching was completed, the instrument was turned off, the sample was removed, and the etched sample was immersed in deionized water for 5 minutes and then dried with nitrogen to prepare the mesoporous GaN-based MQW with mesoporous GaN DBR.
[0044] Step 3: Using the mesoporous GaN-based MQW with mesoporous GaN DBR as the substrate, the p-GaN layer was regrown by MOCVD to prepare a mesoporous GaN-based LED with mesoporous GaN DBR. The p-GaN layer was a Mg-doped p-GaN layer with a growth temperature of 950°C and a doping concentration of 5.0×10 19 cm -3 , with a thickness of 200nm.
[0045] Example 3
[0046] The method for preparing a mesoporous GaN-based LED having a mesoporous GaN DBR is specifically implemented according to the following steps:
[0047] Step 1: epitaxially grow a GaN buffer layer on a 2-inch quartz substrate using metal organic chemical vapor deposition technology; then, grow a u-GaN / n-GaN periodic structure with 20 periods, where n-GaN is Si-doped with a doping concentration of 1×10 19 cm -3 , the thickness of n-GaN is 65nm, and the thickness of u-GaN is 50nm; then, 10 cycles of In 0.05 Ga 0.95 N / GaN superlattice structure, where the well and barrier thicknesses are 3nm and 7nm respectively, and the doping concentration is 1×10 19 cm -3 ; Finally, grow 20 cycles of In 0.2 Ga 0.8 N / GaN multi-quantum well structure, the growth thickness is 4nm and 10nm, and the doping concentration is 1×10 19 cm -3 .
[0048] Step 2: 0.3 mol / L NaNO 3 As the electrolyte, the GaN-based MQW structure was used as the anode and etched for 30 minutes at a constant voltage of 15 V. After the etching was completed, the instrument was turned off, the sample was removed, and the etched sample was immersed in deionized water for 5 minutes and then dried with nitrogen to prepare the mesoporous GaN-based MQW with mesoporous GaN DBR.
[0049] Step 3: Using the mesoporous GaN-based MQW with mesoporous GaN DBR as the substrate, the p-GaN layer was regrown by MOCVD to prepare a mesoporous GaN-based LED with mesoporous GaN DBR. The p-GaN layer was a Mg-doped p-GaN layer with a growth temperature of 1000°C and a doping concentration of 4.0×10 19 cm -3 , thickness is 250nm.
[0050] Comparative Example 1
[0051] The u-GaN / n-GaN periodic structure, GaN-based superlattice and multi-quantum well are grown sequentially on the c-plane sapphire substrate by the method of step 1 of embodiment 1, and the GaN-based LED is prepared using the same process conditions as step 3 of embodiment 1.
[0052] Comparing Example 1 with Comparative Example 1, the LED prepared in Example 1 has a luminous efficiency improved by 3-8 times, a stability improved by more than 1.5 times, and a smooth surface, compared with the LED obtained in Comparative Example 1.
[0053] Comparative Example 2
[0054] The preparation method is the same as that of Example 1, except that the etching voltage is increased from 16 V to 35 V. The surface of the prepared mesoporous GaN-based LED with mesoporous GaN DBR shows obvious peeling phenomenon and becomes uneven.
[0055] Comparing Example 2 with Comparative Example 2, the LED prepared in Example 2 has a luminous efficiency improved by 3-8 times, a stability improved by more than 1.5 times, and a smooth surface compared with the LED obtained in Comparative Example 2.
[0056] Comparative Example 3
[0057] The preparation method is the same as that in Example 1, except that in step 3, during the regrowth process on the mesoporous GaN-based MQW with mesoporous GaN DBR using an organic metal chemical vapor deposition method, the growth temperature of the p-GaN layer is 1100°C. Although the surface of the prepared LED is flat and smooth, the surface color becomes black and metal gallium is precipitated.
[0058] Comparing Example 3 with Comparative Example 3, the LED prepared in Example 3 has a luminous efficiency improved by 3-8 times, a stability improved by more than 1.5 times, and a smooth surface, compared with the LED obtained in Comparative Example 3.
[0059] Figure 1 : is a cross-sectional SEM photograph of the mesoporous GaN-based MQW with mesoporous GaN DBR prepared in Example 1, showing a three-layer structure, and the period number of the mesoporous GaN DBR is 11. Compared with the LED obtained in Comparative Example 1, the mesoporous GaN-based LED with mesoporous GaN DBR prepared in Example 1 has the following characteristics: The cross-sectional SEM photograph of the MP LED with MP GaN DBR prepared in Example 1 is as follows: Figure 2 As shown, the scale bar is 500nm. Figure 2 It can be seen that the LED prepared by the present invention has a unique mesoporous structure.
[0060] The rocking curves corresponding to the InGaN (0002) peaks of the two LEDs prepared in Example 1 are as follows: Figure 3 As shown, according to Figure 3 It can be seen that the line width of the rocking curve of the InGaN (0002) peak of the mesoporous GaN-based LED with mesoporous GaN DBR obtained in the present invention is small, indicating that its crystal quality is improved;
[0061] The Raman spectra of the two LEDs prepared in Example 1 are as follows: Figure 4 As shown, according to Figure 4 It can be seen that the E2 Raman peak moves toward the low frequency direction, indicating that stress relaxation occurs. The reflectance spectra of the two LEDs prepared in Example 1 are as follows: Figure 5 As shown, according to Figure 5It can be seen that its reflectivity is significantly improved; the current-voltage curves of the two LEDs prepared in Example 1 are as follows Figure 6 As shown, according to Figure 6 It can be seen that the turn-on voltage is slightly increased; the electroluminescence (EL) spectra of the two LEDs prepared in Example 1 are as follows Figure 7 As shown, according to Figure 7 It can be seen that the EL intensity is significantly improved.
[0062] By the above-mentioned method, the mesoporous GaN-based MQW with mesoporous GaN DBR of the present invention has a unique mesoporous structure, a high light reflection effect, a large stress relaxation, and a low defect density. With the mesoporous GaN DBR as a substrate, the p-GaN film grown therefrom exhibits a large stress relaxation and a high crystal quality, and is expected to significantly improve the luminous efficiency, the service life, and the heat dissipation capacity of the GaN-based LED; the growth temperature of the p-GaN layer can affect the light reflection capacity of the mesoporous GaN-based MQW with the mesoporous GaN DBR and the crystal quality of the p-GaN film; when the p-GaN layer regrowth temperature is between 800-1100° C., the mesoporous GaN-based MQW with the mesoporous GaN DBR maintains a relatively high reflectivity, and the crystal quality of the film is significantly improved, which is beneficial to improving the luminous efficiency of the GaN-based LED; the process conditions in the present invention are easy to accurately control, and the prepared mesoporous GaN-based LED with the mesoporous GaN DBR has good uniformity and repeatability, and is convenient for industrial production; the prepared LED also has excellent characteristics such as high luminous efficiency, high stability, long service life, and strong heat dissipation capacity, and has broad application prospects.
Claims
1. A method for preparing a mesoporous GaN-based LED having a mesoporous GaN DBR, characterized in that: Follow the steps below to implement it: Step 1: epitaxially growing a GaN buffer layer, a u-GaN / n-GaN periodic structure, a GaN-based superlattice and a multi-quantum well layer on a substrate in sequence by using an organic metal chemical vapor deposition technique to obtain a GaN-based MQW structure; The u-GaN / n-GaN periodic structure includes a low-doped GaN layer and a high-doped GaN layer, both of which have a thickness of 51-67 nm. The doping concentration of the low-doped GaN layer is 4.1×10 15 -9.9×10 17 cm -3 The doping concentration of the highly doped GaN layer is 3.1×10 18 -1×10 19 cm -3 , the number of cycles is 5-20; The doping concentrations of the GaN-based superlattice and the multi-quantum well layer are both 3.1×10 18 -3.9×10 19 cm -3 The superlattice structure is an In period of 10-11 x Ga 1-x N / GaN superlattice structure, where 0<x<0.09, In each period, x Ga 1-x The thickness of N is 3-4nm, and the thickness of GaN is 7nm; the multi-quantum well layer is In with a period of 15-29 y Ga 1-y N / GaN multi-quantum well structure, where 0.1<y<0.4, In each period, y Ga 1-y N thickness is 4-6nm, GaN thickness is 10-11nm; Step 2, electrochemically etching the GaN-based MQW structure in an electrolyte to prepare a mesoporous GaN-based MQW having a mesoporous GaN DBR; Step 3: Using the mesoporous GaN-based MQW as a substrate, a p-GaN layer is grown using a regrowth technique to prepare a mesoporous GaN-based LED having a mesoporous GaN DBR.
2. The method for preparing a mesoporous GaN-based LED having a mesoporous GaN DBR according to claim 1, characterized in that: The electrolyte in step 2 is any one of aqueous solutions of nitric acid, sodium nitrate, sodium chloride and sodium sulfate, with a concentration of 0.3-0.5 mol / ·L, an electrochemical etching voltage of 6-49 V, and an etching time range of 6-78 min.
3. The method for preparing a mesoporous GaN-based LED having a mesoporous GaN DBR according to claim 1, characterized in that: The p-GaN layer in step 3 is a Mg-doped p-GaN layer.
4. The method for preparing a mesoporous GaN-based LED having a mesoporous GaN DBR according to claim 3, characterized in that: The specific process of growing the p-GaN layer by the regrowth technology described in step 3 is as follows: the p-GaN layer is doped with Mg at a growth temperature of 800-1100°C and a doping concentration of 1.1×10 19 cm -3 -5.9×10 19 cm -3 , thickness is 110-290nm.